An ultra-low rebound silent energy-absorbing sponge
Through the addition of specific formulas and soft modifiers, the problem of slow rebound sponge hardening at low temperatures is solved, and a sponge with ultra-low rebound and good silent energy absorption effect is prepared, improving user experience and low temperature resistance.
Patent Information
- Application Number
- CN202410526391.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-04-29
AI Technical Summary
The existing slow rebound sponge becomes hard under low temperature conditions, resulting in poor rebound effect and silent energy absorption effect, and poor user experience.
30-50 parts of open pore polyether, 42-58 parts of slow rebound polyether, 6-10 parts of monofunctional polyether, 50-58 parts of polymerized MDI, 2-3 parts of liquefied MDI, 0.8-1 part of silicone oil, 2.2 were used. - The formula of 5.8 parts of soft modifier, 0.55-0.65 parts of catalyst and 2.8-3.3 parts of deionized water is prepared through the sponge foaming mechanism, and the soft modifier is added to improve the low-temperature resistance and Reduce rebound rate.
The prepared sponge has ultra-low resilience, good silentness and energy absorption effect, maintains softness at low temperatures, is suitable for use in cold areas, and has no sense of bloating or bloating sound, improving the user experience.
Smart Images

Figure CN118325024B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sponges, and in particular to an ultra-low rebound silent energy-absorbing sponge. Background Art
[0002] Commonly used sponges are made of wood cellulose fibers or foamed plastic polymers. There are also natural sponges made from sponge animals. Most natural sponges are used for body cleaning or painting. Synthetic sponges are mainly polyether polyurethane sponges and polyester polyurethane sponges.
[0003] Slow rebound sponge is also called inert sponge, memory sponge, low rebound sponge, slow rebound cotton, zero pressure sponge. Slow rebound sponge feels soft. When you hold the slow rebound sponge in your hand, you will feel that the palm of your hand is constantly emptying, like a sand hole, without any expansion force. You will not feel tired even if you squeeze it for a long time. When you lie on the slow rebound sponge cushion, you will feel the gradual sinking process, like falling into a quagmire, and hear the subtle sound of the gas flowing in the slow rebound sponge. When people sit on the slow rebound sponge waist cushion, it starts to deform continuously, and then the resistance disappears, and the waist pain that should occur after sitting for a long time is hard to find.
[0004] The production of slow-rebound sponges is highly automated. The entire process consists of an automatically controlled feeding system, a foaming machine, a cutting machine, and a computer-programmed molding system. The key procedures are the batching and foaming stages. Professional technicians batch the ingredients according to the manufacturer's requirements for density, hardness and other parameters, and set different foaming times based on the characteristics of each sponge (density, hardness). Manual operation is not strong, and the quality of the final sponge depends on the quality of the ingredients. In addition, many slow-rebound sponges will become very hard in winter or when the temperature drops. In this way, their soft and comfortable advantages cannot be brought into play, which not only leads to poor rebound effect and poor silent energy absorption effect, but also poor experience for people. Summary of the invention
[0005] In view of the problems existing in the prior art, the purpose of the present invention is to provide an ultra-low rebound silent energy-absorbing sponge.
[0006] The purpose of the present invention is achieved by adopting the following technical solutions:
[0007] In a first aspect, the present invention provides an ultra-low rebound silent energy-absorbing sponge, calculated by weight, comprising:
[0008] 30-50 parts of open-cell polyether, 42-58 parts of slow-rebound polyether, 6-10 parts of monofunctional polyether, 50-58 parts of polymerized MDI, 2-3 parts of liquefied MDI, 0.8-1 parts of silicone oil, 2.2-5.8 parts of softening modifier, 0.55-0.65 parts of catalyst and 2.8-3.3 parts of deionized water.
[0009] Preferably, the open-cell polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using glycerol as an initiator; the hydroxyl value is 38 mgKOH / g, and the content of ethylene oxide is not less than 70% of the total mass.
[0010] Preferably, the slow-rebound polyether is the first slow-rebound polyether or the second slow-rebound polyether; wherein the first slow-rebound polyether is obtained by polymerization with propylene oxide (PO) using glycerol as an initiator, and has a molecular weight of 550; the second slow-rebound polyether is obtained by polymerization with propylene oxide (PO) using glycerol as an initiator, and has a molecular weight of 700.
[0011] Preferably, the monofunctional polyether is a first monofunctional polyether or a second monofunctional polyether; wherein the first monofunctional polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) with n-butanol as an initiator, and has a molecular weight of 1000, and the mass proportion of ethylene oxide is 50%; the second monofunctional polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) with isomeric tridecanol as an initiator, and has a molecular weight of 1200, and the mass proportion of ethylene oxide is 40%.
[0012] Preferably, the polymeric MDI is polyphenyl polymethylene polyisocyanate, with a brand of PM-200.
[0013] Preferably, the liquefied MDI is carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate, with a brand of MDI-100L.
[0014] Preferably, the brand of the silicone oil is TEGOSTAB B8002.
[0015] Preferably, the catalyst comprises tin catalyst T9, amine catalyst A33 and amine catalyst A1; wherein the mass ratio of tin catalyst T9, amine catalyst A33 and amine catalyst A1 is 0.05-0.1:0.45-0.5:0.05.
[0016] Preferably, the preparation method of the soft modifier comprises:
[0017] S1. Weigh dihydroxy-terminated polydimethylsiloxane and add it to chloroform, then add a polymerization inhibitor, stir and dissolve thoroughly to obtain solution A; weigh acryloyl chloride and add it to tetrahydrofuran, and dissolve thoroughly to obtain solution B;
[0018] S2, placing solution A in an ice water bath and stirring for half an hour, then adding solution B dropwise, when half of solution B has been added, removing the ice water bath and gradually raising the temperature to 40-50°C, continuing to dropwise add the remaining solution B, after all solution B has been added, keeping the temperature and stirring to react for 10-20 hours, the reaction is completed, removing the solvent under reduced pressure, and washing and drying the obtained product in turn to obtain acryloyl polydimethylsiloxane;
[0019] S3. Mix acryl polydimethylsiloxane and allyl polyoxyethylene ether into N,N-dimethylformamide, stir thoroughly, introduce nitrogen as protective gas, add catalyst, heat to 75-85°C, stir and react for 6-10 hours. After the reaction is completed, remove the solvent, wash with alcohol three times, and vacuum dry to obtain a soft modifier.
[0020] Preferably, in S1, the dihydroxy-terminated polydimethylsiloxane is purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with a purity of >99%, a viscosity of 700-750 cps, and a molecular weight of 5000-6000.
[0021] Preferably, in the solution A of S1, the polymerization inhibitor is hydroquinone, and the mass ratio of dihydroxy-terminated polydimethylsiloxane, hydroquinone and chloroform is 1:0.06-0.12:5-10.
[0022] Preferably, in the solution B of S1, the mass ratio of acryloyl chloride to tetrahydrofuran is 0.4-0.8:3-5.
[0023] Preferably, in S2, the mass ratio of solution A to solution B is 1:1.2-1.6.
[0024] Preferably, in S2, washing is performed by using 15 wt% soda water and saturated salt water at least twice in sequence; and drying is performed in a vacuum oven at 60°C.
[0025] Preferably, in S2, the dripping speed of solution B is controlled to be 60-80 drops / minute, and the dripping is performed under light-proof conditions.
[0026] Preferably, in S3, allyl polyoxyethylene ether is purchased from Hai'an Petrochemical Plant in Jiangsu Province, model APEG-1000, hydroxyl value is 50-55 mgKOH / g, and unsaturation is ≥0.8 mmol / g.
[0027] Preferably, in S3, the mass ratio of acryl polydimethylsiloxane, allyl polyoxyethylene ether and N,N-dimethylformamide is 1:2.1-3.2:15-25.
[0028] Preferably, in S3, the catalyst is azobisisobutyronitrile, and the added amount is 2%-6% of the mass of acryl polydimethylsiloxane.
[0029] In a second aspect, the present invention provides a method for preparing an ultra-low rebound silent energy-absorbing sponge, comprising the following steps:
[0030] Step (1), determining the flow rates of raw materials such as polymeric MDI, liquefied MDI, open-cell polyether, slow-rebound polyether, monofunctional polyether, silicone oil, softening modifier, catalyst and deionized water according to weight percentage;
[0031] Step (2), flowing each raw material into the stirring chamber of the sponge foaming machine according to the formula ratio, stirring at high speed, flowing into the sponge foaming production line, foaming to form a sponge, and obtaining an ultra-low rebound, silent, energy-absorbing large sponge.
[0032] Preferably, in step (2), the stirring temperature is 20-25° C., the speed is 1800-4000 r / min, and the stirring time is 1-3 s.
[0033] The beneficial effects of the present invention are:
[0034] 1. The present invention prepares a slow-rebound sponge, which not only has ultra-low resilience, but also has good quietness and energy absorption effect, and does not have the flatulence and flatulence sound of traditional ordinary slow-rebound sponges. In addition, the sponge prepared by the present invention has high strength, good slow-rebound effect, and can still maintain good softness at a lower temperature, and is suitable for use in low-temperature or colder areas.
[0035] 2. In the present invention, a variety of polyether polyols (including open-cell polyether, slow-rebound polyether, and monofunctional polyether) are mixed and used as polyols, and polymerized MDI and liquefied MDI are used as mixed isocyanates, which are combined and reacted under certain conditions to synthesize polyurethane sponge.
[0036] 3. The additional soft modifier added in the present invention is designed to cope with the problem that the sponge tends to harden at lower temperatures. The soft modifier is composed of a polymerization product of acryloyl polydimethylsiloxane and allyl polyoxyethylene ether. Acryloyl polydimethylsiloxane is based on dihydroxy-terminated polydimethylsiloxane. Through the acyl chloride esterification reaction of acryloyl chloride and the elimination of HCl, polydimethylsiloxane grafted with acryloyl groups is obtained. The soft modifier prepared by the present invention has excellent compatibility in the sponge and has a relatively obvious improvement effect on the low temperature resistance of the sponge. In addition, the present invention also found that it can reduce the resilience of the sponge to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The present invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the present invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.
[0038] Figure 1 This is a product schematic diagram of the sponge prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0040] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0041] The present invention will be further described below in conjunction with the following examples.
[0042] Example 1
[0043] An ultra-low rebound silent energy-absorbing sponge, calculated by weight, comprising:
[0044] 40 parts of open-cell polyether, 50 parts of first slow-rebound polyether, 10 parts of first monofunctional polyether, 50 parts of polymerized MDI, 2 parts of liquefied MDI, 0.8 parts of silicone oil, 3.6 parts of softening modifier, 2.8 parts of deionized water, 0.06 parts of T9 catalyst, 0.5 parts of A33 catalyst, and 0.05 parts of A1 catalyst.
[0045] The open-cell polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using glycerol as an initiator; the hydroxyl value is 38 mgKOH / g, and the content of ethylene oxide is not less than 70% of the total mass.
[0046] The first slow-rebound polyether is obtained by polymerization of propylene oxide (PO) with glycerol as the initiator and has a molecular weight of 550.
[0047] The first monofunctional polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using n-butanol as an initiator, with a molecular weight of 1000, and the mass proportion of ethylene oxide is 50%.
[0048] Among them, polymeric MDI is polyphenyl polymethylene polyisocyanate, with the brand name PM-200.
[0049] Among them, liquefied MDI is carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate, with the brand name MDI-100L.
[0050] Among them, the brand of silicone oil is TEGOSTAB B8002.
[0051] Wherein, the preparation method of the soft modifier comprises:
[0052] S1. Weigh dihydroxy-terminated polydimethylsiloxane (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with a purity of >99%, a viscosity of 725 cps, and a molecular weight of 5500) and add it to chloroform, then add the polymerization inhibitor hydroquinone, stir and dissolve thoroughly to obtain solution A; wherein the mass ratio of dihydroxy-terminated polydimethylsiloxane, hydroquinone and chloroform is 1:0.09:10.
[0053] Acryloyl chloride was weighed and added into tetrahydrofuran, and after being fully dissolved, a solution B was obtained; wherein the mass ratio of acryloyl chloride to tetrahydrofuran was 0.6:4.
[0054] S2. Place solution A in an ice water bath and stir for half an hour, then add solution B dropwise under light-proof conditions, and control the dropping speed to 60 drops / minute. When half of solution B is added, remove the ice water bath and gradually heat to 45°C, and continue to add the remaining solution B. The mass ratio of solution A to solution B is 1:1.4. After all solution B is added, keep warm and continue to stir and react for 15 hours. After the reaction is completed, remove the solvent under reduced pressure, and wash the product with 15wt% soda water and saturated brine at least twice, and dry it in a vacuum oven at 60°C to obtain acryloyl polydimethylsiloxane.
[0055] S3. Mix acryl polydimethylsiloxane and allyl polyoxyethylene ether (purchased from Hai'an Petrochemical Plant, Jiangsu Province, model APEG-1000, hydroxyl value of 50-55 mgKOH / g, unsaturation ≥0.8 mmol / g) into N,N-dimethylformamide, the mass ratio of acryl polydimethylsiloxane, allyl polyoxyethylene ether and N,N-dimethylformamide is 1:2.6:20. After sufficient stirring, introduce nitrogen as a protective gas, and then add azobisisobutyronitrile as a catalyst in an amount of 4% of the mass of acryl polydimethylsiloxane. Heat to 80°C, stir and react for 8 hours under heat preservation and stirring. After the reaction is completed, remove the solvent, wash three times with alcohol, and vacuum dry to obtain a soft modifier.
[0056] The method for preparing the ultra-low rebound silent energy-absorbing sponge comprises the following steps:
[0057] Step (1), weighing polymerized MDI, liquefied MDI, open-cell polyether, slow-rebound polyether, monofunctional polyether, silicone oil, softening modifier, catalyst and deionized water respectively according to weight proportions;
[0058] Step (2), adding each raw material into a sponge foaming machine according to the formula ratio, stirring at high speed, the raw material temperature is 23°C, the speed is 3000r / min, the stirring time is 3s, flowing into the sponge foaming production line, foaming to form a sponge, and obtaining an ultra-low rebound silent energy-absorbing sponge.
[0059] Example 2
[0060] An ultra-low rebound silent energy-absorbing sponge, calculated by weight, comprising:
[0061] 30 parts of open-cell polyether, 58 parts of second slow-rebound polyether, 12 parts of second monofunctional polyether, 58 parts of polymerized MDI, 3 parts of liquefied MDI, 1 part of silicone oil, 2.2 parts of softening modifier, 3.3 parts of deionized water, 0.05 parts of T9 catalyst, 0.45 parts of A33 catalyst, and 0.05 parts of A1 catalyst.
[0062] The open-cell polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using glycerol as an initiator; the hydroxyl value is 38 mgKOH / g, and the content of ethylene oxide is not less than 70% of the total mass.
[0063] The second slow-rebound polyether is obtained by polymerizing propylene oxide (PO) with glycerol as the initiator and has a molecular weight of 700.
[0064] The second monofunctional polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using isomeric tridecanol as an initiator, with a molecular weight of 1200, and the mass proportion of ethylene oxide is 40%.
[0065] Among them, polymeric MDI is polyphenyl polymethylene polyisocyanate, with the brand name PM-200.
[0066] Among them, liquefied MDI is carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate, with the brand name MDI-100L.
[0067] Among them, the brand of silicone oil is TEGOSTAB B8002.
[0068] Wherein, the preparation method of the soft modifier comprises:
[0069] S1. Weigh dihydroxy-terminated polydimethylsiloxane (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with a purity of >99%, a viscosity of 725 cps, and a molecular weight of 5500) and add it to chloroform, then add the polymerization inhibitor hydroquinone, stir thoroughly to dissolve, and obtain solution A; wherein the mass ratio of dihydroxy-terminated polydimethylsiloxane, hydroquinone, and chloroform is 1:0.06:5.
[0070] Acryloyl chloride was weighed and added into tetrahydrofuran, and after being fully dissolved, a solution B was obtained; wherein the mass ratio of acryloyl chloride to tetrahydrofuran was 0.4:3.
[0071] S2. Place solution A in an ice water bath and stir for half an hour, then add solution B dropwise under light-proof conditions, and control the dropping speed to 60 drops / minute. When half of solution B is added, remove the ice water bath and gradually heat to 40°C, and continue to drop the remaining solution B. The mass ratio of solution A to solution B is 1:1.2. After all solution B is added, keep warm and continue to stir and react for 10 hours. After the reaction is completed, remove the solvent under reduced pressure, and wash the product with 15wt% soda water and saturated brine at least twice, and dry it in a vacuum oven at 60°C to obtain acryloyl polydimethylsiloxane.
[0072] S3. Mix acryl polydimethylsiloxane and allyl polyoxyethylene ether (purchased from Hai'an Petrochemical Plant in Jiangsu Province, model APEG-1000, hydroxyl value of 50-55 mgKOH / g, unsaturation ≥0.8 mmol / g) into N,N-dimethylformamide, the mass ratio of acryl polydimethylsiloxane, allyl polyoxyethylene ether and N,N-dimethylformamide is 1:2.1:15. After sufficient stirring, introduce nitrogen as a protective gas, and then add azobisisobutyronitrile as a catalyst in an amount of 2% of the mass of acryl polydimethylsiloxane. Heat to 75°C, stir and react for 6 hours under heat preservation and stirring. After the reaction is completed, remove the solvent, wash three times with alcohol, and vacuum dry to obtain a soft modifier.
[0073] The method for preparing the ultra-low rebound silent energy-absorbing sponge comprises the following steps:
[0074] Step (1), weighing polymerized MDI, liquefied MDI, open-cell polyether, slow-rebound polyether, monofunctional polyether, silicone oil, softening modifier, catalyst and deionized water respectively according to weight proportions;
[0075] Step (2), adding each raw material into a sponge foaming machine according to the formula ratio, stirring at high speed, the raw material temperature is 22°C, the speed is 3500r / min, the stirring time is 2.5s, flowing into the sponge foaming production line, foaming to form a sponge, and obtaining an ultra-low rebound silent energy-absorbing sponge.
[0076] Example 3
[0077] An ultra-low rebound silent energy-absorbing sponge, calculated by weight, comprising:
[0078] 50 parts of open-cell polyether, 42 parts of first slow-rebound polyether, 8 parts of second monofunctional polyether, 52 parts of polymerized MDI, 3 parts of liquefied MDI, 1 part of silicone oil, 5.8 parts of softening modifier, 3.3 parts of deionized water, 0.08 parts of T9 catalyst, 0.5 parts of A33 catalyst, and 0.05 parts of A1 catalyst.
[0079] The open-cell polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using glycerol as an initiator; the hydroxyl value is 38 mgKOH / g, and the content of ethylene oxide is not less than 70% of the total mass.
[0080] The first slow-rebound polyether is obtained by polymerization of propylene oxide (PO) with glycerol as the initiator and has a molecular weight of 550.
[0081] The second monofunctional polyether is obtained by random polymerization of propylene oxide (PO) and ethylene oxide (EO) using isomeric tridecanol as an initiator, with a molecular weight of 1200, and the mass proportion of ethylene oxide is 40%.
[0082] Among them, polymeric MDI is polyphenyl polymethylene polyisocyanate, with the brand name PM-200.
[0083] Among them, liquefied MDI is carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate, with the brand name MDI-100L.
[0084] Among them, the brand of silicone oil is TEGOSTAB B8002.
[0085] Wherein, the preparation method of the soft modifier comprises:
[0086] S1. Weigh dihydroxy-terminated polydimethylsiloxane (purchased from Wuhan Huaxiang Kejie Biotechnology Co., Ltd., with a purity of >99%, a viscosity of 725 cps, and a molecular weight of 5500) and add it to chloroform, then add the polymerization inhibitor hydroquinone, stir thoroughly to dissolve, and obtain solution A; wherein the mass ratio of dihydroxy-terminated polydimethylsiloxane, hydroquinone, and chloroform is 1:0.12:10.
[0087] Acryloyl chloride was weighed and added into tetrahydrofuran, and after being fully dissolved, a solution B was obtained; wherein the mass ratio of acryloyl chloride to tetrahydrofuran was 0.8:5.
[0088] S2. Place solution A in an ice water bath and stir for half an hour, then add solution B dropwise under light-proof conditions, and control the dropping speed to 80 drops / minute. When half of solution B is added, remove the ice water bath and gradually heat to 50°C, and continue to drop the remaining solution B. The mass ratio of solution A to solution B is 1:1.6. After all solution B is added, keep warm and continue to stir and react for 20 hours. After the reaction is completed, remove the solvent under reduced pressure, and wash the product with 15wt% soda water and saturated brine at least twice, and dry it in a vacuum oven at 60°C to obtain acryloyl polydimethylsiloxane.
[0089] S3. Mix acryl polydimethylsiloxane and allyl polyoxyethylene ether (purchased from Hai'an Petrochemical Plant in Jiangsu Province, model APEG-1000, hydroxyl value of 50-55 mgKOH / g, unsaturation ≥0.8 mmol / g) into N,N-dimethylformamide, the mass ratio of acryl polydimethylsiloxane, allyl polyoxyethylene ether and N,N-dimethylformamide is 1:3.2:25. After sufficient stirring, introduce nitrogen as a protective gas, and then add azobisisobutyronitrile as a catalyst in an amount of 6% of the mass of acryl polydimethylsiloxane. Heat to 85°C, stir and react for 10 hours under heat preservation and stirring. After the reaction is completed, remove the solvent, wash three times with alcohol, and vacuum dry to obtain a soft modifier.
[0090] The method for preparing the ultra-low rebound silent energy-absorbing sponge comprises the following steps:
[0091] Step (1), weighing polymerized MDI, liquefied MDI, open-cell polyether, slow-rebound polyether, monofunctional polyether, silicone oil, softening modifier, catalyst and deionized water respectively according to weight proportions;
[0092] Step (2), adding each raw material into a sponge foaming machine according to the formula ratio, stirring at high speed, the raw material temperature is 23°C, the speed is 3000r / min, the stirring time is 3s, flowing into the sponge foaming production line, foaming to form a sponge, and obtaining an ultra-low rebound silent energy-absorbing sponge.
[0093] Comparative Example 1
[0094] A low-resilience sponge, which differs from Example 1 in that no softness modifier is added into the composition.
[0095] Comparative Example 2
[0096] A low-resilience sponge, which differs from Example 1 in that the softening modifier added to the composition is dihydroxy-terminated polydimethylsiloxane.
[0097] Comparative Example 3
[0098] A low-resilience sponge, which differs from Example 1 in that the softness modifier added to the composition is acryl polydimethylsiloxane (prepared in the same manner as Example 1).
[0099] Experimental example
[0100] In order to more clearly illustrate the present invention, the low-rebound sponges prepared in Example 1 and Comparative Examples 1-3 were tested and compared in terms of performance, with tensile strength according to GB / T 6344-2008, rebound rate according to GB / T 6670-2008, and hardness value according to ISO 2439-2008 (testing conditions: -10°C / 50%RH).
[0101] The test results are shown in Table 1 below:
[0102] Table 1 Performance test results of different low rebound sponges
[0103] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Density (kg / m 3 )]]> 48.2 47.5 48.9 48.3 Tensile strength(KPa) 126 108 117 121 Rebound rate (%) 1.8 2.3 2 2.3 Low temperature hardness value (N) 152.6 186.7 173.2 165.1 Is there any bloating sound when pressing? Basically no Basically no Basically no Basically no
[0104] It can be seen from Table 1 that the low-rebound sponge prepared in Example 1 of the present invention has a relatively good mute effect, and there is basically no flatulence sound when pressed; the tensile strength is slightly high, but the rebound rate is low, indicating that it has good firmness and a good slow rebound effect, and is less prone to damage; the hardness value under low temperature (-10°C / 50%RH) conditions is relatively small, indicating that it is suitable for use in cold weather conditions, can be softer, and the experience is more comfortable.
[0105] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0106] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. An ultra-low rebound silent energy-absorbing sponge, characterized in that: Calculated by weight, including: 30-50 parts of open-cell polyether, 42-58 parts of slow-rebound polyether, 6-10 parts of monofunctional polyether, 50-58 parts of polymeric MDI, 2-3 parts of liquefied MDI, 0.8-1 parts of silicone oil, 2.2-5.8 parts of soft modifier, 0.55-0.65 parts of catalyst and 2.8-3.3 parts of deionized water; The open-cell polyether is obtained by random polymerization of propylene oxide and ethylene oxide using glycerol as an initiator; the hydroxyl value is 38 mgKOH / g, and the content of ethylene oxide is not less than 70% of the total mass; The slow-rebound polyether is the first slow-rebound polyether or the second slow-rebound polyether; wherein the first slow-rebound polyether is obtained by polymerizing propylene oxide with glycerol as an initiator, and has a molecular weight of 550; the second slow-rebound polyether is obtained by polymerizing propylene oxide with glycerol as an initiator, and has a molecular weight of 700; The monofunctional polyether is a first monofunctional polyether or a second monofunctional polyether; wherein the first monofunctional polyether is obtained by random polymerization of propylene oxide and ethylene oxide using n-butanol as an initiator, and has a molecular weight of 1000, and the mass proportion of ethylene oxide is 50%; the second monofunctional polyether is obtained by random polymerization of propylene oxide and ethylene oxide using isomeric tridecanol as an initiator, and has a molecular weight of 1200, and the mass proportion of ethylene oxide is 40%; The polymeric MDI is polyphenyl polymethylene polyisocyanate, with the brand name WANNATE®PM-200; the liquefied MDI is carbodiimide-uretonimine modified 4,4'-diphenylmethane diisocyanate, with the brand name WANNATE®MDI-100L; the brand name of the silicone oil is TEGOSTAB B8002; The preparation method of the soft modifier comprises: S1. Weigh dihydroxy-terminated polydimethylsiloxane and add it to chloroform, then add a polymerization inhibitor, stir and dissolve thoroughly to obtain solution A; weigh acryloyl chloride and add it to tetrahydrofuran, and dissolve thoroughly to obtain solution B; S2, placing solution A in an ice water bath and stirring for half an hour, then adding solution B dropwise, when half of solution B has been added, removing the ice water bath and gradually raising the temperature to 40-50°C, continuing to dropwise add the remaining solution B, after all solution B has been added, keeping the temperature and stirring to react for 10-20 hours, the reaction is completed, removing the solvent under reduced pressure, and washing and drying the obtained product in turn to obtain acryloyl polydimethylsiloxane; S3, mixing acryloyl polydimethylsiloxane and allyl polyoxyethylene ether into N,N-dimethylformamide, stirring thoroughly, introducing nitrogen as protective gas, adding a catalyst, heating to 75-85°C, stirring and reacting for 6-10 hours, removing the solvent after the reaction, washing with alcohol three times, and vacuum drying to obtain a soft modifier; In the S3, the mass ratio of acryl polydimethylsiloxane, allyl polyoxyethylene ether and N,N-dimethylformamide is 1:2.1-3.2:15-25; in the S3, the catalyst is azobisisobutyronitrile, and the added amount is 2%-6% of the mass of acryl polydimethylsiloxane.
2. The ultra-low rebound silent energy absorbing sponge according to claim 1, characterized in that: The catalyst includes tin catalyst T9, amine catalyst A33 and amine catalyst A1; wherein the mass ratio of tin catalyst T9, amine catalyst A33 and amine catalyst A1 is 0.05-0.1:0.45-0.5:0.
05.
3. The ultra-low rebound silent energy absorbing sponge according to claim 1, characterized in that: In the solution A of S1, the inhibitor is hydroquinone, and the mass ratio of dihydroxy-terminated polydimethylsiloxane, hydroquinone and chloroform is 1:0.06-0.12:5-10; in the solution B of S1, the mass ratio of acryloyl chloride and tetrahydrofuran is 0.4-0.8:3-5.
4. The ultra-low rebound silent energy absorbing sponge according to claim 1, characterized in that: In the S2, the mass ratio of solution A to solution B is 1:1.2-1.6; in the S2, washing is performed by washing at least twice with 15wt% soda water and saturated salt water in sequence; drying is performed in a vacuum oven at 60°C; in the S2, the dripping speed of solution B is controlled to be 60-80 drops / minute, and the dripping is performed under light-proof conditions.
Citation Information
Patent Citations
Method for preparing side-chain-modified organosilicon softener
CN104452311A
Preparation method of hyperbranched ternary polymerization organic silicon