A wear-resistant coating containing modified aluminum oxide and preparation method thereof
By adding hyperbranched polymers to modify alumina in epoxy resin coatings, and by modifying the surface of nano-alumina with oleic acid and grafting it onto the surface, the toughness and wear resistance problems of epoxy resin coatings were solved, and the performance was significantly improved.
Patent Information
- Application Number
- CN202410596453.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Epoxy resin coatings suffer from poor toughness, low flexural strength and impact strength, and poor abrasion resistance.
Hyperbranched polymer-modified alumina is combined with waterborne epoxy resin. The surface of nano-alumina is modified with oleic acid and grafted with hyperbranched polymer to form hyperbranched polymer-modified alumina with thiol-terminated groups, which enhances its dispersibility and compatibility in epoxy resin.
It significantly improves the flexural properties, impact strength, and abrasion resistance of epoxy resin. The flexible ether bonds and rigid polyimide structure of the hyperbranched polymer enhance the stability and abrasion resistance of the coating.
Smart Images

Figure BDA0004839102560000021 
Figure BDA0004839102560000022 
Figure BDA0004839102560000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum oxide, in particular to a wear-resistant coating containing modified aluminum oxide and a preparation method thereof. Background Art
[0002] As a common inorganic nanoparticle, nano-alumina has good heat resistance, antistatic, mechanical strength and friction resistance, and is widely used in coatings, films, plastics, etc. Surface modification of nano-alumina and improving its dispersibility in polymer materials are research hotspots. Chinese patent CN104371274B discloses modified alumina composite materials, copper-clad substrates and their preparation methods. After the alumina particles are modified by silane coupling agents, active chemical groups such as amino groups and hydroxyl groups are formed on the surface, which can be connected with liquid crystal epoxy resins through chemical bonds, thereby improving the interaction between interfaces, reducing clustering, and improving the thermal conductivity and other properties of epoxy resins and copper-clad laminates. However, this patent does not improve the mechanical properties of epoxy resin materials such as bending and wear resistance.
[0003] Epoxy resin coating is a kind of thermosetting coating with excellent performance, which is widely used in the fields of sporting goods, electronic appliances, etc. However, traditional epoxy resin coating has problems such as poor toughness, low bending performance and impact strength, and poor wear resistance. Filling and modifying epoxy resin with fillers such as hyperbranched polymers and nano-alumina is an effective way to improve the mechanical properties of epoxy resin. Summary of the invention
[0004] The invention solves the problem that the mechanical properties and wear resistance of epoxy resin coating are poor.
[0005] The technical solution of the present invention is: a wear-resistant coating containing modified alumina, comprising the following raw materials, 82-96 parts by weight of waterborne epoxy resin, 4-18 parts by weight of hyperbranched polymer modified alumina, 0.2-0.4 parts by weight of defoamer, 0.1-0.3 parts by weight of leveling agent, and 0.15-0.3 parts by weight of thickener.
[0006] The preparation method of the hyperbranched polymer modified alumina is as follows:
[0007] Step S1, add glacial acetic acid, pyridine, 4,4'-biphenyl ether dianhydride, and 4-aminosalicylic acid to a reaction flask equipped with a reflux condenser, filter after the reaction, wash the precipitate with distilled water, and dry to obtain 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide). The preparation reaction formula is:
[0008]
[0009] Step S2, add toluene, 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide) in a ratio of 1 mol:(2-2.6) mol:(2-2.4) mol, pyridine and acryloyl chloride to a reaction bottle, react at 15-30°C for 6-10 hours, remove toluene by rotary evaporation after the reaction, wash with distilled water and methanol in turn, and dry to obtain 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide). The preparation reaction formula is:
[0010]
[0011] Step S3, adding N,N-dimethylformamide, 4,4'-biphenyl ether di(3-acryloxy-4-carboxybenzamide), trimethylolpropane tri(3-mercaptopropionate), and benzoin dimethyl ether to a reaction bottle, stirring to dissolve, placing the reaction bottle under an ultraviolet lamp, and performing a polymerization reaction under illumination to generate a hyperbranched polymer with terminal thiol groups; then adding oleic acid-modified alumina, dispersing it evenly, performing a modification reaction, filtering, washing the precipitate with distilled water and ethanol in turn, and drying to obtain a hyperbranched polymer-modified alumina.
[0012] The ratio of pyridine, 4,4'-biphenyl ether dianhydride and 4-aminosalicylic acid in step S1 is (4.5-7) mol:1 mol:(2-2.1) mol.
[0013] The reaction temperature in step S1 is 110-115° C. and the reaction time is 12-18 hours.
[0014] In step S3, the ratio of 4,4'-biphenyl ether di(3-acryloxy-4-carboxybenzamide), trimethylolpropane tri(3-mercaptopropionate), benzoin dimethyl ether, and oleic acid-modified alumina is (0.7-0.9) mol:1 mol:(0.008-0.01) mol:(150-400) g.
[0015] The polymerization reaction temperature in step S3 is 30-40°C and the time is 8-12h; the modification reaction temperature is 30-40°C and the time is 2-4h.
[0016] The preparation method of oleic acid modified alumina is as follows: add toluene and nano alumina into a reaction bottle equipped with a reflux condenser, and add oleic acid after uniform dispersion, wherein the ratio of nano alumina to oleic acid is 1g:(0.6-1.5)g; heat to 100-110°C, react for 12-24h, filter, wash with ethanol, and dry to obtain oleic acid modified alumina.
[0017] The preparation method of the wear-resistant coating containing modified alumina is as follows: 82-96 parts by weight of water-based epoxy resin are added to distilled water, and then 4-18 parts by weight of hyperbranched polymer modified alumina, 0.2-0.4 parts by weight of defoamer, 0.1-0.3 parts by weight of leveling agent, and 0.15-0.3 parts by weight of thickener are added, and shear dispersion is performed to obtain the wear-resistant coating containing modified alumina.
[0018] The technical effect of the present invention is that the present invention utilizes the carboxyl group of oleic acid to react with the hydroxyl group of nano-alumina at high temperature to achieve surface modification of the nano-alumina.
[0019] The 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzyl imide) of the invention contains two alkenyl groups, and a mercapto-ene photo-click reaction occurs with trimethylolpropane tris(3-mercaptopropionate) containing three mercapto groups under ultraviolet light, and the reaction ratio of the two is controlled to make trimethylolpropane tris(3-mercaptopropionate) excessive, so as to obtain a hyperbranched polymer with terminal mercapto groups, and then oleic acid-modified alumina is added, and the terminal mercapto groups of the hyperbranched polymer and the alkenyl groups of oleic acid modified on the surface of the alumina undergo a mercapto-ene click reaction, so as to obtain a hyperbranched polymer-modified alumina. The grafting of oleic acid molecular chains and hyperbranched polymers on the surface of nano-alumina is achieved.
[0020] The invention adds hyperbranched polymer modified alumina to epoxy resin coating. After being grafted and modified by oleic acid and hyperbranched polymer, nano alumina has better dispersibility, excellent compatibility with epoxy resin matrix, and is not easy to agglomerate; the uniformly dispersed nano alumina significantly improves the bending performance, impact strength and wear resistance of epoxy resin.
[0021] The hyperbranched polymer molecular chain grafted on the surface of nano-alumina contains flexible ether bonds and rigid polyimide structures, and has the advantages of high strength, strong structural stability, and good wear resistance. At the same time, the main chain of the hyperbranched polymer contains a large number of carboxyl groups. In the curing agent system such as 2-ethyl-4-methylimidazole, its carboxyl group can react with the epoxy resin, thereby grafting the hyperbranched polymer molecular chain into the epoxy resin, playing an excellent toughening and modification role, and further improving the bending performance, impact strength and wear resistance of the epoxy resin. DETAILED DESCRIPTION
[0022] The applicant will further explain the method of the present invention in detail below in conjunction with specific embodiments, with the purpose of enabling those skilled in the art to clearly understand the present invention. However, the following embodiments should not be understood to any extent as limiting the scope of protection claimed in the claims of the present invention.
[0023] The waterborne epoxy resin model in the present invention is epoxy resin E44. The CAS registration number of 4,4'-biphenyl ether dianhydride is 1823-59-2. The CAS registration number of 4-aminosalicylic acid is 65-49-6. The CAS registration number of trimethylolpropane tris(3-mercaptopropionate) is 33007-83-9. The nano-alumina brand is DCA-NL, and the average particle size is 500nm. The defoamer brand is BYK-021, the leveling agent brand is HR-6115, and the thickener brand is NP-606A.
[0024] Example 1
[0025] Step S1, add 40mL glacial acetic acid, 18mmol pyridine, 4mmol 4,4'-biphenyl ether dianhydride, 8mmol 4-aminosalicylic acid to a reaction bottle equipped with a reflux condenser, heat to 115°C and react for 12h, filter after reaction, wash the precipitate with distilled water, and dry to obtain 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide). The actual yield is 1.31g, and the yield is 56.5%.
[0026] Step S2, add 30mL toluene, 5mmol of 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide), 10mmol of pyridine and 10mmol of acryloyl chloride to a reaction bottle, react at 15°C for 10h, remove toluene by rotary evaporation after the reaction, wash with distilled water and methanol in turn, and dry to obtain 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide). The actual yield is 3.02g, and the yield is 87.8%.
[0027] Example 2
[0028] Step S1, add 50mL glacial acetic acid, 28mmol pyridine, 4mmol 4,4'-biphenyl ether dianhydride, 8.4mmol 4-aminosalicylic acid to a reaction bottle equipped with a reflux condenser, heat to 110°C and react for 18h, filter after reaction, wash the precipitate with distilled water, and dry to obtain 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide). The actual yield is 1.45g, and the yield is 62.5%.
[0029] Step S2: Add 40 mL of toluene, 5 mmol of 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide), 13 mmol of pyridine and 12 mmol of acryloyl chloride to a reaction bottle, react at 30°C for 6 hours, remove toluene by rotary evaporation after the reaction, wash with distilled water and methanol in turn, and dry to obtain 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide). The actual yield is 2.88 g, and the yield is 83.7%.
[0030] Example 3
[0031] (1) Add 100 mL of toluene and 10 g of nano-alumina to a reaction bottle equipped with a reflux condenser, add 6 g of oleic acid after uniform dispersion, heat to 110° C., react for 18 h, filter, wash with ethanol, and dry to obtain oleic acid-modified alumina.
[0032] (2) Add 100 mL of N,N-dimethylformamide and 18 mmol of the structural formula 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide) (prepared according to the method of Example 1), 20mmol of the structural formula is 0.2 mmol of trimethylolpropane tris(3-mercaptopropionate) and 0.2 mmol of benzoin dimethyl ether are stirred to dissolve, and the reaction bottle is placed under a 600 W ultraviolet lamp. The polymerization reaction is carried out at 30°C for 10 hours under illumination to generate a hyperbranched polymer with terminal thiol groups. Then, 2.8 g of oleic acid-modified alumina is added, and after uniform dispersion, the modification reaction is carried out at 30°C for 3 hours. The precipitate is filtered, and the precipitate is washed with distilled water and ethanol in turn, and dried to obtain a hyperbranched polymer-modified alumina.
[0033] (3) 96 g of waterborne epoxy resin was added to 100 mL of distilled water, and then 4 g of hyperbranched polymer modified alumina, 0.3 g of defoamer, 0.3 g of leveling agent, and 0.3 g of thickener were added, and sheared and dispersed to obtain a wear-resistant coating containing modified alumina.
[0034] Example 4
[0035] (1) Add 150 mL of toluene and 10 g of nano-alumina to a reaction bottle equipped with a reflux condenser, add 10 g of oleic acid after uniform dispersion, heat to 110° C., react for 12 h, filter, wash with ethanol, and dry to obtain oleic acid-modified alumina.
[0036] (2) Add 100 mL of N,N-dimethylformamide, 16 mmol of 4,4'-biphenyl ether di(3-acryloxy-4-carboxybenzamide) (prepared according to the method of Example 1), 20 mmol of trimethylolpropane tri(3-mercaptopropionate), and 0.2 mmol of benzoin dimethyl ether to a reaction flask, stir and dissolve, place the reaction flask under a 600 W ultraviolet lamp, and carry out polymerization reaction at 30° C. for 12 h under illumination, at which time a hyperbranched polymer with terminal thiol groups is generated; then add 5.6 g of oleic acid-modified alumina, disperse evenly, carry out modification reaction at 40° C. for 2 h, filter, wash the precipitate with distilled water and ethanol in turn, and dry to obtain a hyperbranched polymer-modified alumina.
[0037] (3) Add 90 g of waterborne epoxy resin to 100 mL of distilled water, then add 10 g of hyperbranched polymer modified alumina, 0.4 g of defoamer, 0.1 g of leveling agent, and 0.15 g of thickener, and shear and disperse to obtain a wear-resistant coating containing modified alumina.
[0038] Example 5
[0039] (1) Add 200 mL of toluene and 10 g of nano-alumina to a reaction bottle equipped with a reflux condenser, add 15 g of oleic acid after uniform dispersion, heat to 100° C., react for 24 h, filter, wash with ethanol, and dry to obtain oleic acid-modified alumina.
[0040] (2) Add 100 mL of N,N-dimethylformamide, 14 mmol of 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide) (prepared according to the method of Example 1), 20 mmol of trimethylolpropane tri(3-mercaptopropionate), and 0.16 mmol of benzoin dimethyl ether to a reaction flask, stir and dissolve, place the reaction flask under a 600 W ultraviolet lamp, and carry out polymerization reaction at 40° C. for 8 h under illumination, at which time a hyperbranched polymer with terminal thiol groups is generated; then add 8 g of oleic acid-modified alumina, disperse evenly, carry out modification reaction at 30° C. for 4 h, filter, wash the precipitate with distilled water and ethanol in turn, and dry to obtain a hyperbranched polymer-modified alumina.
[0041] (3) 82 g of waterborne epoxy resin was added to 100 mL of distilled water, and then 18 g of hyperbranched polymer modified alumina, 0.2 g of defoamer, 0.3 g of leveling agent, and 0.15 g of thickener were added, and sheared and dispersed to obtain a wear-resistant coating containing modified alumina.
[0042] Comparative Example 1
[0043] (3) Add 96 g of water-based epoxy resin into 100 mL of distilled water, then add 0.3 g of defoamer, 0.3 g of leveling agent, and 0.3 g of thickener, and shear and disperse to obtain a wear-resistant coating.
[0044] Comparative Example 2
[0045] (1) Add 100 mL of toluene and 10 g of nano-alumina to a reaction bottle equipped with a reflux condenser, add 6 g of oleic acid after uniform dispersion, heat to 110° C., react for 18 h, filter, wash with ethanol, and dry to obtain oleic acid-modified alumina.
[0046] (2) Add 96 g of water-based epoxy resin into 100 mL of distilled water, then add 4 g of oleic acid-modified alumina, 0.3 g of defoamer, 0.3 g of leveling agent, and 0.3 g of thickener, and shear and disperse to obtain a wear-resistant coating.
[0047] Comparative Example 3
[0048] (1) Add 100 mL of N,N-dimethylformamide, 18 mmol of 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide) (prepared according to the method of Example 1), 20 mmol of trimethylolpropane tri(3-mercaptopropionate), and 0.2 mmol of benzoin dimethyl ether into a reaction flask, stir and dissolve, place the reaction flask under a 600 W ultraviolet lamp, and perform polymerization reaction at 30° C. for 10 h under illumination, then add 2.8 g of oleic acid-modified alumina, disperse evenly, and perform modification reaction at 30° C. for 3 h, filter by suction, wash the precipitate with distilled water and ethanol in turn, and dry to obtain a hyperbranched polymer with terminal thiol groups.
[0049] (3) 96 g of waterborne epoxy resin was added to 100 mL of distilled water, and then 4 g of hyperbranched polymer, 0.3 g of defoamer, 0.3 g of leveling agent, and 0.3 g of thickener were added, and sheared and dispersed to obtain a wear-resistant coating.
[0050] Comparative Example 4
[0051] (1) Add 100 mL of N,N-dimethylformamide, 18 mmol of 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide) (prepared according to the method of Example 1), 20 mmol of trimethylolpropane tri(3-mercaptopropionate), and 0.2 mmol of benzoin dimethyl ether to a reaction flask, stir and dissolve, place the reaction flask under a 600 W ultraviolet lamp, and perform polymerization reaction at 30° C. for 10 h under illumination, thereby generating a hyperbranched polymer with terminal thiol groups; then add 2.8 g of nano-alumina, disperse evenly, mix at 30° C. for 3 h, filter, wash the precipitate with distilled water and ethanol in turn, and dry to obtain a hyperbranched polymer-alumina mixture.
[0052] (2) 96 g of waterborne epoxy resin was added to 100 mL of distilled water, and then 4 g of hyperbranched polymer-alumina mixture, 0.3 g of defoamer, 0.3 g of leveling agent, and 0.3 g of thickener were added, and sheared and dispersed to obtain a wear-resistant coating.
[0053] Performance test of the wear-resistant coating: 4 g of 2-ethyl-4-methylimidazole curing agent was added to the wear-resistant coating, first cured at 100°C for 2 hours, and then cured at 120°C for 3 hours to obtain an epoxy resin film.
[0054] The bending performance and impact strength of the film samples were tested according to the standard of GB / T2567-2008.
[0055] Table 1 Epoxy resin mechanical properties test
[0056]
[0057] Wear resistance test of epoxy resin film. The epoxy resin film was worn using a friction and wear tester. The film sample size was 30mm×10mm×8mm. The wear part was a 45# steel ring, the load was 19.6N, and the speed was 300r / min. The mass loss rate W was calculated.
[0058] W = (m-m1) / (L×d). m is the mass of the film sample before friction. m1 is the mass of the film sample after friction. L is the width of the sample. d is the width of the wear scar.
[0059] Table 2 Wear resistance test of epoxy resin
[0060] <![CDATA[Mass loss rate (g / m 2 )]]> Example 3 14.6 Example 4 9.8 Example 5 8.4 Comparative Example 1 31.9 Comparative Example 2 23.3 Comparative Example 3 27.2 Comparative Example 4 23.0
[0061] As can be seen from Table 1 and Table 2, hyperbranched polymer modified alumina is added to the epoxy resin coatings of Examples 3-5. After the nano alumina is grafted and modified by oleic acid and hyperbranched polymer, its dispersibility is better, its compatibility with the epoxy resin matrix is excellent, and it is not easy to agglomerate; the uniformly dispersed nano alumina has significantly improved the bending performance, impact strength and wear resistance of the epoxy resin. In addition, the hyperbranched polymer molecular chain contains flexible ether bonds and rigid polyimide structures, which have the advantages of high strength, strong structural stability, good wear resistance, etc. At the same time, the main chain of the hyperbranched polymer contains a large number of carboxyl groups. In the curing agent system such as 2-ethyl-4-methylimidazole, its carboxyl group can react with the epoxy resin, so that the hyperbranched polymer molecular chain is grafted into the epoxy resin, which plays an excellent toughening and modification role, and further improves the bending performance and impact strength of the epoxy resin.
[0062] Comparative Example 1 is a common epoxy resin coating, which has low bending performance and impact strength, large mass loss rate and poor wear resistance.
[0063] Compared with Example 1 and Comparative Example 1, oleic acid-modified alumina is added to the epoxy resin coating of Comparative Example 2. After the nano-alumina is modified with oleic acid, it has better dispersibility, excellent compatibility with the epoxy resin matrix, and is not easy to agglomerate, which is beneficial to improving the bending performance, impact strength and wear resistance of the epoxy resin. However, no hyperbranched polymer is added, and its mechanical properties are lower than those of Example 1.
[0064] The epoxy resin coating of Comparative Example 3 is added with a hyperbranched polymer, which contains a flexible ether bond and a rigid polyimide structure, and contains a large number of carboxyl groups in the main chain, which can react with the epoxy resin, so that the hyperbranched polymer molecular chain is grafted into the epoxy resin, which plays an excellent toughening and modification role and is beneficial to improving the mechanical properties of the epoxy resin. However, without the addition of nano-alumina, its bending performance, impact strength and wear resistance are lower than those of Example 1.
[0065] Compared with Example 1, in Comparative Example 4, when preparing the hyperbranched polymer-alumina mixture, the added nano alumina is not modified with oleic acid, the nano alumina does not contain olefinic groups, and cannot react with the terminal thiol groups of the hyperbranched polymer, resulting in no grafted oleic acid molecular chains and hyperbranched polymers on the surface of the nano alumina. The nano alumina has poor dispersibility, poor compatibility with epoxy resin, is prone to agglomeration, and has poor effect on enhancing the mechanical properties of the epoxy resin. The mechanical strength and wear resistance are lower than those of Example 1.
[0066] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A wear-resistant coating containing modified alumina, characterized in that: The wear-resistant coating comprises the following raw materials: 82-96 parts by weight of waterborne epoxy resin, 4-18 parts by weight of hyperbranched polymer modified alumina, 0.2-0.4 parts by weight of defoamer, 0.1-0.3 parts by weight of leveling agent, and 0.15-0.3 parts by weight of thickener; The preparation method of the hyperbranched polymer modified alumina is as follows: Step S1, adding glacial acetic acid, pyridine, 4,4'-biphenyl ether dianhydride, and 4-aminosalicylic acid to a reaction bottle equipped with a reflux condenser, filtering after the reaction, washing, and drying to obtain 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide); Step S2, adding toluene, 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide), pyridine and acryloyl chloride into a reaction bottle, removing toluene by rotary evaporation after the reaction, washing, and drying to obtain 4,4'-biphenyl ether di(3-acryloyloxy-4-carboxybenzamide); Step S3, adding N,N-dimethylformamide, 4,4'-biphenyl ether di(3-acryloxy-4-carboxybenzamide), trimethylolpropane tri(3-mercaptopropionate), and benzoin dimethyl ether to a reaction bottle, stirring to dissolve, placing the reaction bottle under an ultraviolet lamp, and performing a polymerization reaction under illumination, then adding oleic acid-modified alumina, dispersing evenly, performing a modification reaction, filtering, washing, and drying to obtain a hyperbranched polymer-modified alumina; In the step S1, the ratio of pyridine, 4,4'-biphenyl ether dianhydride, and 4-aminosalicylic acid is (4.5-7) mol: 1 mol: (2-2.1) mol; In step S2, the ratio of 4,4'-biphenyl ether di(3-hydroxy-4-carboxybenzamide), pyridine and acryloyl chloride is 1 mol:(2-2.6) mol:(2-2.4) mol; In the step S3, the ratio of 4,4'-biphenyl ether di(3-acryloxy-4-carboxybenzamide), trimethylolpropane tri(3-mercaptopropionate), benzoin dimethyl ether, and oleic acid-modified alumina is (0.7-0.9) mol:1 mol:(0.008-0.01) mol:(150-400) g.
2. The wear-resistant coating containing modified aluminum oxide according to claim 1, characterized in that: The reaction temperature in step S1 is 110-115° C. and the reaction time is 12-18 hours.
3. The wear-resistant coating containing modified aluminum oxide according to claim 1, characterized in that: The reaction temperature in step S2 is 15-30° C. and the reaction time is 6-10 h.
4. The wear-resistant coating containing modified aluminum oxide according to claim 1, characterized in that: In step S3, the polymerization reaction temperature is 30-40° C., and the time is 8-12 hours; the modification reaction temperature is 30-40° C., and the time is 2-4 hours.
5. The wear-resistant coating containing modified aluminum oxide according to claim 1, characterized in that: The preparation method of the oleic acid modified alumina is as follows: toluene and nano-alumina are added to a reaction bottle equipped with a reflux condenser, oleic acid is added after uniform dispersion, the temperature is raised to 100-110° C., the reaction is performed for 12-24 hours, suction filtered, washed, and dried to obtain the oleic acid modified alumina.
6. The wear-resistant coating containing modified alumina and the preparation method thereof according to claim 5, characterized in that: The ratio of the nano-alumina to oleic acid is 1g:(0.6-1.5)g.
7. A method for preparing a wear-resistant coating containing modified aluminum oxide according to any one of claims 1 to 6, characterized in that: 82-96 parts by weight of waterborne epoxy resin are added to distilled water, and then 4-18 parts by weight of hyperbranched polymer modified alumina, 0.2-0.4 parts by weight of defoamer, 0.1-0.3 parts by weight of leveling agent, and 0.15-0.3 parts by weight of thickener are added, and shear dispersion is performed to obtain a wear-resistant coating containing modified alumina.