A method for preparing plant-derived aerogel fiber
Through β-cyclodextrin inclusion and oxidation modification treatment combined with aminolated silica aerogel grafting technology, the problem of insufficient antibacterial and hygroscopicity of synthetic fibers was solved, and plants with high efficiency antibacterial and good textile properties were prepared. Source aerogel fiber.
Patent Information
- Application Number
- CN202410394410.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-02
AI Technical Summary
Existing synthetic fibers have defects in hygroscopicity and antibacterial properties. Plant extracts are prone to loss and have poor binding effect, resulting in a decrease in fiber strength and a short-lasting antibacterial effect.
β-cyclodextrin inclusion of plant extracts, and through oxidative modification treatment and aminated silica aerogel grafting technology, plant-source modified aerogel fiber is formed to improve the high temperature resistance and antibacterial persistence of the extracts. sex.
The fiber has good spinning and long-lasting antibacterial effect, and the antibacterial rate of many bacteria is high, the fiber breathability and hygroscopicity are also improved, and the antibacterial loss rate is low after washing.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic fibers, and in particular relates to a method for preparing plant-derived aerogel fibers. Background Art
[0002] Synthetic fibers are made of synthetic polymer compounds. Common synthetic fibers include polyester, nylon, polypropylene, acrylic, spandex, etc. Among them, polyester raw materials are cheap and have excellent performance, ranking first among synthetic fibers. Polyester and nylon have good strength and wear resistance, but poor hygroscopicity, easy to generate static electricity, low comfort when wearing, hot and stuffy, and easy to breed bacteria, which will pose a certain threat to human health. In order to give the fiber an antibacterial effect, researchers often blend antibacterial agents with polymer chips for spinning or use post-finishing methods to treat the fiber.
[0003] Most plant extracts have antibacterial effects and can be used as natural antibacterial agents. In the prior art, researchers have added plant extracts to synthetic fibers to give them natural antibacterial properties. For example, in the patent number "CN202111519624.0" entitled "Polyester fiber preparation method containing honeysuckle plant Chinese medicine antibacterial, antioxidant and skin care", high temperature resistant natural plant Chinese medicine powder is blended with PET slices to make masterbatch, and then the plant Chinese medicine antibacterial, antioxidant and skin care PET masterbatch is blended with PET slices for melt spinning to make polyester fiber; the patent number "CN201911076259.3" entitled "A plant functional polyester filament and its preparation method" heats the PET slices until they are melted, first add antioxidants and dispersants and stir, then add protective agents and plant extracts, mix at high speed, and finally add modifiers, mix evenly to obtain a mixture, and melt spin after extrusion granulation.
[0004] In the above patents, plant extracts are directly made into masterbatches and then melt-spun. However, most plant extracts are not resistant to high temperatures and are easily lost when directly added to fibers, which can easily cause a decrease in fiber strength and affect the spinnability of the fibers. Secondly, the binding effect between plant extracts and fibers is poor, and the antibacterial properties decrease after repeated washings, and the antibacterial effect is not long-lasting. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a method for preparing plant-derived aerogel fibers, which achieves the invention purpose of reducing the water washing loss of plant extracts in the fibers and improving the high temperature resistance of the plant extracts.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A method for preparing plant-derived aerogel fibers comprises the following steps:
[0008] S1. Inclusion of plant extracts
[0009] Add β-cyclodextrin to deionized water and stir for 10-20 minutes, then add the plant extract, continue stirring for 10-20 minutes, and ultrasonically treat at 40-50°C for 2-3 hours. After the reaction is completed, rotary evaporate at 80-90°C to 35-40%, cool to room temperature, and then place in an environment of 0-10°C for 4-6 hours to precipitate crystals. Wash the crystals and dry them to obtain a plant extract inclusion complex.
[0010] Preferably, the plant extract is one or more of wormwood extract, seaweed extract, tea extract, ginkgo extract, honeysuckle extract, geranium extract, peppermint extract, etc., and the particle size is 100-200nm.
[0011] Preferably, the mass ratio of the β-cyclodextrin to the plant extract is 2-3:1; the mass ratio of the β-cyclodextrin to deionized water is 1:6-8.
[0012] Preferably, the frequency of the ultrasonic treatment is 80 to 140 kHz.
[0013] Preferably, the drying process is carried out at a temperature of 70 to 80° C. and for a time of 4 to 6 hours.
[0014] S2, Oxidation
[0015] The plant extract inclusion compound is placed in 6 to 8 times of deionized water, and stirred at room temperature for 20 to 30 minutes to obtain a plant extract inclusion compound solution;
[0016] Sodium periodate and deionized water are placed in a reaction kettle at a ratio of 1:9-11, and ultrasonically dissolved at 45-50° C. for 15-20 minutes at an ultrasonic frequency of 60-80 kHz to prepare a sodium periodate solution;
[0017] The sodium periodate solution is added to the plant extract inclusion compound solution, and ultrasonic reaction is carried out at 35-40° C. for 2-3 hours, and the ultrasonic frequency is 160-180 kHz, and the hydroxyl groups on the outer layer of β-cyclodextrin are oxidized to aldehyde groups. After the reaction is completed, ethylene glycol is added to terminate the reaction, and then anhydrous ethanol is added and stirred for 8-12 minutes, centrifuged and washed with an ethanol solution with a concentration of 80-90wt% for 3-4 times, and dried to obtain an oxidatively modified inclusion compound;
[0018] Preferably, the molar ratio of sodium periodate to β-cyclodextrin in the plant extract inclusion complex is 2 to 4:1.
[0019] Preferably, the amount of ethylene glycol added is 55-60% of the mass of sodium periodate.
[0020] Preferably, the centrifugal speed is 4000-6000 r / min, and the time is 5-8 min.
[0021] Preferably, the drying process is carried out at a temperature of 70 to 80° C. and for a time of 4 to 6 hours.
[0022] S3. Preparation of Aminated Silica Aerogel
[0023] Mix ethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol, stir for 15-20 minutes, add 1-2 mol / L hydrochloric acid solution to adjust the pH to 2-4, heat to 40-50°C and react for 50-60 minutes, add 2-5% HF solution and aminosilane coupling agent and continue to react for 30-40 minutes, and after the reaction, use 1-3% ammonia water to adjust the pH to 7-8 and let stand for 60-80 minutes to form a gel;
[0024] The gel was placed in a high-pressure reactor for aging, then washed with n-hexane and dried at 100-120°C for 2-4 hours to obtain amino-modified silica aerogel with a specific surface area of 635.2-764 m 2 / g, the porosity is greater than 98%, and the average pore size is 12-15nm.
[0025] Preferably, the molar ratio of tetraethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol is 2-3:10-14:0.8-1.5:1-2.
[0026] Preferably, the amount of HF solution added is 3-6 wt % of ethyl orthosilicate.
[0027] Preferably, the aminosilane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane, and the added amount is 9-12wt% of ethyl orthosilicate.
[0028] S4. Grafting
[0029] The oxidatively modified inclusion compound and deionized water are mixed in a ratio of 1:7-10, stirred at 40-50°C for 10-15 minutes at a stirring rate of 500-600 r / min, and then the amino-modified silica aerogel and ammonium sulfate are added, stirred for reaction for 1-2 hours at a stirring rate of 200-300 r / min, the amino groups of the amino-modified silica aerogel and the aldehyde groups of the oxidized β-cyclodextrin produce a Schiff base reaction, ethylene glycol is added to terminate the reaction, the mixture is concentrated under reduced pressure, centrifuged and washed, dried at 80-100°C for 1-2 hours, and then ground to 2-5 μm to obtain a plant-derived modified aerogel.
[0030] The amount of the amino-modified silica aerogel added is 32-37 wt % of the oxidatively modified inclusion compound, and the amount of the ammonium sulfate added is 1.5-3 wt % of the oxidatively modified inclusion compound.
[0031] Preferably, the centrifugal speed is 4000-6000 r / min, and the time is 5-8 min.
[0032] In aqueous solution, the grafted amino groups doped in the aminated silica aerogel are positively charged, while the aldehyde groups on the surface of the oxidatively modified inclusion complex are negatively charged, and the adsorption force between the two is stronger. The micropores of the aminated silica aerogel can adsorb more oxidatively modified inclusion complexes. At the same time, under the catalytic action of ammonium sulfate, a Schiff base reaction occurs between the two, and the oxidatively modified inclusion complexes are grafted into the micropores of the aminated silica aerogel to obtain a plant-derived modified aerogel.
[0033] S5. Blending and granulation
[0034] The polymer slices, the plant-derived modified aerogel and the additives are blended and granulated by a twin-screw extruder, and the plant-derived modified aerogel functional masterbatch is obtained after drying.
[0035] Preferably, the polymer slice is one of PET slice, PP slice, PA6 slice and the like.
[0036] Preferably, the mass ratio of the plant-derived modified aerogel to the polymer slice is 16-20:80-84.
[0037] Preferably, the auxiliary agents are EBS dispersant, antioxidant and ethylene glycol dimethacrylate, wherein the addition amount of EBS dispersant is 0.5-1.5wt% of the polymer slice, the addition amount of antioxidant is 0.3-0.6wt% of the polymer slice, and the addition amount of ethylene glycol dimethacrylate is 2-3wt% of the polymer slice.
[0038] S6. Spinning
[0039] The plant-derived modified aerogel functional masterbatch is mixed with polymer slices and then melt-spun to obtain the plant-derived aerogel fiber of the present invention.
[0040] Preferably, the mass ratio of the plant-derived modified aerogel functional masterbatch to the polymer chips is 8-12:88-92.
[0041] Due to the adoption of the above technical solution, the technical effects achieved by the present invention are:
[0042] 1. The plant-derived aerogel fiber prepared by the present invention has good spinnability and natural antibacterial effect, wherein the antibacterial rate against Staphylococcus aureus is 98.7-99.3%, the antibacterial rate against Candida albicans is 97.7-98.4%, and the antibacterial rate against Escherichia coli is 98.8-99.6% (determined in accordance with GB / T 20944.3-2008), which meets the antibacterial standards for textiles and can be applied to clothing, furniture, automotive products and other fields.
[0043] 2. The plant-derived aerogel fiber prepared by the present invention has improved air permeability and moisture absorption effect due to the addition of aerogel with a porous structure and a variety of plant extracts, which makes up for the defect of synthetic fibers being stuffy and airtight, and is more comfortable to wear.
[0044] 3. The plant-derived modified aerogel of the present invention has a thermal weight loss of 1.52-1.87% at 300°C and has a sustained release effect. The functionality of the plant extract is also more durable and is not easily lost after washing.
[0045] 4. The present invention includes plant extracts, and then oxidizes the plant extract inclusion compound to modify aldehyde groups on the surface. The oxidatively modified inclusion compound with modified aldehyde groups on the surface is grafted onto the amino-modified silica aerogel through a Schiff base reaction, thereby improving the high temperature resistance of the inclusion compound and enhancing the antibacterial and long-lasting effect of the plant extract. After the plant-derived aerogel fiber of the present invention is washed 50 times, the antibacterial loss rate is less than 2%. DETAILED DESCRIPTION
[0046] The present invention is further described below in conjunction with specific embodiments.
[0047] Example 1
[0048] A method for preparing plant-derived aerogel fibers comprises the following steps:
[0049] S1. Inclusion of plant extracts
[0050] Add β-cyclodextrin to deionized water and stir for 15 minutes, then add the plant extract, continue stirring for 15 minutes, and ultrasonically treat at 45°C for 3 hours. After the reaction is completed, rotary evaporate at 85°C to 37%, cool to room temperature, and then place in an environment of 5°C for 5 hours to precipitate crystals. Wash the crystals and dry them to obtain a plant extract inclusion complex.
[0051] The plant extract is wormwood extract, seaweed extract and tea extract in a mass ratio of 1:1:1, and the particle size is 150nm.
[0052] The mass ratio of the β-cyclodextrin to the plant extract is 2.2:1; the mass ratio of the β-cyclodextrin to deionized water is 1:7.
[0053] The frequency of the ultrasonic treatment was 100 kHz.
[0054] The drying process was carried out at a temperature of 75° C. and for 5 hours.
[0055] S2, Oxidation
[0056] The plant extract inclusion compound was placed in 7 times deionized water and stirred at room temperature for 25 minutes to obtain a plant extract inclusion compound solution;
[0057] Sodium periodate and deionized water were placed in a reaction kettle at a ratio of 1:10, and ultrasonically dissolved at 45°C for 20 minutes at an ultrasonic frequency of 70kHz to prepare a sodium periodate solution;
[0058] The sodium periodate solution was added to the plant extract inclusion compound solution, and ultrasonic reaction was carried out at 35°C for 2.5 hours with an ultrasonic frequency of 170kHz. After the reaction was completed, ethylene glycol was added to terminate the reaction, and then anhydrous ethanol was added and stirred for 10 minutes. The solution was centrifuged and washed with an ethanol solution with a concentration of 85wt% for 4 times, and then dried to obtain an oxidatively modified inclusion compound.
[0059] The molar ratio of sodium periodate to beta-cyclodextrin in the plant extract inclusion complex is 3:1.
[0060] The added amount of ethylene glycol is 58% of the mass of sodium periodate.
[0061] The centrifugal speed is 5000 r / min and the time is 6 min.
[0062] The drying process was carried out at a temperature of 75° C. and for 5 hours.
[0063] S3. Preparation of Aminated Silica Aerogel
[0064] TEOS, deionized water, N,N-dimethylformamide and anhydrous ethanol were mixed and stirred for 17 minutes, and then a 1.5 mol / L hydrochloric acid solution was added to adjust the pH to 3, and the temperature was raised to 45°C for reaction for 55 minutes, and then a 4% HF solution and an aminosilane coupling agent were added to continue the reaction for 35 minutes. After the reaction, a 2% ammonia solution was used to adjust the pH to 7.5 and the mixture was allowed to stand for 70 minutes to form a gel;
[0065] The gel was aged in a high-pressure reactor, washed with n-hexane, and dried at 110 °C for 3 h to obtain amino-modified silica aerogel with a specific surface area of 764 m 2 / g, the porosity is 99.3% and the average pore size is 13nm.
[0066] The molar ratio of the tetraethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol is 2.4:12:1.2:1.6.
[0067] The amount of the HF solution added is 4.5 wt % of ethyl orthosilicate.
[0068] The aminosilane coupling agent is 3-aminopropyltriethoxysilane, and the added amount is 10wt% of ethyl orthosilicate.
[0069] S4. Grafting
[0070] The oxidatively modified inclusion complex and deionized water were mixed in a ratio of 1:8, stirred at 45°C for 12 min at a stirring rate of 550 r / min, and then amino-modified silica aerogel and ammonium sulfate were added. The reaction was stirred for 1.5 h at a stirring rate of 250 r / min. Ethylene glycol was added to terminate the reaction, and the mixture was concentrated under reduced pressure, centrifuged and washed. After drying at 90°C for 2 h, the mixture was ground to 3 μm to obtain a plant-derived modified aerogel.
[0071] The amount of the amino-modified silica aerogel added is 35 wt % of the oxidatively modified inclusion compound, and the amount of the ammonium sulfate added is 2 wt % of the oxidatively modified inclusion compound.
[0072] The centrifugal speed is 5000 r / min and the time is 6 min.
[0073] The plant-derived modified aerogel has a thermal weight loss of 1.52% at 300°C.
[0074] S5. Blending and granulation
[0075] PET slices, plant-derived modified aerogel and additives are blended and granulated by a twin-screw extruder, and then dried to obtain plant-derived modified aerogel functional masterbatch.
[0076] The mass ratio of the plant-derived modified aerogel to the PET slice is 18:82.
[0077] The auxiliary agents are EBS dispersant, antioxidant and ethylene glycol dimethacrylate, wherein the addition amount of EBS dispersant is 1wt% of the PET slice, the addition amount of antioxidant is 0.4wt% of the PET slice, and the addition amount of ethylene glycol dimethacrylate is 2.5wt% of the PET slice.
[0078] S6. Spinning
[0079] The plant-derived modified aerogel functional masterbatch is mixed with PET chips and then melt-spun to obtain the plant-derived aerogel fiber of the present invention.
[0080] The mass ratio of plant-derived modified aerogel functional masterbatch and PET chips is 10:90.
[0081] The plant-derived aerogel fiber prepared in Example 1 has a breaking strength of 3.71 cN / dtex, an elongation at break of 47%, a fiber regain of 3.6%, an antibacterial rate against Staphylococcus aureus of 99%, an antibacterial rate against Candida albicans of 98.1%, an antibacterial rate against Escherichia coli of 99.1%, and an antibacterial loss rate of 0.9% after washing 50 times.
[0082] Example 2
[0083] A method for preparing plant-derived aerogel fibers comprises the following steps:
[0084] S1. Inclusion of plant extracts
[0085] Add β-cyclodextrin to deionized water and stir for 10 minutes, then add the plant extract, continue stirring for 10 minutes, and ultrasonically treat at 40°C for 2 hours. After the reaction is completed, rotary evaporate at 80°C to 35%, cool to room temperature, and then place in an environment of 0°C for 4 hours to precipitate crystals. Wash the crystals and dry them to obtain a plant extract inclusion complex.
[0086] The plant extracts are wormwood extract, tea extract and ginkgo extract in a mass ratio of 1:1:1, and the particle size is 100 nm.
[0087] The mass ratio of the β-cyclodextrin to the plant extract is 2:1; the mass ratio of the β-cyclodextrin to deionized water is 1:6.
[0088] The frequency of the ultrasonic treatment was 80 kHz.
[0089] The drying process was carried out at a temperature of 70° C. and for a period of 6 hours.
[0090] S2, Oxidation
[0091] The plant extract inclusion compound was placed in 6 times deionized water and stirred at room temperature for 20 minutes to obtain a plant extract inclusion compound solution;
[0092] Sodium periodate and deionized water were placed in a reaction kettle at a ratio of 1:9, and ultrasonically dissolved at 45°C for 15 minutes at an ultrasonic frequency of 60 kHz to prepare a sodium periodate solution;
[0093] The sodium periodate solution was added to the plant extract inclusion compound solution, and ultrasonic reaction was carried out at 35°C for 2 hours with an ultrasonic frequency of 160kHz. After the reaction was completed, ethylene glycol was added to terminate the reaction, and then anhydrous ethanol was added and stirred for 8 minutes. The solution was centrifuged and washed three times with an ethanol solution having a concentration of 80wt%, and then dried to obtain an oxidatively modified inclusion compound.
[0094] The molar ratio of sodium periodate to beta-cyclodextrin in the plant extract inclusion complex is 2:1.
[0095] The added amount of ethylene glycol is 55% of the mass of sodium periodate.
[0096] The centrifugal speed is 4000 r / min and the time is 5 min.
[0097] The drying process was carried out at a temperature of 70° C. and for a period of 6 hours.
[0098] S3. Preparation of Aminated Silica Aerogel
[0099] TEOS, deionized water, N,N-dimethylformamide and anhydrous ethanol were mixed and stirred for 15 minutes, and then 1 mol / L hydrochloric acid solution was added to adjust the pH to 2, and the temperature was raised to 40°C for reaction for 50 minutes, and then 2% HF solution and aminosilane coupling agent were added to continue the reaction for 30 minutes. After the reaction, 1% ammonia water was used to adjust the pH to 7 and the mixture was allowed to stand for 60 minutes to form a gel;
[0100] The gel was aged in a high-pressure reactor, washed with n-hexane, and dried at 100 °C for 2 h to obtain amino-modified silica aerogel with a specific surface area of 635.2 m 2 / g, the porosity is 98.3% and the average pore size is 15nm.
[0101] The molar ratio of the tetraethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol is 2:10:0.8:1.
[0102] The amount of the HF solution added is 3 wt % of ethyl orthosilicate.
[0103] The aminosilane coupling agent is 3-aminopropyltriethoxysilane, and the added amount is 9wt% of ethyl orthosilicate.
[0104] S4. Grafting
[0105] The oxidatively modified inclusion complex and deionized water were mixed in a ratio of 1:7, stirred at 40°C for 10 min at a stirring rate of 500 r / min, and then amino-modified silica aerogel and ammonium sulfate were added. The reaction was stirred for 1 h at a stirring rate of 200 r / min. Ethylene glycol was added to terminate the reaction, and the mixture was concentrated under reduced pressure, centrifuged and washed. After drying at 80°C for 1 h, it was ground to 5 μm to obtain a plant-derived modified aerogel.
[0106] The amount of the amino-modified silica aerogel added is 32 wt % of the oxidatively modified inclusion compound, and the amount of the ammonium sulfate added is 1.5 wt % of the oxidatively modified inclusion compound.
[0107] The centrifugal speed is 4000 r / min and the time is 5 min.
[0108] The plant-derived modified aerogel has a thermal weight loss of 1.87% at 300°C.
[0109] S5. Blending and granulation
[0110] PET slices, plant-derived modified aerogel and additives are blended and granulated by a twin-screw extruder, and then dried to obtain plant-derived modified aerogel functional masterbatch.
[0111] The mass ratio of the plant-derived modified aerogel to the PET slice is 16:84.
[0112] The auxiliary agents are EBS dispersant, antioxidant and ethylene glycol dimethacrylate, wherein the addition amount of EBS dispersant is 0.5wt% of the PET slice, the addition amount of antioxidant is 0.3wt% of the PET slice, and the addition amount of ethylene glycol dimethacrylate is 2wt% of the PET slice.
[0113] S6. Spinning
[0114] The plant-derived modified aerogel functional masterbatch is mixed with PET chips and then melt-spun to obtain the plant-derived aerogel fiber of the present invention.
[0115] The mass ratio of plant-derived modified aerogel functional masterbatch and PET chips is 8:92.
[0116] The plant-derived aerogel fiber prepared in Example 2 has a breaking strength of 3.55 cN / dtex, an elongation at break of 42%, a fiber regain of 3.2%, an antibacterial rate against Staphylococcus aureus of 98.7%, an antibacterial rate against Candida albicans of 97.7%, an antibacterial rate against Escherichia coli of 98.8%, and an antibacterial loss rate of 1.6% after washing 50 times.
[0117] Example 3
[0118] A method for preparing plant-derived aerogel fibers comprises the following steps:
[0119] S1. Inclusion of plant extracts
[0120] Add β-cyclodextrin to deionized water and stir for 20 minutes, then add the plant extract, continue stirring for 20 minutes, and ultrasonically treat at 50°C for 3 hours. After the reaction is completed, rotary evaporate to 40% at 90°C, cool to room temperature, and then place in an environment of 10°C for 6 hours to precipitate crystals. Wash the crystals and dry them to obtain a plant extract inclusion complex.
[0121] The plant extracts are wormwood extract, honeysuckle extract and geranium extract in a mass ratio of 1:1:1, and have a particle size of 200 nm.
[0122] The mass ratio of the β-cyclodextrin to the plant extract is 3:1; the mass ratio of the β-cyclodextrin to deionized water is 1:8.
[0123] The frequency of the ultrasonic treatment was 140 kHz.
[0124] The drying process was carried out at a temperature of 80° C. and for a period of 4 hours.
[0125] S2, Oxidation
[0126] The plant extract inclusion compound was placed in 8 times deionized water and stirred at room temperature for 30 minutes to obtain a plant extract inclusion compound solution;
[0127] Sodium periodate and deionized water were placed in a reaction kettle at a ratio of 1:11, and ultrasonically dissolved at 50°C for 20 minutes at an ultrasonic frequency of 80kHz to prepare a sodium periodate solution;
[0128] The sodium periodate solution was added to the plant extract inclusion compound solution, and ultrasonic reaction was carried out at 40°C for 3 hours with an ultrasonic frequency of 180kHz. After the reaction was completed, ethylene glycol was added to terminate the reaction, and then anhydrous ethanol was added and stirred for 12 minutes. The solution was centrifuged and washed with a 90wt% ethanol solution for 4 times, and then dried to obtain an oxidatively modified inclusion compound.
[0129] The molar ratio of sodium periodate to beta-cyclodextrin in the plant extract inclusion complex is 4:1.
[0130] The added amount of ethylene glycol is 60% of the mass of sodium periodate.
[0131] The centrifugal speed is 6000 r / min and the time is 8 min.
[0132] The drying process was carried out at a temperature of 80° C. and for a period of 6 hours.
[0133] S3. Preparation of Aminated Silica Aerogel
[0134] TEOS, deionized water, N,N-dimethylformamide and anhydrous ethanol were mixed and stirred for 20 minutes, and then a 2 mol / L hydrochloric acid solution was added to adjust the pH to 4, and the temperature was raised to 50°C for reaction for 60 minutes, and then a 5% by mass HF solution and an aminosilane coupling agent were added to continue the reaction for 40 minutes. After the reaction, a 3% by mass ammonia solution was used to adjust the pH to 8 and the mixture was allowed to stand for 80 minutes to form a gel;
[0135] The gel was aged in a high-pressure reactor, washed with n-hexane, and dried at 120 °C for 4 h to obtain amino-modified silica aerogel with a specific surface area of 713.8 m 2 / g, the porosity is 98.7% and the average pore size is 12nm.
[0136] The molar ratio of the tetraethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol is 3:14:1.5:2.
[0137] The amount of the HF solution added is 6 wt % of ethyl orthosilicate.
[0138] The aminosilane coupling agent is 3-aminopropyltrimethoxysilane, and the added amount is 12wt% of ethyl orthosilicate.
[0139] S4. Grafting
[0140] The oxidatively modified inclusion complex and deionized water were mixed in a ratio of 1:10, stirred at 50°C for 15 min at a stirring rate of 600 r / min, and then amino-modified silica aerogel and ammonium sulfate were added. The reaction was stirred for 2 h at a stirring rate of 300 r / min. Ethylene glycol was added to terminate the reaction, and the mixture was concentrated under reduced pressure, centrifuged and washed. After drying at 100°C for 2 h, it was ground to 2 μm to obtain a plant-derived modified aerogel.
[0141] The amount of the amino-modified silica aerogel added is 37 wt % of the oxidatively modified inclusion compound, and the amount of the ammonium sulfate added is 3 wt % of the oxidatively modified inclusion compound.
[0142] The centrifugal speed is 6000 r / min and the time is 8 min.
[0143] The plant-derived modified aerogel has a thermal weight loss of 1.69% at 300°C.
[0144] S5. Blending and granulation
[0145] PET slices, plant-derived modified aerogel and additives are blended and granulated by a twin-screw extruder, and then dried to obtain plant-derived modified aerogel functional masterbatch.
[0146] The mass ratio of the plant-derived modified aerogel to the PET slice is 20:80.
[0147] The auxiliary agents are EBS dispersant, antioxidant and ethylene glycol dimethacrylate, wherein the addition amount of EBS dispersant is 1.5wt% of the PET slice, the addition amount of antioxidant is 0.6wt% of the PET slice, and the addition amount of ethylene glycol dimethacrylate is 3wt% of the PET slice.
[0148] S6. Spinning
[0149] The plant-derived modified aerogel functional masterbatch is mixed with PET chips and then melt-spun to obtain the plant-derived aerogel fiber of the present invention.
[0150] The mass ratio of plant-derived modified aerogel functional masterbatch and PET chips is 12:88.
[0151] The plant-derived aerogel fiber prepared in Example 3 has a breaking strength of 3.64 cN / dtex, an elongation at break of 44%, a fiber regain of 3.7%, an antibacterial rate against Staphylococcus aureus of 99.3%, an antibacterial rate against Candida albicans of 98.4%, an antibacterial rate against Escherichia coli of 99.6%, and an antibacterial loss rate of 1.4% after washing 50 times.
[0152] Comparative Example 1
[0153] The representative Example 1 was selected, the plant-derived modified aerogel was removed, and an equal amount of the oxidatively modified inclusion compound was directly added during the blending and granulation process, and the rest was consistent with Example 1, as Comparative Example 1. During the granulation process, the oxidatively modified inclusion compound had poor high temperature resistance, a large amount of carbonization loss, poor antibacterial effect, fiber breaking strength of 2.63 cN / dtex, elongation at break of 20%, and fiber strength also decreased significantly; the antibacterial rate against Staphylococcus aureus was 36%, the antibacterial rate against Candida albicans was 33%, the antibacterial rate against Escherichia coli was 34%, and the fiber regain was 1.2%.
[0154] Comparative Example 2
[0155] The representative Example 1 was selected, the S2 step was removed, and the same amount of plant extract inclusion compound was directly used in the S4 grafting step, and the rest was consistent with Example 1, as Comparative Example 2. The fiber prepared in Comparative Example 2 had a breaking strength of 3.49 cN / dtex, an elongation at break of 41%, a fiber regain of 3.45%, an antibacterial rate of 98.7% against Staphylococcus aureus, an antibacterial rate of 98% against Candida albicans, and an antibacterial rate of 98.9% against Escherichia coli, and an antibacterial loss rate of 15.4% after 50 washings.
[0156] In Comparative Example 2, since the plant extract inclusion compound has not modified the aldehyde group, the Schiff base reaction cannot occur. The plant extract inclusion compound and the amino-containing silica aerogel are combined by physical adsorption, and the interaction force is weak. After multiple water washings, the plant extract is lost and the antibacterial function is reduced.
[0157] In Example 1-3, the plant extract is included, and then the plant extract inclusion compound is oxidized to modify the aldehyde group on the surface. The oxidatively modified inclusion compound with the surface modified aldehyde group is grafted onto the amino-modified silica aerogel through a Schiff base reaction to improve the high temperature resistance of the inclusion compound. At the same time, the grafting reaction of the two enhances the antibacterial and long-lasting effect of the plant extract, and the antibacterial effect is still good after multiple water washings.
[0158] Unless otherwise specified, the ratios and percentages described in the present invention are all weight ratios and weight percentages; and the raw materials are all commercially available.
[0159] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing plant-derived aerogel fibers, characterized in that: The preparation method includes inclusion, oxidation, preparation, grafting, blending granulation and spinning of plant extracts, amination of silica aerogels; The inclusion of the plant extract comprises the following steps: adding β-cyclodextrin to deionized water and stirring for 10 to 20 minutes, then adding the plant extract, continuing stirring for 10 to 20 minutes, ultrasonically treating at 40 to 50° C. for 2 to 3 hours, rotary evaporating at 80 to 90° C. to 35 to 40 wt% after the reaction is completed, cooling to room temperature, and then placing in an environment of 0 to 10° C. for 4 to 6 hours to precipitate crystals, washing the crystals and drying them to obtain a plant extract inclusion compound; The oxidation comprises adding a sodium periodate solution to a plant extract inclusion compound solution, subjecting the solution to an ultrasonic reaction at 35-40° C. for 2-3 hours and an ultrasonic frequency of 160-180 kHz, oxidizing the hydroxyl groups on the outer layer of β-cyclodextrin to aldehyde groups, adding ethylene glycol to terminate the reaction after the reaction is completed, adding anhydrous ethanol and stirring for 8-12 minutes, centrifuging and washing with an ethanol solution having a concentration of 80-90wt% for 3-4 times, and drying to obtain an oxidatively modified inclusion compound; The molar ratio of sodium periodate to β-cyclodextrin in the plant extract inclusion complex is 2 to 4:1; The amount of ethylene glycol added is 55-60% of the mass of sodium periodate; The preparation of the aminated silica aerogel is as follows: tetraethyl orthosilicate, deionized water, N,N-dimethylformamide, and anhydrous ethanol are mixed, stirred for 15 to 20 minutes, then 1 to 2 mol / L hydrochloric acid solution is added to adjust the pH to 2 to 4, the temperature is raised to 40 to 50° C. and the reaction is carried out for 50 to 60 minutes, then 2 to 5% by mass HF solution and aminosilane coupling agent are added to continue the reaction for 30 to 40 minutes, and after the reaction is completed, the pH is adjusted to 7 to 8 with 1 to 3% by mass ammonia water and the reaction is allowed to stand for 60 to 80 minutes to form a gel; The gel is placed in a high pressure reactor for aging, then washed with n-hexane, and dried at 100-120° C. for 2-4 hours to obtain an amino-modified silica aerogel; The grafting comprises mixing the oxidatively modified inclusion compound and deionized water in a mass ratio of 1:7-10, stirring at 40-50° C. for 10-15 min at a stirring rate of 500-600 r / min, adding amino-modified silica aerogel and ammonium sulfate, stirring for 1-2 h at a stirring rate of 200-300 r / min, adding ethylene glycol to terminate the reaction, concentrating under reduced pressure, centrifuging and washing, drying at 80-100° C. for 1-2 h, and grinding to 2-5 μm to obtain a plant-derived modified aerogel; The blending and granulation is to blend the polymer slices, the plant-derived modified aerogel and the additives, and then use a twin-screw extruder to granulate, and then dry to obtain the plant-derived modified aerogel functional masterbatch; The polymer slice is one of PET slice, PP slice and PA6 slice; The mass ratio of the plant-derived modified aerogel to the polymer slice is 16-20:80-84.
2. The method for preparing a plant-derived aerogel fiber according to claim 1, characterized in that: The molar ratio of the tetraethyl orthosilicate, deionized water, N,N-dimethylformamide and anhydrous ethanol is 2-3:10-14:0.8-1.5:1-2; The amount of HF solution added is 3-6wt% of ethyl orthosilicate; The aminosilane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and N-β (aminoethyl)-γ-aminopropyltrimethoxysilane, and the added amount is 9-12wt% of ethyl orthosilicate.
3. The method for preparing a plant-derived aerogel fiber according to claim 1, characterized in that: The amount of the amino-modified silica aerogel added is 32-37 wt % of the oxidatively modified inclusion compound, and the amount of the ammonium sulfate added is 1.5-3 wt % of the oxidatively modified inclusion compound.
4. The method for preparing a plant-derived aerogel fiber according to claim 1, characterized in that: The auxiliary agents are EBS dispersant, antioxidant and ethylene glycol dimethacrylate, wherein the addition amount of EBS dispersant is 0.5-1.5wt% of the polymer slice, the addition amount of antioxidant is 0.3-0.6wt% of the polymer slice, and the addition amount of ethylene glycol dimethacrylate is 2-3wt% of the polymer slice.
5. The method for preparing a plant-derived aerogel fiber according to claim 1, characterized in that: The spinning comprises mixing plant-derived modified aerogel functional masterbatch with polymer slices and then melt-spinning to obtain plant-derived aerogel fibers; The mass ratio of plant-derived modified aerogel functional masterbatch to polymer chips is 8-12:88-92.
Citation Information
Patent Citations
Plant functional polyester filament and preparation method thereof
CN110863252A
Preparation method of antibacterial, antioxidant and skincare polyester fiber containing honeysuckle plant traditional Chinese medicine
CN114164517A
Preparation method of plant-source long-acting mosquito-repellent composite functional filament
CN114150392A
Preparation method of multifunctional plant source composite material for fiber spinning
CN115506042A
Preparation method of plant source aerogel modified lightweight functional PA6 fiber
CN116163028A