Polymer nanospray needle manufacturing method based on stress induction and polymer nanospray needle

Through the stress-induced manufacturing method of polymer nano-jet needles, the bending and stretching method is used to generate nano-cracks, combined with the hot bonding method, which solves the problems of high cost and low efficiency of nano-jet needle manufacturing in the existing technology, and achieves low-cost, high-efficiency Manufacture of polymer nanojet needles.

CN118342833BActive Publication Date: 2024-10-18SUZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410777829.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-18
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

It is difficult to manufacture nano-jet needles at low cost and efficiently with existing technology, especially due to the reliance on expensive equipment and high-cost processing processes, which results in high cost and low efficiency of manufacturing nano-jet needles.

Method used

Using a manufacturing method based on stress-induced polymer nano-jet needles, nano-cracks are generated on the polymer micron jet needles through bending and stretching methods to form nano-channels, and the nano-channels are sealed by thermal bonding methods to realize polymer nano-jet needles. of manufacturing.

Benefits of technology

The manufacturing of nano-injection needles with simple process, high efficiency and low cost was realized. Micron structures were prepared through photolithography technology and nano-cracks were generated using bending and stretching methods. The nano-channels were sealed using the thermal bonding method to obtain a complete polymer nano-injection needle. Needle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118342833B_ABST
    Figure CN118342833B_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a polymer nanospray needle based on stress induction and a polymer nanospray needle. The manufacturing method includes: using PDMS as a flexible substrate and photoresist as a target material; preparing a micron spray needle pattern by photolithography and manufacturing a stress concentration point; using a bending and stretching method to cause nanocracks to occur at the stress concentration point of the micron spray needle, generating a nanochannel, thereby obtaining a polymer nanospray needle bottom plate; bonding the polymer spray needle cover plate to the polymer nanospray needle bottom plate under oxygen plasma treatment by a thermal bonding method, and sealing the nanochannel, using photolithography to perform ultraviolet exposure on the polymer spray needle cover plate, obtaining a spray needle liquid reservoir, and obtaining a complete polymer nanospray needle. The invention discloses a method for manufacturing a polymer nanospray needle based on stress induction and a polymer nanospray needle. Using a bending and stretching method to cause nanocracks to occur at the stress concentration point of the microspray needle, generating a nanochannel, thereby obtaining a polymer nanospray needle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of micro-electromechanical technology, and in particular to a manufacturing method of a polymer nano-spray needle based on stress induction and a polymer nano-spray needle. Background Art

[0002] Electrohydraulic jet printing is an additive manufacturing technology that can directly deposit the desired material onto the target substrate without a mask. This technology uses electric field force to drive the ink to flow through the needle and generate a jet, and its jet diameter is much smaller than the inner diameter of the needle. Therefore, electrohydraulic jet printing has a scale effect, and how to further reduce the inner diameter of the needle and improve the printing resolution is a key issue that needs to be solved urgently.

[0003] At present, nanochannel preparation technologies mostly use electron beam exposure, ion beam direct writing, laser direct writing and other methods, which have extremely high manufacturing precision. However, the above methods all rely on expensive processing equipment and dust-free environment, are costly and have the characteristics of serial and time-consuming processing.

[0004] In summary, how to manufacture nanospray needles at low cost and high efficiency remains a difficult problem. Summary of the invention

[0005] The present invention overcomes the shortcomings of the prior art and provides a stress-induced polymer nanospray needle manufacturing method and a polymer nanospray needle that are simple in process, high in efficiency, low in cost, and easy to implement. The bending and stretching method is used to cause nanocracks to occur at the stress concentration point of the micron spray needle to generate nanochannels, thereby obtaining a polymer nanospray needle.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for manufacturing a polymer nanospray needle based on stress induction, comprising the following steps:

[0007] Step 1, prepare a polymer nanospray needle bottom plate and a polymer spray needle cover plate, and proceed to step 2;

[0008] The preparation method of the polymer nanospray needle bottom plate comprises the following steps:

[0009] Step a1, obtaining a flexible substrate and placing it on a supporting substrate, and then spin coating a layer of photoresist on the outer surface of the flexible substrate to serve as a needle bottom plate substrate;

[0010] Step a2, placing the needle bottom plate substrate on which the photoresist is spin-coated in step a1 on a hot plate for step baking, and then cooling to room temperature;

[0011] Step a3, placing the needle base plate substrate spun with photoresist processed in step a2 on a photolithography machine, placing the needle mask plate on the photoresist on the needle base plate substrate for ultraviolet lithography, performing post-baking and development after lithography, and obtaining a needle micron structure on the photoresist of the needle base plate substrate;

[0012] Step a4, removing the supporting substrate of the nozzle bottom plate substrate after the treatment in step a3, bending the two ends of the flexible substrate together, with a curvature radius of 1-3 mm, and causing nanocracks on the photoresist, wherein the nanocracks are between the end of the nozzle micron channel and the nozzle port, and the photoresist between the nanocracks occurs, so as to obtain a polymer nano nozzle bottom plate;

[0013] The preparation method of the polymer spray needle cover plate comprises the following steps:

[0014] Step b1, obtaining a flexible substrate, and subjecting the flexible substrate to oxygen plasma treatment;

[0015] Step b2, spin coating photoresist on the flexible substrate treated in step b1, and performing step baking to manufacture a polymer spray needle cover plate;

[0016] Step 2, respectively subjecting the polymer nanospray needle bottom plate and the polymer spray needle cover plate to oxygen plasma treatment, and proceeding to step 3;

[0017] Step 3, hot-pressing the polymer nano-spray needle and the polymer spray needle cover plate after the treatment in step 2 to obtain a polymer nano-spray needle bonded body, and then proceeding to step 4;

[0018] Step 4, ultraviolet exposure is performed on one side of the polymer needle cover plate of the polymer nano-needle bonded body through the cover plate mask, and then the polymer nano-needle bonded body is post-baked and developed in sequence to obtain a needle reservoir on the side of the needle cover plate of the polymer nano-needle bonded body, and then step 5 is entered;

[0019] Step 5, drying the polymer nanospray needle bonded body after the treatment in step 4, and placing it on a hot plate for hardening; and proceeding to step 6;

[0020] Step 6, removing waste and trimming the polymer nanospray needle bonded body treated in step 5 to obtain a complete polymer nanospray needle.

[0021] In a preferred embodiment of the present invention, in step a1, the photoresist is spin-coated at a low speed of 600-900 rpm, a spin-coating time of 6-9 s, and a high speed of 3000-5000 rpm, a spin-coating time of 20-30 s;

[0022] In step a2, the step baking is performed by placing the product on a horizontal hot plate at 65-85°C;

[0023] In step a3, the exposure time of UV lithography is 4-9 minutes, and the post-baking is performed by heating on a horizontal hot plate at 65-85° C. for 2-5 minutes and then cooling to room temperature; the development is performed by respectively placing the sample in developer, ethanol, and deionized water for 45-90 seconds.

[0024] In a preferred embodiment of the present invention, in step b1, the oxygen plasma treatment has a treatment power of 10 to 20 W and a treatment time of 10 to 20 s;

[0025] In step b2, the photoresist is spin-coated at a low speed of 600-900 rpm, a spin-coating time of 6-9 s, a high speed of 3000-5000 rpm, and a spin-coating time of 20-30 s; and the step baking is performed on a horizontal hot plate at 65-85°C.

[0026] In a preferred embodiment of the present invention, in step 2, the treatment power of the oxygen plasma treatment is 20-30 W, and the treatment time is 20-30 s;

[0027] and / or, in step 3, the bonding temperature is 40-50° C., the bonding pressure is 0.1-0.3 MPa, and the bonding time is 5-10 min;

[0028] And / or, in step 4, the exposure time is 4 to 9 minutes, followed by post-baking on a horizontal hot plate at 65 to 85° C. for 2 to 5 minutes, cooling to room temperature, and developing in SU-8 developer, ethanol, and deionized water for 45 to 90 seconds respectively;

[0029] And / or, in step 5, the drying treatment is carried out by drying with a nitrogen air gun, and the film is hardened by placing the film on a horizontal hot plate at 65-85° C. for 20-30 minutes;

[0030] And / or, in step 6, the waste removal and finishing uses a coated tool to remove excess flexible substrate.

[0031] In a preferred embodiment of the present invention, the flexible substrate is a PDMS flexible substrate, and the preparation process of the PDMS flexible substrate comprises the following steps:

[0032] Step c1, wrapping a circle of aluminum foil tape around the bottom plate base, wherein the aluminum foil tape is arranged on the bottom plate base to form a fence to form a casting container;

[0033] Step c2, injecting the PDMS mixed solution onto the bottom plate substrate in the enclosure of the casting container prepared in step c1;

[0034] Step c3, placing the casting container with the PDMS mixed solution in step c2 in a vacuum oven and evacuating the vacuum oven for 5 to 10 minutes to remove bubbles;

[0035] Step c4, placing the PMMA substrate with the PDMS mixed solution treated in step c3 in a 60-85° C. oven for curing for 2-4 hours to obtain a PDMS flexible substrate.

[0036] In a preferred embodiment of the present invention, in step c1, the enclosure shape is a cube or a cuboid; in step c2, the PDMS mixed solution is a mixture of PDMS and a curing agent in a ratio of 4:1 to 10:1, and the mixed PDMS mixed solution is placed in a vacuum oven and evacuated for 5 to 10 minutes to remove bubbles.

[0037] In a preferred embodiment of the present invention, the photoresist used is SU-8 photoresist;

[0038] The bottom plate substrate adopts a PMMA substrate, a glass substrate, a silicon wafer substrate, a PET substrate, or a PVP substrate.

[0039] In a preferred embodiment of the present invention, the PDMS flexible substrate used in the flexible substrate is replaced with a PET film, a PI film, a PMMA film, a hydrogel film, or a rubber layer;

[0040] The aluminum foil tape is replaced by sealing film, BOPP tape, PET double-sided tape, glass fiber tape, Teflon tape, copper foil tape, plasma spray tape, polyimide tape, glass cloth tape, or masking tape.

[0041] In a preferred embodiment of the present invention, the step baking parameters of the photoresist are as follows: the temperature is increased from 65°C to 85°C, and the temperature is increased by 5°C every 15 minutes. When the temperature reaches 85°C, the photoresist is baked for 30 minutes and then cooled to room temperature on the hot plate;

[0042] And / or, in step 3, the bonding temperature is 40-50° C., the bonding pressure is 0.1-0.3 MPa, and the bonding time is 5-10 min.

[0043] In a preferred embodiment of the present invention, a stress-induced polymer nanospray needle can be prepared by using the stress-induced polymer nanospray needle manufacturing method.

[0044] The present invention solves the defects existing in the technical background, and the beneficial technical effects of the present invention are:

[0045] The invention discloses a method for manufacturing a polymer nanospray needle based on stress induction, which is simple in process, high in efficiency, low in cost and easy to realize, and a polymer nanospray needle. The method adopts a flexible substrate and a photoresist as a target material. A micron spray needle pattern is prepared by photolithography technology, and a stress concentration point is obtained at the same time. A bending and stretching method is used to cause nano cracks to occur at the stress concentration point of the micron spray needle, and a nano channel is generated, so as to obtain a polymer nanospray needle bottom plate. A polymer spray needle cover plate is bonded to a polymer nanospray needle bottom plate under oxygen plasma treatment by a thermal bonding method, and the nano channel is sealed to obtain a complete polymer nanospray needle. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0047] Figure 1 1 is a process flow chart for manufacturing a flexible substrate in a preferred embodiment of the present invention.

[0048] Figure 2 It is a process flow chart for preparing a polymer nanospray needle base plate in preparing a polymer nanospray needle in a preferred embodiment of the present invention.

[0049] Figure 3 It is a process flow chart for preparing a polymer spray needle cover plate in a polymer nano spray needle in a preferred embodiment of the present invention.

[0050] Figure 4 It is a process flow chart of preparing a polymer nano-spray needle by combining a polymer spray needle cover plate and a polymer nano-spray needle bottom plate in a preferred embodiment of the present invention.

[0051] Figure 5 It is a schematic diagram of the structure of the polymer nanospray needle in a preferred embodiment of the present invention.

[0052] Figure 6 This is a microscope image of a polymer nanospray needle tool based on stress induction in a preferred embodiment of the present invention.

[0053] Figure 7 It is a schematic diagram of the local structure of the stress-induced polymer nanospray needle in a preferred embodiment of the present invention.

[0054] In the figure: 1. base plate; 2. aluminum foil tape; 3. flexible base; 4. photoresist, 41. nanocrack; 5. needle mask; 6. ultraviolet light; 7. cover mask, 8. vacuum oven, A-first stress concentration point, B-second stress concentration point, C-micrometer channel. DETAILED DESCRIPTION

[0055] The present invention will now be further described in detail with reference to the accompanying drawings and embodiments. These drawings are simplified schematic diagrams that only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.

[0056] It should be noted that if there are directional indications (such as up, down, bottom, top, etc.) involved in the embodiments of the present invention, the directional indication is only used to explain the relative position relationship, movement, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly. The terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. Unless otherwise clearly specified and defined, the terms "set", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal connection of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. Embodiment 1

[0057] like Figure 1-Figure 7 As shown, a method for manufacturing a polymer nanospray needle based on stress induction comprises the following steps:

[0058] Step 1, prepare a polymer nanospray needle bottom plate and a polymer spray needle cover plate, and proceed to step 2;

[0059] The preparation method of the polymer nanospray needle bottom plate comprises the following steps:

[0060] Step a1, obtain a piece of flexible substrate 3 and place it on a supporting substrate (on Figure 2 A layer of photoresist 4 is then spin-coated on the flexible substrate 3 as a nozzle bottom plate substrate (eg, Figure 2 2a); further, in this embodiment, the supporting substrate is a clean glass substrate, which is ultrasonically cleaned in acetone, ethanol, and deionized water for 30 minutes, blown dry with a nitrogen air gun, and placed in a 100-150°C oven to remove moisture. The photoresist 4 is SU-8 photoresist. A layer of photoresist 4 is spin-coated on the flexible substrate 3 using a coating machine, and the spin-coating speed of the photoresist 4 is a low speed of 600-900 rpm, a spin-coating time of 6-9s, a high speed of 3000-5000 rpm, and a spin-coating time of 20-30s.

[0061] Step a2, placing the needle bottom plate substrate spun with photoresist obtained in step a1 on a hot plate for step baking, and then cooling to room temperature; step baking is to place it on a horizontal hot plate at 65~85°C for step baking. Furthermore, the step baking parameters of photoresist 4 are: the temperature is increased from 65°C to 85°C, and the temperature is increased by 5°C every 15 minutes. When the temperature reaches 85°C, photoresist 4 is baked for 30 minutes, and then cooled to room temperature with the hot plate. If step baking is not performed, uncontrollable cracks will appear in the SU-8 photoresist during the development process. At the same time, it must be cooled to room temperature with the hot plate, otherwise uncontrollable cracks will also occur.

[0062] Step a3, placing the needle base substrate with the photoresist spun on it after the step a2 on the photolithography machine, placing the needle mask 5 on the photoresist 4 on the needle base substrate for ultraviolet light 6 lithography (such as Figure 2 2b), after photolithography, post-baking and development are performed, and finally, the needle micron pattern (as shown in FIG. Figure 2 As shown in 2c). Furthermore, the exposure time of UV 6 lithography is 4~9min, and the post-baking is performed by placing it on a horizontal hot plate at 65~85℃ for 2~5min, and then cooling it to room temperature; the development is performed by placing it in developer, ethanol, and deionized water for 45~90s. Among them, the specific steps of development include: first placing it in the developer to develop and obtain the pattern, then placing it in ethanol to remove the SU-8 developer, and finally placing it in deionized water to wash away the ethanol. In this way, the sample is clean. In short, the SU-8 development process is SU-8 developer-ethanol-deionized water, three steps.

[0063] Step a4, removing the support substrate of the spray needle bottom plate substrate after the treatment in step a3, and bending the two ends of the flexible substrate 3 (such as Figure 2 As shown in 2d, the radius of curvature is 1-3 mm, and nanocracks occur on the photoresist 4. The nanocracks are nanocracks in the photoresist 4 between the end of the nozzle micron channel and the nozzle port, that is, the polymer nano nozzle bottom plate (such as Figure 2 Furthermore, if the radius of curvature is too large (>3 mm), the bending force is insufficient to generate nanocracks.

[0064] The preparation method of the polymer spray needle cover plate comprises the following steps:

[0065] Step b1, obtain a piece of flexible substrate 3, and perform oxygen plasma treatment on the flexible substrate 3; the treatment power of the oxygen plasma treatment is 10~20W, and the treatment time is 10~20s. If the power is too small or the time is too short, the surface hydrophilic effect cannot be achieved, so that in the subsequent spin coating process of SU-8 photoresist, SU-8 photoresist is easily separated from the flexible substrate 3; if the power is too large or the time is too long, the surface of the flexible substrate 3 is over-etched, the contact angle is too large, and the surface hydrophobic effect is caused instead. The optimal surface hydrophilic effect of the flexible substrate 3 can be obtained within the parameter range.

[0066] Step b2, spin coating the photoresist 4 on the flexible substrate 3 treated in step b1, the spin coating speed of the photoresist 4 is 600-900 rpm at a low speed, the spin coating time is 6-9 s, and the high speed is 3000-5000 rpm, the spin coating time is 20-30 s; then step baking is performed, the step baking is performed on a horizontal hot plate at 65-85°C; the polymer spray needle cover plate (such as Figure 3 3f). Further, in this embodiment, the photoresist 4 is SU-8 photoresist. The step baking parameters of the photoresist 4 are that the temperature is increased from 65°C to 85°C, and the temperature is increased by 5°C every 15 minutes. When the temperature reaches 85°C, the photoresist 4 is baked for 30 minutes and then cooled to room temperature along with the hot plate.

[0067] Step 2, respectively subjecting the polymer nanospray needle bottom plate and the polymer spray needle cover plate to oxygen plasma treatment, wherein the treatment power of the oxygen plasma treatment is 20-30 W and the treatment time is 20-30 s; proceeding to step 3;

[0068] Step 3, hot-pressing and bonding the polymer nano-spray needle and the polymer spray needle cover plate to obtain a polymer nano-spray needle bonded body (such as Figure 4 As shown in Figure 4g), the bonding temperature is 40~50℃, the bonding pressure is 0.1~0.3MPa, and the bonding time is 5~10min; proceed to step 4.

[0069] Step 4, ultraviolet exposure is performed on one side of the polymer needle cover plate of the polymer nano-needle bonded body through the cover plate mask 7 (eg Figure 4 4h in the figure), the exposure time is 4~9min, then the polymer nanospray needle bonded body is placed on a horizontal hot plate at 65~85℃ and baked for 2~5min, cooled to room temperature, and then placed in developer, ethanol, and deionized water for development for 45~90s respectively; a spray needle reservoir (as shown in Figure 4 Go to step 5.

[0070] Further, the needle reservoir is the present invention Figure 5The middle circle is the nozzle reservoir. The polymer nano nozzle has an inlet and an outlet. The inlet is where the ink enters, which is the nozzle reservoir, and the outlet is the nozzle port. Figure 4 As shown in 4g, a layer of photoresist 4 is spin-coated on the PDMS substrate, and then removed and Figure 4 The bonding is shown in 4h, and after bonding, the PDMS is removed to prevent the upper mask from being exposed to ultraviolet light.

[0071] Step 5, drying the polymer nanospray needle bonded body after the treatment in step 4 and hardening the film; the drying process is carried out by blowing with a nitrogen air gun, and the hardening process is carried out by heating on a horizontal hot plate at 65-85° C. for 20-30 minutes; then proceed to step 6.

[0072] Step 6, the polymer nanospray needle bonded body treated in step 5 is subjected to waste removal and trimming, wherein the waste removal and trimming adopts a coated tool to remove the excess flexible substrate 3; a complete polymer nanospray needle (such as Figure 4 (as shown in Figure 4j).

[0073] In this embodiment, the flexible substrate 3 is a PDMS (polydimethylsiloxane) flexible substrate. However, it is not limited thereto. In other embodiments, the PDMS flexible substrate can be replaced by a PET film, a PI film, a PMMA (polymethylmethacrylate) film, a hydrogel film, or a rubber layer.

[0074] The preparation process of PDMS flexible substrate includes the following steps:

[0075] Step c1, wrap a circle of aluminum foil tape 2 around the bottom plate base 1, and the aluminum foil tape 2 is arranged on the bottom plate base 1 to form a fence to form a casting container (such as Figure 1 1a). Further, the enclosure shape of the enclosure is a cube or a cuboid. In this embodiment, the bottom plate substrate 1 adopts a PMMA substrate, but it is not limited to this. In other embodiments, the PMMA substrate can be replaced by a glass substrate, a silicon wafer substrate, a PET substrate, or a PVP substrate. But it is not limited to this. The aluminum foil tape 2 can also be replaced by a sealing film, a BOPP tape, a PET double-sided tape, a glass fiber tape, a Teflon tape, a copper foil tape, a plasma spray tape, a polyimide tape, a glass cloth tape, or a masking tape.

[0076] Step c2, the PDMS mixed solution is a mixture of PDMS and curing agent in a ratio of 4:1 to 10:1, and the mixed PDMS mixed solution is placed in a vacuum oven 8 for 5 to 10 minutes to remove excess bubbles, and then the PDMS mixed solution is injected onto the bottom plate substrate 1 in the enclosure of the casting container prepared in step c1 (such as Figure 1 1b). If the vacuuming time in step c2 is too short, many air bubbles will appear inside the PDMS after solidification, which greatly reduces the fracture toughness of the PDMS substrate and makes it easy to tear during the bending process.

[0077] Step c3, placing the casting container with the PDMS mixed solution in step c2 into a vacuum oven 8 and evacuating the vacuum oven for 5 to 10 minutes to remove excess bubbles (such as Figure 1 1c); if the vacuuming time in step c3 is too short, many air bubbles will appear inside the PDMS after solidification, which greatly reduces the fracture toughness of the PDMS substrate and is prone to tearing during the bending process.

[0078] Step c4, placing the PMMA substrate with the PDMS mixed solution treated in step c3 in a 60-85°C oven for curing for 2-4 hours, and after cooling to room temperature, removing the aluminum foil tape 2 (such as Figure 1 As shown in 1d, and use the coated tool to cut off the uneven parts around it (such as Figure 1 1e), a PDMS flexible substrate was obtained (as shown in Figure 1 1f). Embodiment 2

[0079] The polymer nanospray needle is prepared by the stress-induced polymer nanospray needle manufacturing method of Example 1, such as Figure 5 shown.

[0080] Working principle:

[0081] The present invention provides a method for manufacturing a polymer nanospray needle based on stress induction, which is simple in process, high in efficiency, low in cost and easy to implement. Figure 1-Figure 7 As shown, PDMS is used as the flexible substrate 3, and the photoresist 4 uses SU-8 photoresist as the target material. The micron needle pattern is prepared by photolithography technology, and the stress concentration point is manufactured at the same time. Figure 7 After photolithography, the micron channel C is obtained and the entire outline of the needle is obtained, wherein the first stress concentration point A and the second stress concentration point B are as shown in FIG. Figure 7 As shown. The bending and stretching method is used to cause nanocracks to occur at the stress concentration point of the micron spray needle to generate nanochannels, thereby obtaining a polymer SU-8 nanospray needle. Finally, the polymer spray needle cover plate is bonded to the nanospray needle bottom plate under optimized oxygen plasma treatment parameters by a thermal bonding method to seal the nanochannels and obtain a complete polymer nanospray needle. The polymer nanospray needle prepared by the stress-induced polymer nanospray needle manufacturing method of the present invention is a polymer SU-8 nanospray needle. The preparation process of the polymer nanospray needle of the present invention is simple, efficient, low-cost, and easy to implement.

[0082] The above specific implementation methods are specific support for the scheme ideas proposed in the present invention, and cannot be used to limit the protection scope of the present invention. Any equivalent changes or equivalent modifications made on the basis of this technical scheme in accordance with the technical ideas proposed in the present invention still fall within the scope of protection of the technical scheme of the present invention.

Claims

1. A method for manufacturing a polymer nanospray needle based on stress induction, characterized in that: The following steps are involved: Step 1, prepare a polymer nanospray needle bottom plate and a polymer spray needle cover plate, and proceed to step 2; The preparation method of the polymer nanospray needle bottom plate comprises the following steps: Step a1, obtaining a flexible substrate and placing it on a supporting substrate, and then spin coating a layer of photoresist on the outer surface of the flexible substrate to serve as a needle bottom plate substrate; Step a2, placing the needle bottom plate substrate on which the photoresist is spin-coated in step a1 on a hot plate for step baking, and then cooling to room temperature; Step a3, placing the needle base plate substrate spun with photoresist processed in step a2 on a photolithography machine, placing the needle mask plate on the photoresist on the needle base plate substrate for ultraviolet lithography, performing post-baking and development after lithography, and obtaining a needle micron structure on the photoresist of the needle base plate substrate; Step a4, removing the supporting substrate of the nozzle bottom plate substrate after the treatment in step a3, bending the two ends of the flexible substrate together, with a curvature radius of 1-3 mm, and causing nanocracks on the photoresist, wherein the nanocracks are between the end of the nozzle micron channel and the nozzle port, and the photoresist between the nanocracks occurs, so as to obtain a polymer nano nozzle bottom plate; The preparation method of the polymer spray needle cover plate comprises the following steps: Step b1, obtaining a flexible substrate, and subjecting the flexible substrate to oxygen plasma treatment; Step b2, spin coating photoresist on the flexible substrate treated in step b1, and performing step baking to manufacture a polymer spray needle cover plate; Step 2, respectively subjecting the polymer nanospray needle bottom plate and the polymer spray needle cover plate to oxygen plasma treatment, and proceeding to step 3; Step 3, hot-pressing the polymer nano-spray needle and the polymer spray needle cover plate after the treatment in step 2 to obtain a polymer nano-spray needle bonded body, and then proceeding to step 4; Step 4, ultraviolet exposure is performed on one side of the polymer needle cover plate of the polymer nano-needle bonded body through the cover plate mask, and then the polymer nano-needle bonded body is post-baked and developed in sequence to obtain a needle reservoir on the side of the needle cover plate of the polymer nano-needle bonded body, and then step 5 is entered; Step 5, drying the polymer nanospray needle bonded body after the treatment in step 4, and placing it on a hot plate for hardening; and proceeding to step 6; Step 6, performing waste removal and trimming on the polymer nanospray needle bonded body treated in step 5 to obtain a complete polymer nanospray needle; In step a1, the photoresist is spin-coated at a low speed of 600-900 rpm for a spin-coating time of 6-9 s, and at a high speed of 3000-5000 rpm for a spin-coating time of 20-30 s; In step a2, the step baking is performed by placing the product on a horizontal hot plate at 65-85°C; In step a3, the exposure time of UV lithography is 4-9 minutes, and the post-baking is performed by heating on a horizontal hot plate at 65-85° C. for 2-5 minutes and then cooling to room temperature; the development is performed by respectively placing the sample in developer, ethanol, and deionized water for 45-90 seconds.

2. The method for manufacturing a polymer nanospray needle based on stress induction according to claim 1, characterized in that: In step b1, the treatment power of the oxygen plasma treatment is 10-20 W, and the treatment time is 10-20 s; In step b2, the photoresist is spin-coated at a low speed of 600-900 rpm, a spin-coating time of 6-9 s, a high speed of 3000-5000 rpm, and a spin-coating time of 20-30 s; and the step baking is performed on a horizontal hot plate at 65-85°C.

3. The method for manufacturing a polymer nanospray needle based on stress induction according to claim 2, characterized in that: In step 2, the treatment power of the oxygen plasma treatment is 20-30 W, and the treatment time is 20-30 s; and / or, in step 3, the bonding temperature is 40-50° C., the bonding pressure is 0.1-0.3 MPa, and the bonding time is 5-10 min; And / or, in step 4, the exposure time is 4 to 9 minutes, followed by post-baking on a horizontal hot plate at 65 to 85° C. for 2 to 5 minutes, cooling to room temperature, and developing in SU-8 developer, ethanol, and deionized water for 45 to 90 seconds respectively; And / or, in step 5, the drying treatment is carried out by drying with a nitrogen air gun, and the film is hardened by placing the film on a horizontal hot plate at 65-85° C. for 20-30 minutes; And / or, in step 6, the waste removal and finishing uses a coated tool to remove excess flexible substrate.

4. The method for manufacturing a polymer nanospray needle based on stress induction according to claim 3, characterized in that: The flexible substrate is a PDMS flexible substrate, and the preparation process of the PDMS flexible substrate comprises the following steps: Step c1, wrapping a circle of aluminum foil tape around the bottom plate base, wherein the aluminum foil tape is arranged on the bottom plate base to form a fence to form a casting container; Step c2, injecting the PDMS mixed solution onto the bottom plate substrate in the enclosure of the casting container prepared in step c1; Step c3, placing the casting container with the PDMS mixed solution in step c2 in a vacuum oven and evacuating the vacuum oven for 5 to 10 minutes to remove bubbles; Step c4, placing the PMMA substrate with the PDMS mixed solution treated in step c3 in a 60-85° C. oven for curing for 2-4 hours to obtain a PDMS flexible substrate.

5. The method for manufacturing a polymer nanospray needle based on stress induction according to claim 4, characterized in that: In step c1, the enclosure shape is a cube or a cuboid; in step c2, the PDMS mixed solution is a mixture of PDMS and a curing agent in a ratio of 4:1 to 10:1, and the mixed PDMS mixed solution is placed in a vacuum oven and evacuated for 5 to 10 minutes to remove bubbles.

6. A method for manufacturing a polymer nanospray needle based on stress induction according to any one of claims 1 to 5, characterized in that: The photoresist used is SU-8 photoresist; The bottom plate substrate adopts a PMMA substrate, a glass substrate, a silicon wafer substrate, a PET substrate, or a PVP substrate.

7. A method for manufacturing a polymer nanospray needle based on stress induction according to claim 4 or 5, characterized in that: The PDMS flexible substrate used in the flexible substrate is replaced by a PET film, a PI film, a PMMA film, a hydrogel film, or a rubber layer; The aluminum foil tape is replaced by sealing film, BOPP tape, PET double-sided tape, glass fiber tape, Teflon tape, copper foil tape, plasma spray tape, polyimide tape, glass cloth tape, or masking tape.

8. A method for manufacturing a polymer nanospray needle based on stress induction according to any one of claims 1 to 5, characterized in that: The step baking parameters of the photoresist are as follows: the temperature is increased from 65°C to 85°C, and the temperature is increased by 5°C every 15 minutes. When the temperature reaches 85°C, the photoresist is baked for 30 minutes and then cooled to room temperature on the hot plate. And / or, in step 3, the bonding temperature is 40-50° C., the bonding pressure is 0.1-0.3 MPa, and the bonding time is 5-10 min.

9. A stress-induced polymer nanospray needle, characterized in that: The polymer nanospray needle is prepared by the stress-induced polymer nanospray needle manufacturing method described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Method for preparing n electric-jet-flow nano printing needle

    CN108466486A

  • Manufacturing method of ground motion sensor based on nanocracks

    CN112456435A