GaN HEMT device for radiation damage detection and its detection and manufacturing method
Through electroluminescence technology and interdigitated gear electrode design, the performance stability problem of GaN HEMT devices in a radiation environment has been solved, systematic and accurate detection of device radiation damage has been achieved, and the accuracy of device reliability evaluation has been improved.
Patent Information
- Application Number
- CN202410751811.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The existing technology lacks a systematic and comprehensive radiation damage characterization method, which causes the performance and stability of GaN HEMT devices to be affected in radiation environments, making it difficult to conduct in-depth research on device damage and failure mechanisms caused by radiation.
The luminescence wavelength and intensity data of the device are collected in the vertical and horizontal directions by means of electroluminescence. The characteristic luminescence wavelength and intensity are used for analysis and comparison to identify the type and location of defects in the material and device after irradiation. The design of the interdigitated gear electrode is adopted Improve collection range and accuracy.
It achieves the precise identification of defect types and locations of GaN HEMT devices after irradiation, provides an in-depth understanding of the radiation damage mechanism, and improves the accuracy of device reliability assessment.
Smart Images

Figure CN118335789B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of radiation damage detection and analysis of semiconductor devices, and in particular relates to a GaN HEMT device for radiation damage detection and a detection and manufacturing method thereof. Background Art
[0002] Gallium nitride (GaN)-based high electron mobility transistors (HEMTs) are considered to have significant application advantages in high-frequency, high-power, high-temperature, and high-voltage environments due to their unique wide-bandgap semiconductor material properties. This advantage combined with their excellent radiation resistance makes these devices have great application potential in key areas such as satellites, space exploration, and nuclear reactors. However, in different aerospace application scenarios, the radiation performance and working stability of gallium nitride HEMT devices still have major problems, such as low single-particle burnout voltage and threshold voltage instability. Theoretical and experimental studies have shown that wide-bandgap gallium nitride materials have radiation resistance characteristics such as high atomic displacement energy. In the actual production process, due to the complexity of the manufacturing process and structure tape-out, its radiation resistance will be affected. For example, in gallium nitride materials manufactured by heteroepitaxial growth technology, there are a certain amount of point defects and line defects, and even large-area non-uniformity. Combined with the more complex heterojunction design in HEMT devices, the devices are extremely sensitive to externally introduced radiation effects. In the working state, the performance and stability of the device are affected due to the uneven distribution of the lateral electric field of the device, especially the presence of a peak electric field on the side of the gate close to the drain.
[0003] Therefore, in order to demonstrate the characteristic advantages and technological maturity of GaN semiconductors in irradiation environments, it is necessary to further strengthen the design of GaN devices, study the static and dynamic degradation mechanisms of devices in irradiation environments, and develop systematic and comprehensive characterization methods for materials and devices after irradiation, so as to conduct in-depth research on device damage and failure mechanisms caused by irradiation. Summary of the invention
[0004] The purpose of the present invention is to provide a GaN HEMT device radiation damage detection technology and implementation method in view of the current lack of a systematic and comprehensive radiation damage characterization method. The characteristic luminescence wavelength and intensity of the substrate layer, gallium nitride layer, barrier layer and p-type gallium nitride layer through the transparent electrode in the vertical direction before and after the device is irradiated are collected by electroluminescence means, and the light intensity emitted from the source to the drain area at different potentials through the specified transparent electrode is analyzed and compared, so as to realize the analysis and determination of the defect type and location that affect the degradation of materials and devices after irradiation.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] A GaN HEMT device for radiation damage detection comprises a substrate layer, a gallium nitride layer, a barrier layer and a dielectric layer, wherein an annular p-type gallium nitride layer is provided on the top surface of the barrier layer, an annular transparent drain electrode and a transparent source electrode are provided on the top surfaces of the gallium nitride layer on both inner and outer sides of the p-type gallium nitride layer, respectively, an annular semi-transparent Schottky metal layer is provided on the top surface of the p-type gallium nitride layer, an annular transparent first ohmic metal layer is provided on the top surface of the barrier layer between the source electrode and the p-type gallium nitride layer, an annular transparent second ohmic metal layer is provided on the top surface of the barrier layer between the drain electrode and the p-type gallium nitride layer, and the second ohmic metal layer comprises a plurality of mutually interdigitated inner gear electrodes and outer gear electrodes, and there is a gap between the inner gear electrodes and the outer gear electrodes.
[0007] Preferably, the tooth roots of the multiple inner gear electrodes are connected to the outer ring to form a whole, and the outer ring is in contact with the p-type gallium nitride layer; the tooth roots of the multiple outer gear electrodes are connected to the inner ring to form a whole, and there is a gap between the inner ring and the drain; the tooth tops of the multiple inner gear electrodes point to the inner ring and are spaced therefrom, and the tooth tops of the multiple outer gear electrodes point to the outer ring and are spaced therefrom.
[0008] Preferably, the number of gears z of the internal gear electrode is an integer greater than and between is the distance from the p-type GaN layer to the drain, is the diameter of the drain electrode; the gear spacing of the inner gear electrode , tooth height L 2 is the tooth top arc length of the external gear electrode; the gear spacing of the external gear electrode , the tooth height is equal to the second ohmic metal layer, L 1 is the arc length of the tooth top of the inner gear electrode; the width of the outer ring 2~5 , the width of the inner ring 2~5 , the distance between the inner ring and the drain 1.5~2.5 and fill a dielectric layer with a thickness of 150nm~200nm; the gap between the tooth top of the inner gear electrode and the inner ring 1~2 , the distance between the tooth top of the outer gear electrode and the outer ring 1~2 , the distance between the inner gear electrode and the outer gear electrode 1~2 .
[0009] Preferably, The curvature of the tooth root connection arc of the internal gear electrode is 1 / 2~1 / 3 -1 and is tangent to the outer ring. The area of the inner gear electrode is , the arc length of the tooth gap of the internal gear electrode is ; The spacing between the tooth top of the outer gear electrode and the outer ring 1~2 , , the area of the outer gear electrode , the arc length of the tooth gap of the outer gear electrode is , The curvature of the tooth root connection arc of the external gear electrode is 1 / 2~1 / 3 -1 The connecting arcs on both sides of the tooth top arcs of the inner gear electrode and the outer gear electrode have a curvature of 1 to 1 / 2 -1 The semicircular arcs are tangent to the corresponding tooth top arcs respectively; the gear size and morphology of each inner gear electrode are consistent; the gear size and morphology of each outer gear electrode are consistent.
[0010] Preferably, the Schottky metal layer is a semi-transparent electrode with 4-7 nm thick Ni and 5-8 nm thick Cr evaporated; the source and drain are transparent electrodes with 85-100 nm thick ITO sputtered; the first ohmic metal layer and the second ohmic metal layer are transparent electrodes with 65-90 nm thick ITO sputtered; the inner side of the first ohmic metal layer is in contact with the p-type gallium nitride layer, and the outer side is spaced 1-2 and fill with a dielectric layer with a thickness of 150 to 200 nm; the ring width of the first ohmic metal layer 4~6 The inner ring curvature K of the first ohmic metal layer 1 satisfy , the outer ring curvature K 2 satisfy , is the distance from the p-type GaN layer to the drain.
[0011] Preferably, electroluminescence is used to collect data on the luminous wavelength, intensity and area of the GaN HEMT device before and after irradiation in the vertical and horizontal directions respectively, and a comparative analysis of the luminous area, wavelength and intensity of the two sets of data before and after irradiation is performed to confirm the type of defects generated in each area.
[0012] Preferably, the data collection method in the vertical direction before and after irradiation is as follows:
[0013] Under low gate voltage, spectral data emitted by the p-type gallium nitride layer and passing through the Schottky metal layer are collected; under higher gate voltage, spectral data emitted by the barrier layer and passing through the inner gear electrode, outer gear electrode and Schottky metal layer are collected; under high gate voltage, spectral data emitted by the gallium nitride layer and passing through the inner gear electrode, outer gear electrode and Schottky metal layer are collected.
[0014] Preferably, the data collection method in the horizontal direction before and after irradiation is as follows:
[0015] The first ohmic metal layer is connected to a positive potential, the drain is connected to a negative potential, and the spectral data of the barrier layer not covered by the p-type gallium nitride layer is collected; the outer gear electrode is connected to a positive potential, the source is connected to a negative potential, and the spectral data of the barrier layer not covered by the p-type gallium nitride layer is collected; the outer gear electrode is connected to a positive potential, the inner gear electrode is connected to a negative potential, and the spectral data of the barrier layer covering the second ohmic metal layer is collected.
[0016] On the basis of the above scheme (i.e., scheme 1) with other designs unchanged, it is further preferred (i.e., scheme 2) to adopt a design in which the gear coverage area increases in sequence, that is, the tooth top arc length of the internal gear electrode is L x , , ; The area of the inner gear electrode The curvature of the tooth root connection arc of the internal gear electrode is 1 / 2~1 / 3 -1 and is tangent to the outer ring. The arc length of the tooth gap of the inner gear electrode is , The tooth arc top length of the outer gear electrode ; The arc length of the tooth gap of the outer gear electrode is , . Other parts not mentioned are designed according to Scheme 1.
[0017] A method for manufacturing a GaN HEMT device for radiation damage detection comprises the following steps:
[0018] 1) The epitaxial wafer is grown from bottom to top in sequence, including a substrate layer, a gallium nitride layer, a barrier layer, and a p-type gallium nitride layer. The p-type gallium nitride layer in the non-patterned area is removed by inductively coupled plasma dry etching, so that only the ring-shaped p-type gallium nitride layer is retained in the gate area;
[0019] 2) Using plasma enhanced chemical vapor deposition method, a dielectric layer is grown on the entire epitaxial wafer; and the dielectric layer and barrier layer are etched in the areas corresponding to the source and drain by inductively coupled plasma dry etching and photolithography stripping method, and ITO is deposited by magnetron sputtering to form the source and drain; then the dielectric layer is etched between the source and the p-type gallium nitride layer, and between the p-type gallium nitride layer and the drain, and an ITO film is deposited by magnetron sputtering, and then the ITO film is exposed and developed by wet etching and photolithography stripping method to form the required annular first ohmic metal layer, inner gear electrode and outer gear electrode pattern, and then the unprotected ITO film is etched to form an electrode; finally, the dielectric layer is etched in the area corresponding to the p-type gallium nitride layer and a Schottky metal layer is deposited;
[0020] 3) Cover the entire epitaxial wafer area with a passivation layer, and open windows above the corresponding areas of the annular first ohmic metal layer, the inner gear electrode, the outer gear electrode and the Schottky metal layer so that the electroluminescent energy can be effectively collected to complete the preparation of the GaN HEMT device.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The innovation of the present invention is mainly reflected in the light-emitting window structure and analysis process as the electroluminescent collection area. The transparent electrode between the gate (i.e., the p-type gallium nitride layer) and the drain (i.e., the inner gear electrode and the outer gear electrode) serves as the main light outlet in the horizontal direction. By constructing the interdigitated gear electrode, on the one hand, the two gear electrodes are independent of each other and do not touch each other, but cover all areas from the gate to the drain, thereby improving the collection range; at the same time, although each gear is an independent individual, the distance they cover from the gate to the drain is the same, that is, each gear is a control group for each other, thereby improving the accuracy of spectral data collection. In scheme 2, on the basis of ensuring that the distance from the gate to the drain covered by the gear remains unchanged, the gear coverage area is increased in sequence. Each gear is a control group for each other and is also used as a means to explore the uniformity of degradation caused by irradiation in the device. The interdigitated electrodes are independent of each other and can achieve more accurate regional detection at different potentials. Through the constructed test analysis process, the defect types and locations caused by irradiation in different layers and regions can be detected.
[0023] The GaN HEMT device provided by the present invention can monitor the emission wavelength, intensity and regional changes of each layer of the GaN HEMT device before and after irradiation from different dimensions by collecting data in the vertical direction (through gate voltage regulation) and the horizontal direction (through different electrode configurations), so as to comprehensively and accurately identify the generation type and distribution of defects in each layer and region of the device. This multi-dimensional detection capability helps to deeply understand the radiation damage mechanism and improve the accuracy of device reliability assessment. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a schematic diagram of the planar structure of the GaN HEMT device of the present invention.
[0025] Figure 2 It is a schematic diagram of the cross-sectional structure of the GaN HEMT device of the present invention.
[0026] Figure 3a This is the schematic diagram of the acquisition and analysis in the vertical direction (bottom gate pressed down).
[0027] Figure 3b This is the schematic diagram of the acquisition and analysis in the vertical direction (under higher gate voltage).
[0028] Figure 3c Schematic diagram of the corresponding vertical direction acquisition and analysis (under high gate voltage).
[0029] Figure 4a This is the schematic diagram of the collection and analysis in the horizontal direction (the first ohmic metal layer is connected to the positive potential, and the drain is connected to the negative potential).
[0030] Figure 4b This is the schematic diagram of the collection and analysis in the horizontal direction (the outer gear electrode is connected to the positive potential, and the source is connected to the negative potential).
[0031] Figure 4c This is the schematic diagram of the horizontal data collection and analysis (the outer gear electrode is connected to the positive potential, and the inner gear electrode is connected to the negative potential).
[0032] Figure 5 It is a flow chart of the implementation of the method for detecting radiation damage of GaN HEMT device of the present invention.
[0033] Figure numerals: 1-substrate layer; 2-gallium nitride layer; 3-barrier layer; 4-p-type gallium nitride layer; 5-drain; 6-source; 7-Schottky metal layer; 8-first ohmic metal layer; 9-second ohmic metal layer; 901-inner gear electrode; 902-outer gear electrode; 903-outer ring; 904-inner ring. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments. However, it should be understood that the drawings are only used for exemplary description and cannot be understood as a limitation on this patent. In order to better illustrate this embodiment, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of the actual product. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted. The positional relationship described in the drawings is only for exemplary description and cannot be understood as a limitation on this patent.
[0035] like Figure 1 and Figure 2As shown, a GaN HEMT device for radiation damage detection includes a substrate layer 1, a gallium nitride layer 2, a barrier layer 3 and a dielectric layer. An annular p-type gallium nitride layer 4 is provided on the top surface of the barrier layer 3. An annular transparent drain 5 and a transparent source 6 are provided on the top surfaces of the gallium nitride layer 2 on both sides inside and outside the p-type gallium nitride layer 4, respectively. The annular electrode closer to the p-type gallium nitride layer 4 is the source 6, and the circular electrode farther away is the drain 5. The p-type gallium nitride layer 4 and the source 6 and drain 5 are filled with a dielectric layer. A circular semi-transparent Schottky metal layer 7 is disposed on the top surface of the p-type gallium nitride layer 4, a circular transparent first ohmic metal layer 8 is disposed on the top surface of the barrier layer 3 between the source 6 and the p-type gallium nitride layer 4, and a circular transparent second ohmic metal layer 9 is disposed on the top surface of the barrier layer 3 between the drain 5 and the p-type gallium nitride layer 4. The second ohmic metal layer 9 includes a plurality of inner gear electrodes 901 and outer gear electrodes 902 that are interdigitated with each other, and there is a gap between the inner gear electrodes 901 and the outer gear electrodes 902. Figure 1 and Figure 2 In the figure, G represents gate, S represents source, and D represents drain.
[0036] Specifically, the tooth roots of the multiple inner gear electrodes 901 are connected to the outer ring 903 to form a whole, and the outer ring 903 is in contact with the p-type gallium nitride layer 4; the tooth roots of the multiple outer gear electrodes 902 are connected to the inner ring 904 to form a whole, and there is a gap between the inner ring 904 and the drain 5; the tooth tops of the multiple inner gear electrodes 901 point to the inner ring 904 and have a gap therewith, and the tooth tops of the multiple outer gear electrodes 902 point to the outer ring 903 and have a gap therewith. The coverage area of the inner gear electrode 901 and the outer gear electrode 902 increases from the tooth root to the tooth top.
[0037] From the above structural design, it can be seen that the use of an annular p-type gallium nitride layer 4, a transparent drain 5 and a source 6, a semi-transparent Schottky metal layer 7, and a unique annular transparent first ohmic metal layer 8 and a second ohmic metal layer 9 (inner gear electrode 901 and outer gear electrode 902) design realizes effective control and accurate collection of the light-emitting area. The interdigital structure of the inner gear electrode 901 and the outer gear electrode 902 not only covers all areas from the gate to the drain, improving the collection range, but also ensures that the gate-to-drain distance covered by each gear is the same, forming a mutual comparison, and enhancing the accuracy of spectral data collection. In addition, the fine control of the gear electrode's parameters such as the tooth top arc length, tooth height, tooth spacing, and connection arc curvature is conducive to further optimizing the luminous efficiency and signal collection quality.
[0038] In some examples, the number of gears z of the inner gear electrode 901 is 20 and is an integer in and between is the distance from the p-type gallium nitride layer 4 to the drain 5, is the diameter of the drain electrode 5; the gear spacing of the inner gear electrode 901 , is 16.5 ; Tooth height ; Gear spacing of the outer gear electrode 902 , which is 22.5 ; The tooth height is equal to the second ohmic metal layer 9; The width of the outer ring 903 For 3 , the width of the inner ring 904 For 3 , the distance between the inner ring 904 and the drain 5 For 2 and fill with a 170nm thick dielectric layer; the gap between the tooth top of the inner gear electrode 901 and the inner ring 904 For 2 , the distance between the tooth top of the outer gear electrode 902 and the outer ring 903 For 2 , the distance between the inner gear electrode 901 and the outer gear electrode 902 For 2 .
[0039] In some examples, the arc length of the tooth top of the inner gear electrode 901 is L 1 =19 , The curvature of the tooth root connection arc of the internal gear electrode 901 is 0.5 -1 and is tangent to the outer ring 903. The area of the inner gear electrode 901 is , the arc length of the tooth gap of the inner gear electrode 901 is ; The distance between the tooth top of the outer gear electrode 902 and the outer ring 903 For 2 , the tooth top arc length of the external gear electrode 902 is L 2 =14 , the area of the outer gear electrode 902 , the arc length of the tooth gap of the outer gear electrode 902 is , The curvature of the tooth root connection arc of the outer gear electrode 902 is 0.5 -1 The connecting arcs on both sides of the top arcs of the inner gear electrode 901 and the outer gear electrode 902 are both 0.5 -1 The semicircular arcs are tangent to the corresponding tooth top arcs respectively; the gear size and shape of each inner gear electrode 901 are consistent; the gear size and shape of each outer gear electrode 902 are consistent.
[0040] In some examples, the Schottky metal layer 7 is a semi-transparent electrode with 6nm thick Ni and 8nm thick Cr evaporated, which serves as the main light outlet of the characteristic light in the vertical direction; the source 6 and the drain 5 are transparent electrodes with 90nm thick ITO sputtered; the first ohmic metal layer 8 and the second ohmic metal layer 9 are transparent electrodes with 70nm thick ITO sputtered, which serve as the light outlet of the characteristic light in the horizontal direction; in order to achieve a higher light extraction rate, the preferred ITO annealing temperature is 450℃, and the annealing time is about 60s. After deposition, the ITO is wet-etched in a 65℃ concentrated sulfuric acid solution for 6 minutes to improve the light extraction efficiency. The inner side of the first ohmic metal layer 8 is in contact with the p-type gallium nitride layer 4, and the outer side is spaced x 2 from the source 6. And fill with a 170nm thick dielectric layer; in order to ensure effective collection of the light emitting area and achieve certain device performance, the ring width of the first ohmic metal layer 8 For 5 The curvature K of the inner ring 904 of the first ohmic metal layer 8 1 =0.055, satisfying , outer ring 903 curvature K 2 =0.046, satisfying , is the distance from the p-type gallium nitride layer 4 to the drain 5 .
[0041] Based on the above GaN HEMT device structure design, the present invention uses electroluminescence to collect data on the wavelength, intensity and area of the GaN HEMT device before and after irradiation in the vertical and horizontal directions, and compares and analyzes the two sets of data before and after irradiation in terms of the area, wavelength and intensity of the light emission to confirm the type of defects generated in each area. The specific collection and analysis methods are as follows:
[0042] like Figure 3a-3c As shown, the data collection method in the vertical direction before and after irradiation is as follows:
[0043] At low gate voltage (3.5~5V) ( Figure 3a ), in the p-type gallium nitride layer 4, the channel electrons first relax to the deep donor energy level, and the holes relax to the deep acceptor energy level, and then recombine in the P-GaN to emit 1.8eV red light and be collected through the Schottky metal layer 7; under higher gate voltage (5.5~7V) ( Figure 3b), the holes in the barrier layer 3 first relax to the deep acceptor energy level, and then recombine with the channel electrons to emit 2.2eV yellow light, which is collected through the inner gear electrode 901 and the outer gear electrode 902. Part of the yellow light passes through the Schottky metal layer 7, and the luminous intensity of the inner gear electrode 901 and the outer gear electrode 902 is higher than that of the Schottky metal layer 7; the yellow light passing through the Schottky metal layer 7 corresponds to the barrier layer 3 covered by the p-type gallium nitride layer 4, and the light passing through the inner gear electrode 901 and the outer gear electrode 902 corresponds to the barrier layer 3 covering the inner gear electrode 901 and the outer gear electrode 902; under high gate voltage (7.5~9V) ( Figure 3c ), the holes and electrons in the gallium nitride layer 2 undergo band edge recombination to emit 3.4eV ultraviolet light which is collected by the inner gear electrode 901 and the outer gear electrode 902, and part of the light passes through the Schottky metal layer 7. The luminous intensity of the inner gear electrode 901 and the outer gear electrode 902 is higher than that of the Schottky metal layer 7. Figure 3a-3c In the figure, S represents the source and D represents the drain.
[0044] From the above design, we can know that three levels of low gate voltage, relatively high gate voltage and high gate voltage are designed to meet the needs of luminescence detection under different conditions (such as the recombination of channel electrons and holes at different energy levels). This design can capture luminescence information at different energy levels (such as red light, yellow light, and ultraviolet light), which helps to fully reveal the impact of different radiation doses and energies on device performance and improve the sensitivity and resolution of radiation damage identification.
[0045] like Figure 4a-4c As shown, the data collection method in the horizontal direction before and after irradiation is as follows:
[0046] like Figure 4a As shown, the first ohmic metal layer 8 is connected to a positive potential, the drain electrode 5 is connected to a negative potential, and the interface between the gallium nitride layer 2 and the barrier layer 3 emits blue light due to electron-hole recombination and is collected by the electroluminescent device through the transparent first ohmic metal layer 8, the inner gear electrode 901, and the outer gear electrode 902. The collection area is the barrier layer 3 that is not covered by the p-type gallium nitride layer 4; Figure 4b As shown, the outer gear electrode 902 is connected to a positive potential, the source electrode 6 is connected to a negative potential, and light is collected by the electroluminescent device through the first ohmic metal layer 8, the inner gear electrode 901, and the outer gear electrode 902, and the collection area is the barrier layer 3 that is not covered by the p-type gallium nitride layer 4; Figure 4c As shown, the outer gear electrode 902 is connected to a positive potential, and the inner gear electrode 901 is connected to a negative potential. Light passes through the inner gear electrode 901 and the outer gear electrode 902 and is collected by the electroluminescent device. The collection area is the barrier layer 3 covering the transparent inner gear electrode 901 and the outer gear electrode 902. Figure 4a-4c In the figure, S represents the source and D represents the drain.
[0047] It can be seen from the above design that in the process of horizontal data collection, by changing the distribution of positive and negative potentials between different electrodes (such as the first ohmic metal layer 8, the source electrode 6, the drain electrode 5, the inner gear electrode 901, and the outer gear electrode 902), the luminous signals from different device regions (such as the barrier layer 3 covering the transparent first ohmic metal layer 8, the inner gear electrode 901, and the outer gear electrode 902) can be specifically excited and collected. This design greatly enriches the detection means, facilitates the analysis of the impact of radiation on different structural units, and helps to identify local defects and non-uniform degradation phenomena.
[0048] The devices before and after irradiation were tested. Figure 5 The analysis and testing process shown is as follows: electroluminescence (EL) is used to collect and analyze the wavelength, intensity, and area of the device's light in the vertical and horizontal directions to confirm the type of defects generated in each area.
[0049] The present invention proposes a set of standardized processes including the collection and analysis of electroluminescence (EL) emission wavelength, intensity, and area in the vertical and horizontal directions, which can systematically and normatively evaluate the changes in device performance before and after irradiation, help to quickly and accurately identify defect types and locations, and provide a reliable basis for the prevention and repair of radiation damage and the optimization of device performance.
[0050] Based on the above structural design, the present invention provides a method for manufacturing a GaN HEMT device for radiation damage detection, comprising the following steps:
[0051] 1) The epitaxial wafer is grown from bottom to top in sequence, including a substrate layer 1, a gallium nitride layer 2, a barrier layer 3 and a p-type gallium nitride layer 4. The p-type gallium nitride layer 4 in the non-patterned area is removed by an inductively coupled plasma dry etching method, so that only the ring-shaped p-type gallium nitride layer 4 is retained in the gate area;
[0052] 2) Using plasma enhanced chemical vapor deposition method, a dielectric layer is grown on the entire epitaxial wafer; and the dielectric layer and barrier layer 3 are etched in the region corresponding to the source 6 and the drain 5 by inductively coupled plasma dry etching method and photolithography stripping method, and ITO is deposited by magnetron sputtering method to form the source 6 and the drain 5; then the dielectric layer is etched between the source and the p-type gallium nitride layer 4, and between the p-type gallium nitride layer 4 and the drain 5, and an ITO film is deposited by magnetron sputtering method, and then the ITO film is exposed and developed by wet etching and photolithography stripping method to form the required annular first ohmic metal layer 8, inner gear electrode 901 and outer gear electrode 902 patterns, and then the unprotected ITO film is etched to form electrodes; finally, the dielectric layer is etched in the region corresponding to the p-type gallium nitride layer 4 and a Schottky metal layer is deposited;
[0053] 3) The entire epitaxial wafer area is covered with a passivation layer, and windows are opened above the corresponding areas of the annular first ohmic metal layer 8, the inner gear electrode 901, the outer gear electrode 902 and the Schottky metal layer so that the electroluminescent energy can be effectively collected, thereby completing the preparation of the GaN HEMT device.
[0054] The present invention uses multiple process technologies such as epitaxial growth, dry etching, plasma enhanced chemical vapor deposition, magnetron sputtering, wet etching, photolithography stripping, etc. to achieve efficient integrated preparation of GaN HEMT devices. In particular, by constructing a light-emitting window structure and optimizing the electrode pattern, the effective collection of electroluminescence and the maintenance of device performance are taken into account, reflecting good process compatibility and practicality.
[0055] In summary, the GaN HEMT device and its manufacturing method significantly improve the accuracy, range and flexibility of radiation damage detection through refined electrode design, multi-level and multi-angle radiation damage detection, gate voltage level design, flexible electrode polarity configuration and standardized test and analysis process, which is helpful for in-depth research on the impact of radiation on the performance of GaN HEMT devices and provides strong technical support for improving the radiation resistance and reliability of the device.
[0056] According to the description and drawings of the present invention, those skilled in the art can easily manufacture or use a GaN HEMT device for radiation damage detection and a detection and manufacturing method thereof of the present invention, and can produce the positive effects described in the present invention.
[0057] Unless otherwise specified, in the present invention, the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicating orientation or positional relationships are based on the orientation or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the orientation or positional relationship in the present invention are only used for illustrative purposes and cannot be understood as limitations on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood in conjunction with the drawings and according to specific circumstances.
[0058] Unless otherwise clearly specified and limited, in the present invention, the terms "disposed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0059] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A GaN HEMT device for radiation damage detection, comprising a substrate layer (1), a gallium nitride layer (2), a barrier layer (3) and a dielectric layer, wherein a ring-shaped p-type gallium nitride layer (4) is provided on the top surface of the barrier layer (3), characterized in that: The top surfaces of the gallium nitride layer (2) on both sides of the inside and outside of the p-type gallium nitride layer are respectively provided with an annular transparent drain electrode (5) and a transparent source electrode (6); the top surface of the p-type gallium nitride layer (4) is provided with an annular semi-transparent Schottky metal layer (7); the top surface of the barrier layer (3) between the source electrode (6) and the p-type gallium nitride layer is provided with an annular transparent first ohmic metal layer (8); the top surface of the barrier layer (3) between the drain electrode (5) and the p-type gallium nitride layer (4) is provided with an annular transparent second ohmic metal layer (9); the second ohmic metal layer (9) comprises a plurality of mutually interdigitated inner gear electrodes (901) and outer gear electrodes (902); and there is a gap between the inner gear electrodes (901) and the outer gear electrodes (902); the transparent first ohmic metal layer (8) and the transparent second ohmic metal layer (9) are both transparent electrodes of ITO.
2. The GaN HEMT device for radiation damage detection according to claim 1, characterized in that: The tooth roots of the plurality of inner gear electrodes (901) are all connected to the outer ring (903) to form a whole, and the outer ring (903) is in contact with the p-type gallium nitride layer (4); the tooth roots of the plurality of outer gear electrodes (902) are all connected to the inner ring (904) to form a whole, and there is a gap between the inner ring (904) and the drain (5); the tooth tops of the plurality of inner gear electrodes (901) are all pointing to the inner ring (904) and there is a gap therebetween, and the tooth tops of the plurality of outer gear electrodes (902) are all pointing to the outer ring (903) and there is a gap therebetween.
3. The GaN HEMT device for radiation damage detection according to claim 2, characterized in that: The number z of the gears of the internal gear electrode (901) is an integer greater than and between is the distance from the p-type gallium nitride layer (4) to the drain (5), is the diameter of the drain electrode (5); the gear spacing of the inner gear electrode (901) , tooth height L2 is the tooth top arc length of the external gear electrode (902); the gear spacing of the external gear electrode (902) , the tooth height is equal to that of the second ohmic metal layer (9), L1 is the tooth top arc length of the inner gear electrode (901); the width of the outer ring (903) is 2~5 , the width of the inner ring (904) 2~5 , the distance between the inner ring (904) and the drain (5) 1.5~2.5 and fill a dielectric layer with a thickness of 150nm to 200nm; the gap between the tooth top of the inner gear electrode (901) and the inner ring (904) 1~2 , the distance between the tooth top of the outer gear electrode (902) and the outer ring (903) 1~2 , the distance between the inner gear electrode (901) and the outer gear electrode (902) 1~2 .
4. The GaN HEMT device for radiation damage detection according to claim 3, characterized in that: The curvature of the tooth root connection arc of the internal gear electrode (901) is 1 / 2 to 1 / 3 -1 and is tangent to the outer ring (903), the area of the inner gear electrode (901) is , the tooth gap arc length of the internal gear electrode (901) is ; The distance between the tooth top of the outer gear electrode (902) and the outer ring (903) 1~2 , , the area of the outer gear electrode (902) , the tooth gap arc length of the outer gear electrode (902) is , The curvature of the tooth root connection arc of the external gear electrode (902) is 1 / 2 to 1 / 3 -1 and is tangent to the inner ring (904); the connecting arcs on both sides of the tooth top arcs of the inner gear electrode (901) and the outer gear electrode (902) have a curvature of 1 to 1 / 2 -1 The semicircular arcs are tangent to the corresponding tooth top arcs respectively; the gear size and shape of each of the inner gear electrodes (901) are consistent; and the gear size and shape of each of the outer gear electrodes (902) are consistent.
5. The GaN HEMT device for radiation damage detection according to claim 3, characterized in that: The tooth top arc length of the internal gear electrode (901) is L x , , ; The area of the inner gear electrode (901) The curvature of the tooth root connection arc of the internal gear electrode (901) is 1 / 2~1 / 3 -1 and is tangent to the outer ring (903). The tooth gap arc length of the inner gear electrode (901) is , The tooth arc top length of the outer gear electrode (902) ; The tooth gap arc length of the outer gear electrode (902) is , .
6. The GaN HEMT device for radiation damage detection according to claim 1, characterized in that: The Schottky metal layer (7) is a semi-transparent electrode with 4-7 nm thick Ni and 5-8 nm thick Cr deposited thereon; the source electrode (6) and the drain electrode (5) are both transparent electrodes with 85-100 nm thick ITO sputtered thereon; the first ohmic metal layer (8) and the second ohmic metal layer (9) are both transparent electrodes with 65-90 nm thick ITO sputtered thereon; the inner side of the first ohmic metal layer (8) is in contact with the p-type gallium nitride layer (4), and the outer side is spaced 1-2 nm from the source electrode (6). And fill with a dielectric layer 150~200nm thick; The ring width of the first ohmic metal layer (8) 4~6 The curvature K1 of the inner ring (904) of the first ohmic metal layer (8) satisfies , the curvature K2 of the outer ring (903) satisfies , is the distance from the p-type gallium nitride layer (4) to the drain (5).
7. A method for detecting radiation damage of a GaN HEMT device, characterized in that: Electroluminescence is used to collect data on the luminescent wavelength, intensity and area of the GaN HEMT device according to any one of claims 1 to 6 in the vertical direction and the horizontal direction before and after irradiation, and the two sets of data before and after irradiation are compared and analyzed in terms of luminescent area, wavelength and intensity to confirm the type of defects generated in each area.
8. The method for detecting radiation damage of a GaN HEMT device according to claim 7, characterized in that: The data collection method in the vertical direction before and after irradiation is as follows: Under low gate voltage, spectrum data emitted by the p-type gallium nitride layer (4) and passing through the Schottky metal layer (7) are collected; under higher gate voltage, spectrum data emitted by the barrier layer (3) and passing through the inner gear electrode (901), the outer gear electrode (902) and the Schottky metal layer (7) are collected; under high gate voltage, spectrum data emitted by the gallium nitride layer (2) and passing through the inner gear electrode (901), the outer gear electrode (902) and the Schottky metal layer (7) are collected.
9. The method for detecting radiation damage of a GaN HEMT device according to claim 7, characterized in that: The data collection method in the horizontal direction before and after irradiation is as follows: The first ohmic metal layer (8) is connected to a positive potential, the drain electrode (5) is connected to a negative potential, and spectrum data of the barrier layer (3) not covered by the p-type gallium nitride layer (4) is collected; the outer gear electrode (902) is connected to a positive potential, the source electrode (6) is connected to a negative potential, and spectrum data of the barrier layer (3) not covered by the p-type gallium nitride layer (4) is collected; the outer gear electrode (902) is connected to a positive potential, the inner gear electrode (901) is connected to a negative potential, and spectrum data of the barrier layer (3) covering the second ohmic metal layer (9) is collected.
10. A method for manufacturing a GaN HEMT device for radiation damage detection according to any one of claims 1 to 6, characterized in that: The steps include: 1) The epitaxial wafer is sequentially grown from bottom to top to include a substrate layer (1), a gallium nitride layer (2), a barrier layer (3) and a p-type gallium nitride layer (4), and the p-type gallium nitride layer (4) in a non-patterned area is removed by an inductively coupled plasma dry etching method, so that only the annular p-type gallium nitride layer (4) is retained in the gate area; 2) using plasma enhanced chemical vapor deposition to grow a dielectric layer on the entire epitaxial wafer; and etching the dielectric layer and the barrier layer in the regions corresponding to the source (6) and the drain (5) by inductively coupled plasma dry etching and photolithography stripping, and depositing ITO by magnetron sputtering to form the source (6) and the drain (5); then etching the dielectric layer between the source and the p-type gallium nitride layer, and between the p-type gallium nitride layer and the drain (5), and depositing an ITO film by magnetron sputtering, and then exposing and developing the ITO film by wet etching and photolithography stripping to form the required annular first ohmic metal layer (8), inner gear electrode (901) and outer gear electrode (902) patterns, and then etching the unprotected ITO film to form electrodes; and finally etching the dielectric layer in the region corresponding to the p-type gallium nitride layer and depositing a Schottky metal layer (7); 3) The entire epitaxial wafer area is covered with a passivation layer, and windows are opened above the corresponding areas of the annular first ohmic metal layer (8), the inner gear electrode (901), the outer gear electrode (902) and the Schottky metal layer (7), so that the electroluminescent energy can be effectively collected, thereby completing the preparation of the GaN HEMT device.
Citation Information
Patent Citations
In-wafer reliability screening method for GaN HEMT (High Electron Mobility Transistor) device
CN102721913A
Test structure for characterization of potential track of GaN-based HEMT device and characterization method
CN111722075A
Thin-film transistor and manufacturing method therefor
CN112236868A
Channel defect detection method and wafer detection method
CN115775745A
Method and apparatus for the molecular identification of defects in semiconductor manufacturing using a radiation scattering technique such as raman spectroscopy
US6067154A