A kind of quick-drying special glue for movable door and window system and preparation method thereof
By using components such as α,ω-dihydroxypolydimethylsiloxane, reinforcement fillers and structural hygroscopic absorbers in silicone sealants, combined with amino-containing silane coupling agents and ketoxime crosslinkers, The problem of insufficient curing speed of silicone sealant is solved, efficient rapid curing and cost reduction are achieved, and the performance of the glue is improved.
Patent Information
- Application Number
- CN202410478940.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-20
AI Technical Summary
The existing silicone sealant has a curing thickness of less than 3mm within 12 hours, which cannot meet the requirements for high curing speed for mobile door and window system production. The rapid curing agent is costly and has no significant effect.
Using α,ω-dihydroxypolydimethylsiloxane and dimethylsiloxane as base components, reinforcing fillers, crosslinking agents, catalysts and structural hygroscopic agents, especially containing epoxy end-capped groups As a structural hygroscopic agent, the EO/PO block polyether is combined with amino-containing silane coupling agent and ketoxime crosslinking agent to promote the crosslinking reaction through moisture in the air and achieve rapid curing.
The curing thickness of silicone glue is achieved above 4mm within 12 hours, reducing the preparation cost, improving the bonding strength, toughness and elastic recovery rate of the glue, and suppressing the yellowing of the glue.
Smart Images

Figure BDA0004801370680000121 
Figure BDA0004801370680000122 
Figure BDA0004801370680000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone sealants, and in particular to a quick-drying special sealant for a movable door and window system and a preparation method thereof. Background Art
[0002] In recent years, the technology of using aluminum profiles to prepare movable door and window systems has developed rapidly, and silicone sealants are a supporting product for aluminum profiles. Silicone sealants are also commonly used in movable door and window systems.
[0003] For the production line of the movable door and window system, the silicone sealant used has a higher curing speed requirement, requiring the curing speed of the silicone sealant to be greater than 4mm in thickness within 12 hours. However, the curing speed of ordinary silicone sealants on the market is less than 3mm in thickness within 12 hours. Therefore, ordinary silicone sealants cannot be used on the production line of the movable door and window system. Therefore, a silicone sealant that can be quickly applied to the production line of the movable door and window system is needed.
[0004] At present, the preparation process for improving the curing speed of silicone sealants mainly involves adding crosslinking agents with fast crosslinking speed, such as vinyl trisbutyl ketoxime silane crosslinkers or tetrasbutyl ketoxime silane crosslinkers. However, the price of such crosslinking agents is generally high, and in many cases, the effect of rapid curing is still not significant enough, so the development of a practical quick-drying silicone sealant is of great significance for the production of aluminum sliding door and window systems. Summary of the invention
[0005] In order to develop a practical quick-drying special adhesive suitable for a movable door and window system, the present application provides a quick-drying special adhesive for a movable door and window system and a preparation method thereof.
[0006] In the first aspect, the present application provides a quick-drying special adhesive for movable door and window systems using the following technical solutions:
[0007] A quick-drying special adhesive for a movable door and window system, comprising the following components in parts by weight: 60-80 parts of α, ω-dihydroxy polydimethylsiloxane, 15-30 parts of dimethyl silicone oil, 100-120 parts of reinforcing filler, 7-12 parts of a cross-linking agent, 0.8-1.5 parts of a coupling agent, 0.07-0.12 parts of a catalyst, and 4-12 parts of a structural moisture absorbent;
[0008] The framework type desiccant is selected from any of the following end-capped EO / PO block polyethers:
[0009] CH 2 =CHCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH3 )O) m CH 2 CHOCH 2
[0010] CH 2 CHOCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2
[0011] CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2
[0012] CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m OCCH 3
[0013] The value ranges of n and m are both 0-10, and n and m are not 0.
[0014] Among them, CH 2 =CHCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 It is an allyl epoxy terminated EO / PO block polyether, CH 2 CHOCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2It is a diepoxy-terminated EO / PO block polyether, CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 It is a monoepoxy-terminated EO / PO block polyether, CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m OCCH 3 It is a monoester-terminated EO / PO block polyether.
[0015] By adopting the above scheme, α, ω-dihydroxy polydimethylsiloxane is used as the basic prepolymer, dimethyl silicone oil is used as the plasticizer, and reinforcing fillers are added to enhance the colloid strength, and then the material is exposed to the air and can be quickly cured by adding a crosslinking agent, a catalyst, and a framework type hygroscopic agent, and then a coupling agent with high reaction functionality is used to maintain good adhesion between the material and the construction material, so that the silicone sealant can achieve the purpose of fast drying. Among them, the framework type hygroscopic agent can be selected from any of the end-capped EO / PO block polyethers of allyl epoxy group end-capped EO / PO block polyether, diepoxy group end-capped EO / PO block polyether, monoepoxy group end-capped EO / PO block polyether, and monoester group end-capped EO / PO block polyether. Since the EO / PO block polyether has an amphiphilic structure, the higher the EO content, the stronger the hydrophilicity; the higher the PO content, the stronger the lipophilicity. The presence of different proportions of EO segments and PO segments in the long chain makes the framework type desiccant have better hygroscopicity and compatibility than ordinary desiccant. Therefore, after adding the framework type desiccant to the basic silicone rubber for modification, the framework type desiccant can be fully mixed in the silicone rubber system, so that the rubber can be exposed to the air and can fully absorb the moisture in the air, which is conducive to promoting the hydrolysis of the crosslinking agent and the curing reaction with the rubber, so that the rubber can reach a cured thickness of more than 4mm within 12 hours.
[0016] Optionally, the coupling agent is an amino-containing silane coupling agent, and the framework-type moisture absorbent is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 .
[0017] By adopting the above scheme, the amino-containing silane coupling agent has a good coupling effect with most substrates and can improve the adhesion between the rubber and other material surfaces. This is because the amino-containing silane coupling agent has free amino groups and has high reactivity. By combining the framework-type hygroscopic agent with epoxy end-capping groups with the amino-containing silane coupling agent and the cross-linking agent, not only the hydrophilicity of the basic rubber is improved, the cross-linking agent is further promoted to hydrolyze and react with the rubber to cure; the yellowing of the rubber is suppressed, the weather resistance of the rubber is improved; the adhesive elasticity of the rubber is also improved, and the rubber has a good elastic recovery rate.
[0018] Optionally, the degree of polymerization of the framework-type hygroscopic agent is n+m=8, wherein n:m=(5-6):(3-2).
[0019] By adopting the above scheme, the framework-type hygroscopic agent with a degree of polymerization in the above range can not only be fully mixed with the basic silicone rubber material, but also the polyoxyethylene chain segments account for a relatively large proportion in the framework-type hygroscopic agent, so that the framework-type hygroscopic agent has strong hydrophilicity and wettability, which is beneficial for the rubber material to be exposed to the air to absorb moisture in the air, promote the hydrolysis of the cross-linking agent and react with the rubber material to undergo a curing reaction, and realize the rapid curing performance of the silicone rubber.
[0020] Optionally, the coupling agent includes a primary amine silane coupling agent, a secondary amine silane coupling agent and a tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent and the tertiary amine silane coupling agent is in the range of (1-2): (1-2): (1-3).
[0021] By adopting the above technical solution, since the aminosilane coupling agent has high activity and self-catalytic polymerization, the use of primary amine silane coupling agents alone easily leads to too fast surface curing of the rubber material, affecting the internal water absorption of the rubber material, resulting in slow internal curing, thereby affecting the overall curing time of the rubber material. Since primary, secondary and tertiary amine silane coupling agents have different reactivity, by using a mixture of primary, secondary and tertiary amine silane coupling agents within this mass ratio range, the aminosilane coupling agent is retained with high activity and self-catalytic polymerization, so that the rubber material has excellent bonding performance with a variety of substrates, while slowing down the surface curing speed, so that the interior of the rubber material can fully absorb water for curing, thereby reducing the overall curing time of the rubber material.
[0022] Optionally, the cross-linking agent is a ketoxime cross-linking agent.
[0023] By adopting the above scheme, the ketoxime crosslinking agent has a strong crosslinking ability. Under the action of the catalyst, the ketoxime crosslinking agent can be rapidly hydrolyzed and the rubber material can be reacted and solidified. By combining the ketoxime crosslinking agent with the framework-type moisture absorbent containing epoxy end-capping groups and the amino-containing silane coupling agent, a uniform dynamic crosslinking network structure is formed inside the rubber material, which can not only effectively improve the bonding strength and bonding toughness inside the rubber material, but also further improve the bonding elasticity of the rubber material, so that the rubber material has a good elastic recovery rate.
[0024] Optionally, the crosslinking agent is methyl tributylidene oxime silane.
[0025] By adopting the above scheme, the crosslinking speed of the methyl tributylanoxime silane crosslinker is faster than that of the vinyl tributylanoxime silane crosslinker or the tetrabutyl ketone oxime silane crosslinker, which are also ketone oxime crosslinkers, but the cost is high. The hydrolysis speed of the methyl tributylanoxime silane crosslinker is promoted by the water absorption of the framework-type moisture absorbent, so that the crosslinking speed of the vinyl tributylanoxime silane crosslinker or the tetrabutyl ketone oxime silane crosslinker with a low cost can be achieved, which is conducive to reducing the preparation cost of preparing the quick-drying special adhesive.
[0026] Optionally, the viscosity range of the α,ω-dihydroxypolydimethylsiloxane is 50000-80000cps, and the viscosity range of the dimethyl silicone oil is 350-500cst.
[0027] By adopting the above technical scheme, when the viscosity of α, ω-dihydroxy polydimethylsiloxane is in the range of 50000-80000cps, the rubber not only has good extrusion properties, but also has high bonding strength; when the viscosity of dimethyl silicone oil is in the range of 350-500cst, the colloid not only has good extrusion properties, but also has good bonding elasticity, which is beneficial to improving the elastic recovery rate of the colloid.
[0028] Optionally, the reinforcing filler is any one of hydrophobic nano-calcium carbonate and hydrophobic fumed silica.
[0029] By adopting the above technical solution, the tensile strength and elongation at break of the rubber compound can be improved by using hydrophobic nano calcium carbonate and fumed silica as fillers. The hydrophobicity is beneficial to improving the compatibility between the reinforcing filler and the rubber compound, so that the reinforcing filler can be fully mixed with the rubber compound.
[0030] Optionally, the catalyst is any one of dibutyltin dilaurate and n-butyltin diacetate.
[0031] By adopting the above technical solution, the organic tin catalyst has a faster reaction efficiency, which is beneficial to catalyze the hydrolysis reaction of the cross-linking agent, thereby accelerating the curing of the rubber.
[0032] In the second aspect, the present application provides a method for preparing a quick-drying special adhesive for a movable door and window system using the following technical solution:
[0033] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0034] S1. Stir α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil evenly, slowly add reinforcing filler, raise the temperature to above 130° C., maintain vacuum state and stir evenly to obtain a base rubber material;
[0035] S2, introduce inert gas to balance the vacuum, wait for the base rubber to cool to room temperature, add the cross-linking agent and the framework type moisture absorbent, maintain the vacuum state and stir evenly to obtain a mixed rubber;
[0036] S3, introducing inert gas to balance the vacuum, after the mixed rubber obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst, maintaining the vacuum state and stirring evenly to obtain the target rubber;
[0037] S4. Inert gas is introduced to balance the vacuum, and then the target rubber material is extruded through a press and sealed for storage.
[0038] By adopting the above scheme, because the reaction speed of the crosslinking agent is fast under the action of the catalyst, the temperature is raised to above 130°C, the moisture in the raw materials is converted into water vapor and discharged by vacuuming, and then the crosslinking agent, the framework type moisture absorbent, the catalyst, and the coupling agent are added in steps and stirred, which can prevent the catalyst from catalyzing the crosslinking agent to hydrolyze during stirring, so that each auxiliary agent is fully stirred and uniformly mixed, and at the same time, it can also prevent the catalyst from catalyzing the crosslinking agent to hydrolyze during storage, which is conducive to increasing the storage time of the rubber. In addition, the production process adopted is simple, the energy consumption is low, and it is conducive to mass production.
[0039] In summary, the present application has at least any one of the following beneficial effects.
[0040] 1. By adding a structural desiccant, the rubber can fully absorb moisture in the air, which is beneficial to promote the hydrolysis of the cross-linking agent, thereby achieving rapid curing of the rubber.
[0041] 2. By adding a framework type desiccant containing an epoxy end-capping group, the framework type desiccant can effectively inhibit the yellowing of the rubber compound to which an amino-containing silane coupling agent is added, which is beneficial to improving the weather resistance of the rubber compound.
[0042] 3. By adding a framework type desiccant containing a single epoxy end-capping group, the rubber can have the characteristics of rapid curing under the cooperation of the framework type desiccant with an amino-containing silane coupling agent and a ketoxime cross-linking agent.
[0043] 4. By adding a framework-type desiccant containing a single epoxy end-capping group, the framework-type desiccant, the amino-containing silane coupling agent, and the ketoxime cross-linking agent cooperate with each other, not only the bonding strength and bonding toughness inside the rubber are improved, but also the rubber has a good elastic recovery rate. DETAILED DESCRIPTION
[0044] The present application is further described below with reference to embodiments and comparative examples.
[0045] Example
[0046] Example 1
[0047] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0048] 60kg of α,ω-dihydroxypolydimethylsiloxane, 30kg of dimethyl silicone oil, 110kg of hydrophobic nano-calcium carbonate, 12kg of cross-linking agent methyl tributylidene oxime silane, 1.5kg of coupling agent, 0.12kg of catalyst dibutyltin dilaurate, and 12kg of framework-type moisture absorbent.
[0049] The viscosity of α,ω-dihydroxypolydimethylsiloxane is 50000cps, and the viscosity of dimethyl silicone oil is 350cst.
[0050] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:2:3. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0051] The framework type desiccant is selected from allyl epoxy terminated EO / PO block polyether, wherein the structural formula is CH 2 =CHCH 2 O(CH 2 CH 2O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=1, m=2.
[0052] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0053] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0054] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and framework type moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0055] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0056] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0057] Example 2
[0058] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0059] α,ω-dihydroxypolydimethylsiloxane 70kg, dimethyl silicone oil 15kg, hydrophobic fumed silica 120kg, crosslinking agent methyl tributylidene oxime silane 7kg, coupling agent 0.8kg, catalyst n-butyl tin diacetate 0.07kg, framework type desiccant 4kg.
[0060] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 80,000 cps, and the viscosity range of dimethyl silicone oil is 500 cst.
[0061] The coupling agent includes a primary amine silane coupling agent, a secondary amine silane coupling agent, and a tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 2:1:1. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 )3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0062] The framework type desiccant is selected from allyl epoxy terminated EO / PO block polyether, wherein the structural formula is CH 2 =CHCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=10, m=10.
[0063] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0064] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic fumed silica, heat to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0065] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and framework type moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0066] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst n-butyltin diacetate, maintaining the vacuum degree at 0.085MPa and stirring evenly for 20min, to obtain the target rubber material;
[0067] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0068] Example 3
[0069] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0070] α,ω-dihydroxypolydimethylsiloxane 80kg, dimethyl silicone oil 20kg, hydrophobic nano calcium carbonate 100kg, cross-linking agent methyl tributylidene oxime silane 10kg, coupling agent 1kg, catalyst dibutyltin dilaurate 0.1kg, framework type desiccant 8kg.
[0071] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 60,000 cps, and the viscosity range of dimethyl silicone oil is 400 cst.
[0072] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:1:2. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0073] The framework type desiccant is selected from the diepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 2 CHOCH 2 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=5, m=3.
[0074] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0075] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0076] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and framework type moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0077] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0078] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0079] Example 4
[0080] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0081] α,ω-dihydroxypolydimethylsiloxane 80kg, dimethyl silicone oil 20kg, hydrophobic nano calcium carbonate 100kg, cross-linking agent methyl tributylidene oxime silane 10kg, coupling agent 1kg, catalyst dibutyltin dilaurate 0.1kg, framework type desiccant 8kg.
[0082] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 60,000 cps, and the viscosity range of dimethyl silicone oil is 400 cst.
[0083] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:1:2. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0084] The framework type desiccant is selected from monoepoxy terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=8, m=7.
[0085] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0086] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0087] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and framework type moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0088] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0089] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0090] Example 5
[0091] A quick-drying special adhesive for a movable door and window system, which differs from Example 4 in that a different structural moisture absorbent is used.
[0092] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=5, m=2.
[0093] Example 6
[0094] A quick-drying special adhesive for a movable door and window system, which differs from Example 4 in that a different structural moisture absorbent is used.
[0095] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=5, m=3.
[0096] Example 7
[0097] A quick-drying special adhesive for movable door and window systems, which differs from Example 6 in that a different structural type moisture absorbent is used.
[0098] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=3, m=5.
[0099] Example 8
[0100] A quick-drying special adhesive for movable door and window systems, which differs from Example 6 in that a different structural type moisture absorbent is used.
[0101] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2, specifically, n=4, m=4.
[0102] Example 9
[0103] A quick-drying special adhesive for movable door and window systems, which differs from Example 6 in that a different structural type moisture absorbent is used.
[0104] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=7, m=1.
[0105] Example 10
[0106] A quick-drying special adhesive for movable door and window systems, which differs from Example 6 in that a different structural type moisture absorbent is used.
[0107] Among them, the framework type desiccant is selected from monoepoxy-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH 2 , specifically, n=6, m=2.
[0108] Embodiment 11
[0109] A quick-drying special adhesive for a movable door and window system, which differs from Example 6 in that a different coupling agent is used.
[0110] Among them, the coupling agent is KH-570.
[0111] Example 12
[0112] A quick-drying special adhesive for a movable door and window system, which differs from Example 6 in that a different coupling agent is used.
[0113] Among them, the coupling agent is KH-550.
[0114] Embodiment 13
[0115] A quick-drying special adhesive for a movable door and window system, which differs from Example 6 in that a different coupling agent is used.
[0116] The coupling agent used includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent is 1:3:4. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0117] Embodiment 14
[0118] A quick-drying special adhesive for movable door and window systems, which differs from Example 6 in that a different structural type moisture absorbent is used.
[0119] Among them, the framework type desiccant is selected from monoester-terminated EO / PO block polyether, wherein the structural formula is CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m OCCH 3 , specifically, n=5, m=3.
[0120] Comparative Example
[0121] Comparative Example 1
[0122] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0123] α,ω-dihydroxypolydimethylsiloxane 80kg, dimethyl silicone oil 20kg, hydrophobic nano calcium carbonate 100kg, cross-linking agent methyl tributylidene oxime silane 10kg, coupling agent 1kg, catalyst dibutyltin dilaurate 0.1kg.
[0124] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 60,000 cps, and the viscosity of dimethyl silicone oil is 400 cst.
[0125] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:1:2. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0126] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0127] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0128] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0129] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0130] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0131] Comparative Example 2
[0132] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0133] α, ω-dihydroxypolydimethylsiloxane 80kg, dimethyl silicone oil 20kg, hydrophobic nano calcium carbonate 100kg, cross-linking agent methyl tributylidene oxime silane 10kg, coupling agent 1kg, catalyst dibutyltin dilaurate 0.1kg, common desiccant 8kg.
[0134] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 60,000 cps, and the viscosity of dimethyl silicone oil is 400 cst.
[0135] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:1:2. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0136] The common hygroscopic agent is polyethylene glycol, wherein the degree of polymerization of polyethylene glycol is 8.
[0137] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0138] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0139] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and common moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0140] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0141] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0142] Comparative Example 3
[0143] A quick-drying special adhesive for a movable door and window system, comprising the following raw materials:
[0144] α,ω-dihydroxypolydimethylsiloxane 80kg, dimethyl silicone oil 20kg, hydrophobic nano calcium carbonate 100kg, cross-linking agent methyl tributylidene oxime silane 10kg, coupling agent 1kg, catalyst dibutyltin dilaurate 0.1kg, framework type desiccant 8kg.
[0145] The viscosity of α, ω-dihydroxy polydimethylsiloxane is 60,000 cps, and the viscosity of dimethyl silicone oil is 400 cst.
[0146] The coupling agent includes primary amine silane coupling agent, secondary amine silane coupling agent, and tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent is 1:1:2. Specifically, the molecular formula of the primary amine silane coupling agent is H 2 N(CH 2 ) 3 Si(OC 2 H 5 ) 3 The molecular formula of secondary amine silane coupling agent is HN[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 2 The molecular formula of tertiary amine silane coupling agent is N[(CH 2 ) 3 Si(OC 2 H 5 ) 3 ] 3 .
[0147] The structural desiccant is selected from CH 3 O(CH 2 CH 2 O) n (CH 2 CH(CH 3 )O) m CH 2 CHOCH2 , specifically, n=12, m=11.
[0148] A method for preparing a quick-drying special adhesive for a movable door and window system comprises the following steps:
[0149] S1. Add α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil into a planetary mixer, stir evenly, slowly add hydrophobic nano calcium carbonate, raise the temperature to 130° C., maintain a vacuum degree of 0.085 MPa and stir evenly for 90 minutes to obtain a base rubber;
[0150] S2, introduce nitrogen balance vacuum, wait for the base rubber to cool to room temperature, add crosslinking agent methyl tributylidene silane and framework type moisture absorbent, maintain the vacuum degree of 0.085MPa and stir evenly for 20min, control the stirring speed at 90 rpm, and obtain a mixed rubber;
[0151] S3, introducing nitrogen to balance the vacuum, after the mixed rubber material obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst dibutyltin dilaurate, maintaining the vacuum degree at 0.085 MPa and stirring evenly for 20 minutes, to obtain the target rubber material;
[0152] S4. Finally, nitrogen is introduced to balance the vacuum, and the target rubber material is extruded, sealed and stored through a press.
[0153] Performance test data
[0154] 1. Curing speed: Refer to GB / T 32369-2005 Determination of curing degree of sealant for testing, and use method 2, wedge groove method, for testing. The test temperature is 25°C and the relative humidity is 50%.
[0155] 2. Surface drying time: Refer to GB / T 13477.5 Test methods for building sealing materials Part 5: Determination of surface drying time for testing, and test according to Method A in the standard. The test temperature is 25°C and the relative humidity is 50%.
[0156] 3. Tack-free time: Refer to GB / T 13477.5 Test methods for building sealing materials Part 5: Determination of surface drying time for testing, and test with reference to method B in the standard until a smooth elastic skin is formed on the surface of the colloid. If there is no stickiness when touched by fingers, the time is recorded as the tack-free time.
[0157] 4. Extrusion: Refer to GB / T 13477.4 Test methods for building sealing materials Part 4: Determination of extrusion properties of original packaged single-component sealing materials for testing. The nozzle should be a plastic nozzle with an inner diameter of 6mm. The test temperature is 25°C and the relative humidity is 50%.
[0158] 5. Tensile modulus: refer to GB / T 13477.8 Test methods for building sealing materials Part 8: Determination of tensile bonding properties for testing. The test temperature is 25°C and the relative humidity is 50%.
[0159] 6. Fixed-tension adhesion: Refer to "GB / T 13477.10 Test methods for building sealing materials Part 10: Determination of fixed-tension adhesion properties" for testing. Treat the test pieces according to Method A in the standard. The test temperature is 25°C and the relative humidity is 50%.
[0160] 7. Elastic recovery rate: refer to GB / T 13477.17 Test methods for building sealing materials Part 17: Determination of elastic recovery rate for testing. The test piece maintains an elongation of 60%, the test temperature is 25°C, and the relative humidity is 50%.
[0161] 8. Color difference value: refer to "GB / T 13477.21 Test methods for building sealing materials Part 21: Determination of color change after artificial accelerated weathering" for testing. The test piece shall first be subjected to automatic cycle exposure test according to the provisions of Table 3 Method A Cycle No. 1 in "GB / T 16422.2-2014 Plastic Laboratory Light Source Exposure Test Method". The exposure time is 1000h, the color difference test temperature is 25℃, and the relative humidity is 50%.
[0162] Table 1 Curing speed of quick-drying special glue
[0163]
[0164] Table 2 Surface drying time and tack-free time of quick-drying special adhesive
[0165]
[0166]
[0167] According to Example 6 and Comparative Example 1 and the data in Table 1, the curing speed of ordinary silicone rubber is less than 4 mm in curing depth within 12 hours, while after adding the framework type desiccant to the formula of ordinary silicone rubber for modification, the overall curing speed of the rubber is significantly improved, and the curing depth is greater than 4 mm within 12 hours. This is because the framework type desiccant has hygroscopicity, so that the rubber can absorb moisture in the air when exposed to the air, promote the rapid hydrolysis of the cross-linking agent and react with the rubber to cure, thereby improving the overall curing speed of the silicone rubber.
[0168] According to Example 6 and Comparative Example 2 and combined with the data in Table 1, it can be seen that compared with the silicone rubber compound added with ordinary polyethylene glycol hygroscopic agent, the curing speed of the silicone rubber compound added with ordinary polyethylene glycol hygroscopic agent is slow, and the curing depth is less than 4 mm within 12 hours. After modification with the framework-type hygroscopic agent, the overall curing speed of the rubber compound is significantly improved, and the curing depth is greater than 4 mm within 12 hours. It may be because the polyoxypropylene chain segment in the framework-type hygroscopic agent has lipophilicity, which can make the framework-type hygroscopic agent fully compatible and mixed with the rubber compound, thereby further improving the wettability and hygroscopic capacity of the rubber compound, enabling the rubber compound to fully absorb more moisture in the air, promoting the rapid hydrolysis of the cross-linking agent and the curing reaction of the rubber compound, and thus improving the overall curing speed of the silicone rubber compound.
[0169] According to Example 6 and Comparative Example 3 and combined with the data in Table 1, it can be seen that the degree of polymerization of the framework-type hygroscopic agent affects the curing speed of the rubber compound. When the degree of polymerization n>10 and m>10 of the framework-type hygroscopic agent, the curing speed of the rubber compound is less than 4 mm within 12 hours, not meeting the target requirements. This may be because when the degree of polymerization n>10 and m>10 of the framework-type hygroscopic agent, the framework-type hygroscopic agent may lose its hygroscopicity, resulting in a decrease in the curing speed of the rubber compound.
[0170] According to Example 6 and Examples 4-10 and combined with the data in Table 1, it can be seen that when the degree of polymerization n+m = 8 of the framework-type hygroscopic agent and n:m = (5-6):(3-2), the modified rubber compound has a fast curing speed, and the curing depth reaches 5 mm within 12 hours.
[0171] This may be because the polyoxyethylene chain segment in the framework-type hygroscopic agent is hydrophilic and has hygroscopicity, but the hydrophilicity and hygroscopicity of the framework-type hygroscopic agent decrease with the increase of the degree of polymerization n of the polyoxyethylene chain segment; while the polyoxypropylene chain segment in the framework-type hygroscopic agent is lipophilic, and the lipophilicity of the framework-type hygroscopic agent increases with the increase of the degree of polymerization m of the polyoxypropylene chain segment, that is, the compatibility between the framework-type hygroscopic agent and the rubber compound increases with the increase of the degree of polymerization m of the polyoxypropylene chain segment.
[0172] When n<m, the curing speed of the rubber compound decreases. It may be because when n<m, the framework-type hygroscopic agent shows relatively strong lipophilicity and relatively weak hydrophilicity. Although it has good compatibility with the colloid, its hygroscopicity is weak; when n>m, the framework-type hygroscopic agent shows relatively strong hydrophilicity and relatively weak lipophilicity. Although the framework-type hygroscopic agent has good hygroscopicity at this time, if the lipophilicity is too weak, the framework-type hygroscopic agent cannot be fully mixed with the colloid, which will also lead to a decrease in the curing speed of the rubber compound. When n+m = 8 and n:m = (5-6):(3-2), the framework-type hygroscopic agent not only has good hygroscopicity but also maintains good compatibility with the colloid. Therefore, when the degree of polymerization of the framework-type hygroscopic agent is within this range, the rubber compound can have excellent curing speed.
[0173] According to Example 6, Example 3, and Example 14, combined with the data in Table 1, the addition of a framework-type hygroscopic agent containing an epoxy end-capping group can effectively promote the hydrolysis of the crosslinking agent and increase the curing speed of the rubber compound. This may be because the epoxy end-capping group in the framework-type hygroscopic agent can cooperate with amino-containing silane coupling agents, crosslinking agents and other auxiliary agents at room temperature, improve the hydrophilicity of the basic rubber compound, further promote the hydrolysis and crosslinking of the crosslinking agent, and increase the curing speed of the rubber compound. However, when both ends of the framework-type hygroscopic agent are epoxy end-capping groups, it may cause excessive crosslinking of the colloid surface, affect the water absorption and curing of the rubber compound, and thus reduce the overall curing speed of the colloid.
[0174] According to Example 6 and Example 12 combined with the data in Table 1 and Table 2, the addition of coupling agents including primary amine silane coupling agents, secondary amine silane coupling agents, and tertiary amine silane coupling agents to the rubber has a faster overall curing speed than the addition of primary amine amino-containing silane coupling agents alone. This is because amino-containing silane coupling agents have the characteristics of high activity and self-catalytic polymerization. The addition of primary amine amino-containing silane coupling agents alone may cause the surface of the rubber to cure quickly and the surface drying time to be short, thereby affecting the water absorption and curing of the rubber inside, resulting in slow curing of the deep layer of the rubber.
[0175] According to Example 6 and Example 13 and the data in Table 1 and Table 2, when the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent, and the tertiary amine silane coupling agent in the coupling agent is in the range of (1-2): (1-2): (1-3), the rubber has a faster overall curing speed. This may be because the secondary amine silane coupling agent and the tertiary amine silane coupling agent can inhibit the high activity and self-catalytic polymerization characteristics of the primary amine silane coupling agent, slow down the curing speed of the rubber surface, enable the rubber interior to fully absorb water and cure, and improve the deep curing speed of the rubber, which is conducive to improving the overall curing speed of the rubber.
[0176] Table 3 Physical and chemical properties of quick-drying special adhesive
[0177]
[0178]
[0179] According to Example 6 and Comparative Examples 1-3 and combined with the data in Table 3, after adding the framework type hygroscopic agent, the extrudability of the rubber compound is improved to a certain extent. This may be because the polyoxypropylene segment in the framework type hygroscopic agent has lubricity, which is conducive to improving the extrudability of the rubber compound. As the degree of polymerization of the polyoxypropylene segment increases, the lubricity of the framework type hygroscopic agent increases, thereby further improving the extrudability of the rubber compound.
[0180] According to Example 6, Example 3, and Example 14, combined with the data in Table 3, the addition of a framework-type hygroscopic agent containing an epoxy-terminated group can effectively inhibit the yellowing of the rubber material, so that the color difference of the rubber material can still be maintained at a relatively low range after a long period of artificial accelerated aging. This may be because the amino-containing silane coupling agent added to the rubber material causes the rubber material to easily turn yellow under the action of ultraviolet rays, and the framework-type hygroscopic agent containing an epoxy-terminated group can inhibit the yellowing of the rubber material, which is conducive to keeping the color difference of the rubber material after long-term storage. Changes are not large.
[0181] According to Example 6 and Example 14 combined with the data in Table 3, the addition of a framework-type hygroscopic agent containing an epoxy end-capping group can effectively improve the elastic recovery rate of the rubber compound. This may be because the epoxy end-capping group in the framework-type hygroscopic agent can cooperate with auxiliary agents such as coupling agents and cross-linking agents at room temperature to form a uniform dynamic cross-linked network structure inside the rubber compound, which can not only effectively improve the bonding strength and bonding toughness inside the rubber compound, so that the rubber compound has a higher tensile modulus, but also further improve the bonding elasticity of the rubber compound, so that the rubber compound has a good elastic recovery rate.
[0182] This specific implementation manner is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make non-creative modifications to the specific implementation manner as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A quick-drying special adhesive for movable door and window systems, characterized by: It includes the following components in parts by mass: 60-80 parts of α,ω-dihydroxy polydimethylsiloxane; 15-30 parts of dimethyl silicone oil; 100-120 parts of reinforcing filler; 7-12 parts of cross-linking agent; Coupling agent 0.8-1.5 parts; Catalyst 0.07-0.12 parts; 4-12 parts of framework type moisture absorbent; Wherein, the coupling agent is an amino-containing silane coupling agent; the crosslinking agent is methyl tributylidene oxime silane; the framework-type moisture absorbent is specifically a single-end epoxy-terminated EO / PO block polyether, and its molecular formula is: CH3O(CH2CH2O) n (CH2CH(CH3)O) m CH2CHOCH2; The degree of polymerization of the framework-type desiccant is n+m=8, wherein n:m=(5-6):(3-2).
2. The quick-drying special adhesive for movable door and window system according to claim 1, characterized in that: The coupling agent includes a primary amine silane coupling agent, a secondary amine silane coupling agent and a tertiary amine silane coupling agent, wherein the mass ratio of the primary amine silane coupling agent, the secondary amine silane coupling agent and the tertiary amine silane coupling agent is in the range of (1-2): (1-2): (1-3).
3. The quick-drying special adhesive for movable door and window system according to claim 1, characterized in that: The viscosity range of the α,ω-dihydroxy polydimethylsiloxane is 50000-80000cps, and the viscosity range of the dimethyl silicone oil is 350-500cst.
4. The quick-drying special adhesive for movable door and window system according to claim 1, characterized in that: The reinforcing filler is any one of hydrophobic nano-calcium carbonate and hydrophobic fumed silica.
5. The quick-drying special adhesive for movable door and window system according to claim 1, characterized in that: The catalyst is any one of dibutyltin dilaurate and n-butyltin diacetate.
6. The method for preparing the quick-drying special adhesive for movable door and window system according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Stir α, ω-dihydroxy polydimethylsiloxane and dimethyl silicone oil evenly, slowly add reinforcing filler, raise the temperature to above 130° C., maintain vacuum state and stir evenly to obtain a base rubber material; S2, introduce inert gas to balance the vacuum, wait for the base rubber to cool to room temperature, add the cross-linking agent and the framework type moisture absorbent, maintain the vacuum state and stir evenly to obtain a mixed rubber; S3, introducing inert gas to balance the vacuum, after the mixed rubber obtained in step S2 is cooled to room temperature, adding coupling agent and catalyst, maintaining the vacuum state and stirring evenly to obtain the target rubber; S4. Inert gas is introduced to balance the vacuum, and then the target rubber material is extruded through a press and sealed for storage.