A filter bag with welding material and preparation method thereof
The two sides of the filter material are overlapped and welded at high temperature through the welding agent material, which solves the problem of the dust filter bag being easy to open and dust escaping in high temperature environment, realizing a seamless and high-strength filter bag, improving the filtration accuracy and service life .
Patent Information
- Application Number
- CN202410772213.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing dust removal filter bags are easy to open in high temperature and corrosive environments, causing dust to escape. Moreover, the processing of thermosetting fiber filter materials requires a large amount of sewing thread, making it difficult to meet discharge standards and improve filtration accuracy.
Welding material is used to overlap both sides of the filter material to form a cylindrical shape, and the welding material is melted and penetrated into the fibers through high-temperature welding to form a seamless, pinhole-free filter bag.
A seamless, high-strength filter bag is achieved, which extends the service life, reduces costs, reduces carbon emissions, improves filtration accuracy, and avoids problems with needle holes and sewing threads.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filter bags, in particular to a filter bag with a welding agent material and a preparation method thereof. Background Art
[0002] The body of the dust filter bag is made by sewing the cut filter material into a long cylindrical bag body through a three-needle sewing device. Some thermoplastic fibers or filter materials mixed with a large amount of thermoplastic fibers (thermoplastic fibers are mainly polypropylene, polyester, and PPS fibers) can be made by direct hot melting when processing the bag body, while many thermosetting fiber filter materials that do not have a melting point can only be processed by three-needle sewing. The problem is that a large amount of sewing thread is used, and needle holes and gaps are generated. During the use of dust removal equipment, repeated filtration and the stitching parts are subjected to long-term scouring, high temperature, corrosion, etc., and there is a risk of open thread, loss of strength, and dust escape, and smoke emissions are difficult to meet standards. Therefore, we propose a filter bag with a welding agent material and a preparation method thereof. Summary of the invention
[0003] The object of the present invention is to provide a filter bag with a welding flux material and a preparation method thereof to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a filter bag with welding material, comprising a bag body and welding material; the bag body is formed into a cylindrical shape by overlapping and bonding two sides of the filter material; the welding material is located at the overlapping and bonding part of the filter material.
[0005] Furthermore, the overlapping width of the filter material is 5 to 30 mm.
[0006] If the overlap width is less than 5mm, the overlapped parts of the filter material are small, the effective area of the welding material is reduced, and the welding strength will be reduced accordingly. When the overlap width is 5-10mm, the welding strength can basically reach 800N or more; when the overlap width is 10-30mm, the effective area of the welding material is large, and the welding strength can reach 2000N or more. If the overlap width is greater than 30mm, the welding strength is better; but because there are too many overlapped parts of the filter material, it will cause waste of welding material and filter material.
[0007] Furthermore, the filter material is a non-woven fabric, including one or more fibers of acrylic (PAC), aramid (PMIA), polyimide (PI, P84), and polytetrafluoroethylene (PTFE).
[0008] Furthermore, the filter material is a mixed material containing a thermosetting material, and the proportion of the thermosetting material is greater than or equal to (≥) 50wt%.
[0009] The filter material contains 50% to 100% of thermosetting fibers without melting point, and the proportion of thermosetting materials is greater than or equal to 50%. If the amount of thermosetting materials in the filter material is less than 50%, the filter material can be directly welded by hot melting.
[0010] Furthermore, the solder material is a thermoplastic resin material, and the weight average molecular weight of the thermoplastic resin material is 1w to 8w.
[0011] The weight average molecular weight of the solder material is 1w to 8w. If the weight average molecular weight of the solder material is less than 1W, the thermal adhesion and permeability of the solder material are very poor and cannot meet the requirements; if it is greater than 8W, although the adhesion and permeability are sufficient, the material is not easy to solidify and rapid production cannot be achieved.
[0012] Furthermore, the molecular formula of the solder material contains a single benzene ring or a cyclic unit of multiple benzene rings.
[0013] The molecular formula of the welding material contains a single benzene ring or a cyclic unit of multiple benzene rings. Without the benzene ring, the heat resistance and bonding strength of the welding material are not stable enough. However, too many benzene rings will cause the thermal stability of the welding material to be higher, and it is not suitable for use as a high-temperature welding material.
[0014] Furthermore, the melting temperature of the solder material is 180-350°C.
[0015] The melting temperature of the solder material depends on the time the solder material stays at high temperature. If the solder material stays below 180℃ for a long time, the solder material will not change; above 180℃, the solder material will be semi-molten; at 350℃, the solder material will be completely melted; if it exceeds 350℃, the solder material will be completely melted, resulting in temperature waste, and the welding may undergo qualitative changes.
[0016] Furthermore, the weight of the solder material is 50 to 300 g / m 2 .
[0017] If the weight of the welding material is less than 50g / m 2 , the molten product is less and the welding strength is poor; if the weight of the welding flux material is higher than 300g / m2, the molten product is less and the welding strength is better, which will cause excess demand.
[0018] A method for preparing a filter bag with a welding material, comprising the following processes:
[0019] Take the filter material and attach the welding material to the overlapping and bonding position; overlap the two sides of the filter material to form a cylinder, and weld at high temperature to obtain a filter bag.
[0020] Furthermore, the temperature of high temperature welding is 200-800° C., and the welding speed is 1-9 m / min.
[0021] In the above technical solution, the filter material containing thermosetting fibers is overlapped and bonded on both sides to prepare a cylindrical seamless, pinhole-free filter bag. The cut filter material is attached to the overlapped and bonded parts by an automated device, and the filter material enters the high-temperature spray gun overlap position through a semicircular cloth guide device, so that the welding material melts at high temperature and penetrates into the fibers of the filter material; the overlapped and bonded parts are bonded to each other by the action of a pressing wheel to form a three-dimensional structure, and after leaving the high temperature, they are cooled and hardened to achieve high strength, thus completing the seamless welding reinforcement of the filter bag to form a seamless cylindrical bag body.
[0022] The filter bags produced have the advantages of no gaps, high strength and long life. They save the use of sewing thread, avoid the formation of pinholes, and solve the problem that thermosetting filter materials can only be sewn with conventional seams, thereby reducing costs, reducing carbon emissions, and improving filtration accuracy. They help to improve the filtration effect and extend the service life of the filter bags. They also solve the problem that the dust filter bags are repeatedly filtered during use in dust removal equipment, and the seams are subjected to long-term erosion, high temperature, corrosion, etc., resulting in the risk of open threads, loss of strength, and dust escape, thereby reducing costs and increasing efficiency.
[0023] Furthermore, the welding material is prepared by the following process:
[0024] Mix phenyl diacid, epichlorohydrin and catalyst, heat to 110-115°C, keep warm and react for 18-25 minutes; distill under reduced pressure to remove unreacted epichlorohydrin; add benzene to dissolve, keep the reaction system at 20-30°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 20-30°C, and stir for 4-6 hours; filter, wash with water until neutral, dry the organic layer, and evaporate benzene under reduced pressure to obtain diglycidyl ester;
[0025] Mix diisocyanate, diglycidyl ester, accelerator and solvent, heat to 153-158°C under nitrogen atmosphere, and react for 10-11 hours; add distilled water to precipitate, filter, wash with water, and dry; soak in methanol for 24 hours, filter, and dry at 50°C to obtain polyoxazolidone as a welding agent material.
[0026] Furthermore, the diisocyanate is one of toluene diisocyanate, 4,4'-diphenylmethane diisocyanate and 1,6-hexamethylene diisocyanate.
[0027] Furthermore, the phenyl-containing diacid is one of terephthalic acid, isophthalic acid, phthalic acid, 2,2'-biphenyl dicarboxylic acid, 5-methylisophthalic acid, 4-methoxyphthalic acid, and 2,5-di(1H-imidazole-1-yl)terephthalic acid.
[0028] Further, the molar ratio of the phenyl diacid to epichlorohydrin is 1:(12-16);
[0029] The catalyst is hexadecyltrimethylammonium bromide, and the amount used is 0.1% of the molar amount of phenyl diacid;
[0030] The amount of sodium hydroxide used is 0.82% to 0.85% of the mass of phenyldiacid.
[0031] Furthermore, the molar ratio of the diisocyanate to diglycidyl ester is (1.02-1.10):1;
[0032] The accelerator is 2-ethyl-4-methylimidazole, and the dosage is 5% to 10% of the total mass of diisocyanate and diglycidyl ester;
[0033] The solvent is N,N-dimethylformamide, and the ratio of diisocyanate to N,N-dimethylformamide is 50 g / 100 mL.
[0034] In the above technical scheme, diglycidyl ester is esterified by the carboxyl group in the benzoic acid and the epoxy group in the epichlorohydrin under the action of a catalyst, and the hydrogen chloride is removed under the action of an alkali to form glycidyl ester by cyclization, thereby obtaining diglycidyl ester containing phenyl. Diglycidyl ester is copolymerized with diisocyanate to obtain a linear polymer polyoxazolidone with a molecular weight between 1.0 and 8.0 W. By controlling the amount of diglycidyl ester and diisocyanate, it is manifested as a thermoplastic resin, and the molecular structure contains a rigid group benzene ring, a five-membered ring of oxazolidone and a six-membered ring of isocyanurate, which can increase the glass transition temperature of the prepared polymer, improve the interface performance between the welding agent material and the filter material, have a higher melting temperature, have good flame retardancy, heat resistance, bonding strength and mechanical properties, show good room temperature, high temperature welding strength and heat aging resistance, and can be suitable for high temperature bonding occasions and high temperature environments.
[0035] Furthermore, the phenyl diacid can be replaced by 4'4-dimercaptodiphenyl sulfide or diphenyl sulfide disulfide acid.
[0036] Thiodiphenyl diacid is prepared by the following process:
[0037] Under nitrogen protection, 4'4-dimercaptodiphenyl sulfide, alkenyl acid and solvent are mixed, an initiator is added, and the mixture is reacted at 30-100° C. for 1-10 hours; rotary evaporation and chromatography are performed to obtain diphenyl sulfide dithio acid.
[0038] Furthermore, the molar ratio of 4'4-dimercaptodiphenyl sulfide to alkenyl acid is 1:(2.01-2.10).
[0039] Further, the initiator is a mixture of one or more of azobisisobutyronitrile, azobisisoheptylnitrile, cumene hydroperoxide, tert-butyl hydroperoxide, and dicumyl peroxide;
[0040] The amount of the initiator used is 0.3% to 0.8% of the total mass of 4'4-dimercaptodiphenyl sulfide and alkenyl acid.
[0041] Further, the solvent is N,N-dimethylformamide;
[0042] The ratio of 4'4-dimercaptodiphenyl sulfide to the solvent is (10-20) g / 100 mL.
[0043] Furthermore, the alkenyl acid is one of 2-octenoic acid, 2-nonenoic acid, 3-nonenoic acid, 3-decenoic acid, 4-decenoic acid, and 4-vinylbenzoic acid.
[0044] In the above technical solution, diphenyl sulfide dithio acid is obtained by reacting 4'4-dithiodiphenyl sulfide and alkenyl acid, and the carboxyl group is grafted through the addition between the thiol group and the alkenyl group to form a diacid containing a diphenyl sulfide group, which helps to improve the polarity of the polyoxazolidone, improve the heat resistance of the welding material, and the bonding strength between it and the filter material; it can also undergo oxidative cross-linking at high temperatures in the welding process, thereby improving the toughness and thermal stability of the welding material. The alkenyl acid contains a soft alkyl segment, which can inhibit the crystallization of the polyoxazolidone, improve its flexibility, improve its processing performance, alleviate the brittleness of the welding material, and help improve the fracture resistance of the welding part of the filter bag.
[0045] Furthermore, the 4'4-dimercaptodiphenyl sulfide can be replaced by the following dimercapto compounds, and the specific preparation process is as follows:
[0046] In a nitrogen atmosphere, at a temperature of 0 to 3°C, 1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane, 3-mercapto-1-propanol, DBU and anhydrous pyridine are mixed, heated to 20 to 35°C, and reacted for 8 to 12 hours; filtered, washed and dried to obtain a dithiol compound.
[0047] Further, the molar ratio of 1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane (CAS No: 2329-10-4), 3-mercapto-1-propanol, and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) is 1:(2.1-2.2):(1.2-2.0);
[0048] The ratio of 1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane (CAS No: 2329-10-4) and anhydrous pyridine is 10 g / 100 mL.
[0049] In the above technical scheme, the dithiol compound is prepared by mixing dichlorocyclodisilazane (1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane) and 3-mercapto-1-propanol, and reacting chlorosilane with hydroxyl groups to replace 4'4-dimercaptodiphenyl sulfide. The cyclodisilazane structure is introduced into the molecular structure of polyoxazolidone, making it have higher thermal stability, further improving its welding strength and heat aging resistance.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] The filter bag with welding material described in the present invention is made by attaching welding material to the overlapping and pasting part of the filter material, and welding at high temperature, so that the welding material melts at high temperature and penetrates into the fiber of the filter material; bonding and cooling are performed by the action of a pressure wheel, so as to realize seamless welding reinforcement of the high-strength filter bag. The filter bag has the advantages of no gaps, high strength, and long life, does not require sewing thread, avoids the generation of pinholes, improves the filtering accuracy, helps to improve the filtering effect, prolongs the service life of the filter bag, and achieves cost reduction and efficiency improvement. DETAILED DESCRIPTION
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] In the following specific implementations,
[0054] The filter material is aramid nonwoven fabric;
[0055] PA: 2175, from Tianyang New Materials (Shanghai) Technology Co., Ltd.
[0056] Embodiment 1: A method for preparing a filter bag with a welding material, comprising the following process:
[0057] S1. Preparation of welding materials:
[0058] Mix terephthalic acid, epichlorohydrin and catalyst hexadecyltrimethylammonium bromide (0.1% of the molar amount of terephthalic acid), heat to 110°C, keep warm and reflux for 18 minutes; remove unreacted epichlorohydrin by distillation under reduced pressure; add benzene to dissolve, keep the reaction system at 20°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 20°C, and stir for 4 hours; filter, wash with water until neutral, dry the organic layer, and distill benzene under reduced pressure to obtain diglycidyl ester; the molar ratio of terephthalic acid to epichlorohydrin is 1:12; the amount of sodium hydroxide used is 0.82% of the mass of terephthalic acid;
[0059] 25g of toluene diisocyanate, diglycidyl ester, 5% accelerator 2-ethyl-4-methylimidazole and 50mL solvent N,N-dimethylformamide were mixed, heated to 153°C under nitrogen atmosphere, and reacted for 10 hours; distilled water was added to precipitate, filtered, washed with water, and dried; methanol was soaked for 24 hours, filtered, and dried at 50°C to obtain polyoxazolidone as a welding material; the molar ratio of toluene diisocyanate and diglycidyl ester (molecular weight 250) was 1.02:1;
[0060] S2. Preparation of filter bags:
[0061] Take the filter material and attach the welding material to the overlapping part. The overlapping width is 5mm and the weight of the welding material is 60g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0062] Example 2-5: A method for preparing a filter bag with a welding material, comprising the following process:
[0063] S1. The preparation of the welding material is the same as that in Example 1, to obtain the welding material;
[0064] S2. The preparation process of the filter bag is different to obtain the filter bag.
[0065] Embodiment 6: A method for preparing a filter bag having a welding material, comprising the following process:
[0066] S1. Preparation of welding materials:
[0067] Mix 4'4-dimercaptodiphenyl sulfide, epichlorohydrin and catalyst hexadecyltrimethylammonium bromide (0.1% of the molar amount of 4'4-dimercaptodiphenyl sulfide), heat to 112°C, keep warm and reflux for 20 minutes; remove unreacted epichlorohydrin by distillation under reduced pressure; add benzene to dissolve, keep the reaction system at 25°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 25°C, and stir for 5 hours; filter, wash with water until neutral, dry the organic layer, and distill benzene under reduced pressure to obtain diglycidyl ester; the molar ratio of 4'4-dimercaptodiphenyl sulfide to epichlorohydrin is 1:14; the amount of sodium hydroxide used is 0.83% of the mass of terephthalic acid;
[0068] 25g of toluene diisocyanate, diglycidyl ester, 8% accelerator 2-ethyl-4-methylimidazole and 50mL solvent N,N-dimethylformamide were mixed, heated to 155°C under nitrogen atmosphere, and reacted for 10.5h; distilled water was added to precipitate, filtered, washed with water, and dried; methanol was soaked for 24h, filtered, and dried at 50°C to obtain polyoxazolidone as a welding material; the molar ratio of toluene diisocyanate and diglycidyl ester (molecular weight 334.4) was 1.06:1;
[0069] S2. Preparation of filter bags:
[0070] Take the filter material and attach the welding material to the overlapping part. The overlapping width is 30mm and the weight of the welding material is 200g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0071] Embodiment 7: A method for preparing a filter bag having a welding material, comprising the following process:
[0072] S1. Preparation of welding materials:
[0073] Under nitrogen protection, 15g of 4'4-dimercaptodiphenyl sulfide, 2-nonenoic acid and 100mL of solvent N,N-dimethylformamide were mixed, 0.6% of initiator azobisisobutyronitrile was added, and the mixture was reacted at 75°C for 6h; rotary evaporation and chromatography were performed to obtain diphenyl sulfide disulfide acid; the molar ratio of 4'4-dimercaptodiphenyl sulfide to 2-nonenoic acid was 1:2.1;
[0074] Mix thiobisphenyl diacid, epichlorohydrin and catalyst hexadecyltrimethylammonium bromide (0.1% of the molar amount of thiobisphenyl diacid), heat to 115°C, keep warm and reflux for 25 minutes; remove unreacted epichlorohydrin by distillation under reduced pressure; add benzene to dissolve, keep the reaction system at 30°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 30°C, and stir for 6 hours; filter, wash with water until neutral, dry the organic layer, and distill benzene under reduced pressure to obtain diglycidyl ester; the molar ratio of thiobisphenyl diacid (molecular weight 563) to epichlorohydrin is 1:16; the amount of sodium hydroxide used is 0.85% of the mass of terephthalic acid;
[0075] 25g of toluene diisocyanate, diglycidyl ester, 10% accelerator 2-ethyl-4-methylimidazole and 50mL solvent N,N-dimethylformamide were mixed, heated to 158°C under nitrogen atmosphere, and reacted for 11h; distilled water was added to precipitate, filtered, washed with water, and dried; methanol was soaked for 24h, filtered, and dried at 50°C to obtain polyoxazolidone as a welding material; the molar ratio of toluene diisocyanate and diglycidyl ester (molecular weight 647) was 1.10:1;
[0076] S2. Preparation of filter bags:
[0077] Take the filter material and attach the welding material to the overlapping part. The overlapping width is 30mm and the weight of the welding material is 200g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0078] Embodiment 8: A method for preparing a filter bag having a welding material, comprising the following process:
[0079] S1. Preparation of welding materials:
[0080] In a nitrogen atmosphere, at 0°C, 10 g of 1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane (CAS No: 2329-10-4), 3-mercapto-1-propanol, DBU and 100 mL of anhydrous pyridine were mixed, heated to 25°C, and reacted for 10 h; filtered, washed, and dried to obtain a dithiol compound; the molar ratio of 1,3-bis(chlorodimethylsilyl)-2,2,4,4-tetramethyl-1,3-diaza-2,4-disilacyclobutane, 3-mercapto-1-propanol, and 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU) was 1:2.1:1.6;
[0081] Mix dithiol compound, epichlorohydrin and catalyst hexadecyltrimethylammonium bromide (0.1% of the molar amount of dithiol compound), heat to 120°C, keep warm and react for 25 minutes; distill under reduced pressure to remove unreacted epichlorohydrin; add benzene to dissolve, keep the reaction system at 30°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 30°C, and stir for 6 hours; filter, wash with water until neutral, dry the organic layer, and distill benzene under reduced pressure to obtain diglycidyl ester; the molar ratio of dithiol compound (molecular weight 442.5) to epichlorohydrin is 1:16; the amount of sodium hydroxide used is 0.85% of the mass of terephthalic acid;
[0082] 25g of toluene diisocyanate, diglycidyl ester, 10% accelerator 2-ethyl-4-methylimidazole and 50mL solvent N,N-dimethylformamide were mixed, heated to 158°C under nitrogen atmosphere, and reacted for 11h; distilled water was added to precipitate, filtered, washed with water, and dried; methanol was soaked for 24h, filtered, and dried at 50°C to obtain polyoxazolidone as a welding material; the molar ratio of toluene diisocyanate and diglycidyl ester (molecular weight 526.5) was 1.1:1;
[0083] S2. Preparation of filter bags:
[0084] Take the filter material and attach the welding material to the overlapping part. The overlapping width is 30mm and the weight of the welding material is 200g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0085] Comparative Example 1: A method for preparing a filter bag with a welding material, comprising the following processes:
[0086] Take the filter material and attach the welding material (PA) to the overlapping part. The overlapping width is 5mm and the weight of the welding material is 60g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0087] Comparative Example 2: A method for preparing a filter bag having a welding material, comprising the following processes:
[0088] S1. Preparation of welding materials:
[0089] 25g of 1,6-hexamethylene diisocyanate, diglycidyl ether, 5% accelerator 2-ethyl-4-methylimidazole and 50mL solvent N,N-dimethylformamide were mixed, heated to 153°C under nitrogen atmosphere, and reacted for 10 hours; distilled water was added to precipitate, filtered, washed with water, and dried; methanol was soaked for 24 hours, filtered, and dried at 50°C to obtain polyoxazolidone as a welding material; the molar ratio of 1,6-hexamethylene diisocyanate to diglycidyl ether was 1.02:1;
[0090] S2. Preparation of filter bags:
[0091] Take the filter material and attach the welding material to the overlapping part. The overlapping width is 5mm and the weight of the welding material is 60g / m 2 ; Overlap the two sides of the filter material to form a cylinder, and weld them at high temperature to obtain a filter bag.
[0092] Experiment: Take the filter bags obtained in Examples 1-8 and Comparative Examples 1-2, prepare samples, test their performances respectively and record the test results:
[0093] Welding strength test: A tensile tester is used to test the filter bag sample, with breaking as the welding strength index. The tensile rate is 10mm / min, and the sample is a 20cm×5cm filter bag containing welding material;
[0094] Heat resistance test: Two groups of filter bag samples were placed in a 240℃ oven for 1 week and a 280℃ oven for 12 hours respectively. Then they were taken out and subjected to welding strength test again.
[0095] Table 1:
[0096]
[0097] Table 2:
[0098]
[0099] According to the data in the above table, we can clearly draw the following conclusions:
[0100] The filter bags obtained in Examples 1-8 were compared with the filter bags obtained in Comparative Examples 1-2. The test results show that:
[0101] Compared with Example 1, the preparation process of the filter bags in Examples 2-5 is different; the preparation process of the welding material in Examples 6-8 is different, and the obtained filter bags have higher welding strength at both room temperature and high temperature, and gradually increase with the increase of overlapping width and gram weight of welding material.
[0102] Compared with Example 1, the selection of the welding material in Comparative Example 1-2 is different, and the welding strength of the obtained filter bag at room temperature and high temperature is reduced. This fully demonstrates that the setting of the welding material preparation process of the present invention can promote the improvement of the room temperature and high temperature welding strength of the prepared filter bag.
[0103] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0104] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a filter bag having a flux material, Features: Including the following processes: Take the filter material and attach the welding material to the overlapping and pasting position; overlap the two sides of the filter material to form a cylinder, and weld at high temperature to obtain a filter bag; The welding material is prepared by the following process: Mix diphenyl sulfide disulfide acid or dithiol compound, epichlorohydrin and catalyst, heat to 110-115°C, keep warm and react for 18-25 minutes; remove unreacted epichlorohydrin by distillation under reduced pressure; add benzene to dissolve, keep the reaction system at 20-30°C, add 50% sodium hydroxide aqueous solution dropwise within 60 minutes, keep the system at 20-30°C, stir for 4-6 hours, and obtain diglycidyl ester; The diisocyanate, diglycidyl ester, accelerator and solvent are mixed, heated to 153-158° C. under the protection of nitrogen atmosphere, and reacted for 10-11 hours to obtain a solder material; The diphenyl sulfide disulfide acid is prepared by the following process: Under nitrogen protection, 4'4-dimercaptodiphenyl sulfide, alkenyl acid and solvent are mixed, an initiator is added, and the mixture is reacted at 30-100° C. for 1-10 hours; rotary evaporation and chromatography are performed to obtain diphenyl sulfide disulfide acid; The dithiol compound is prepared by the following process: In a nitrogen atmosphere, at a temperature of 0 to 3° C., dichlorocyclodisilazane, 3-mercapto-1-propanol, DBU and anhydrous pyridine are mixed, heated to 20 to 35° C., and reacted for 8 to 12 hours; filtered, washed, and dried to obtain a dithiol compound.
2. A method for preparing a filter bag with a welding material according to claim 1, Features: The overlapping width of the filter material is 5 to 30 mm.
3. A method for preparing a filter bag with a welding material according to claim 1, Features: The filter material contains 50-100wt% of thermosetting material.
4. A method for preparing a filter bag with a welding material according to claim 1, Features: The welding material is a thermoplastic resin material, the weight average molecular weight of the thermoplastic resin material is 1w-8w; the melting temperature of the welding material is 180-350°C; the gram weight of the welding material is 50-300g / m 2 .
5. A method for preparing a filter bag with a welding material according to claim 1, Features: The diisocyanate is one of toluene diisocyanate, 4,4'-diphenylmethane diisocyanate and 1,6-hexamethylene diisocyanate.
6. A method for preparing a filter bag with a welding material according to claim 1, Features: The alkenyl acid is one of 2-octenoic acid, 2-nonenoic acid, 3-nonenoic acid, 3-decenoic acid, 4-decenoic acid, and 4-vinylbenzoic acid.
Citation Information
Patent Citations
Optical epoxy resin and synthesis method thereof
CN102391471A
Preparation method of polyphenylene sulfide composite filter material filter bag
CN105107268A
Synthesis technology of diglycidyl p-phthalate
CN108484531A
Stable epoxy-isocyanate mixtures and oxazolidinone-containing polymers obtained therefrom