A heat treatment method for chromium-molybdenum steel plates
By employing normalizing, reheating and low-temperature quenching, and long-term tempering to accelerate cooling, the problems of coarse grains and element segregation in chromium-molybdenum steel plates have been solved, improving their strength and toughness under high temperature and high pressure environments and meeting the application needs of thermal power equipment and the petrochemical industry.
Patent Information
- Application Number
- CN202410322382.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-20
AI Technical Summary
Existing chromium-molybdenum steel plates, after conventional normalizing and tempering processes, have coarse grains and severe element segregation, resulting in insufficient low-temperature impact toughness, making it difficult to meet the strength and toughness requirements under high-temperature and high-pressure environments.
A heat treatment method involving normalizing, reheating and low-temperature quenching, tempering, and long-term tempering to accelerate cooling is adopted. By controlling the heating temperature, time, and cooling rate, the grains are refined and dispersed carbides are formed, thereby improving elemental segregation and toughness.
It achieves high strength, good plasticity and toughness of chromium-molybdenum steel plate, and the transverse low temperature impact energy at -30℃ reaches more than 300J, meeting the use requirements in high temperature and high pressure environments.
Smart Images

Figure CN118345226B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metallurgical technology, specifically relating to a heat treatment method for chromium-molybdenum steel plates. Background Technology
[0002] Chromium-molybdenum steel is a widely used heat-resistant and hydrogen-resistant steel in many countries, and is extensively used in the manufacture of thermal power equipment and petrochemical industries. Because this type of steel operates in high-temperature, high-pressure environments with extremely harsh service conditions, it requires high strength, good plasticity and toughness, excellent weldability, and resistance to temper embrittlement. However, this type of steel is typically produced using conventional normalizing (accelerated cooling) and tempering processes. Due to the coarse initial grain size and elemental segregation after hot rolling, conventional normalizing (accelerated cooling) and tempering processes are insufficient to refine the grain size and improve elemental segregation. Dispersed carbides can pin dislocations, inhibit crack propagation, and improve the strength and toughness of the steel plate. However, after normalizing (accelerated cooling) and tempering, it is difficult to form a sufficiently large and dispersed amount of carbides to inhibit crack propagation, resulting in low low-temperature impact toughness. Typically, the transverse low-temperature impact toughness of the steel plate at -30℃ does not exceed 200J. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide a heat treatment method for chromium-molybdenum steel plates.
[0004] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a heat treatment method for chromium-molybdenum steel plates, characterized in that the heat treatment method includes normalizing, reheating and low-temperature quenching, tempering, and long-time tempering with accelerated cooling processes; the specific control parameters are as follows: 1) In the normalizing process, the steel plate is heated to 910-930℃ with a heating coefficient of 3-3.5 min / mm, and after holding at that temperature, it is removed from the furnace and air-cooled to room temperature; 2) In the reheating and low-temperature quenching process, the steel plate is heated to 870-890℃ with a heating coefficient of 3-3.5 min / mm, and then cooled to room temperature after being taken out of the furnace. 3) In the tempering process, the heating temperature is 650-680℃, the heating coefficient is 3.5-5 min / mm, and after holding at the temperature, the furnace is allowed to cool to room temperature. 4) The long-term tempering accelerated cooling process involves heating at a temperature of 690–710°C, with a heating coefficient of 3.5–5 min / mm, and then accelerating cooling to room temperature at a rate of ≥15°C / s after being taken out of the furnace.
[0005] The holding time in the normalizing process described in this invention is 60-80 minutes.
[0006] The holding time in the reheating low-temperature quenching process described in this invention is 30 to 40 minutes.
[0007] The holding time in the tempering process described in this invention is 50-60 minutes.
[0008] The holding time in the long-time tempering accelerated cooling process described in this invention is 480-600 min.
[0009] The chemical composition and mass percentage of the steel plate described in this invention are as follows: C: 0.11-0.14%, Si: 0.50-0.65%, Mn: 0.40-0.65%, P≤0.009%, S≤0.0014%, Cr: 1.15-1.45%, Al: 0.02-0.04%, Mo: 0.50-0.62%, with the balance being Fe and unavoidable impurities.
[0010] The steel plate of this invention has a thickness of 30-40 mm.
[0011] The steel plate of this invention has a yield strength ≥434MPa, tensile strength ≥578MPa, elongation ≥28%, and average transverse impact energy ≥300J at -30℃.
[0012] The metallographic structure of the steel plate described in this invention is bainite.
[0013] The beneficial effects of adopting the above technical solution are as follows: 1. The present invention performs normalizing heat treatment before reheating and quenching, which re-austenitizes the rolled steel plate structure, improves the original elongated structure of the rolled state, fully refines the grains, and improves the element segregation of the steel plate by uniformly alloying elements through long-term high-temperature holding. 2. The present invention adopts reheating and low-temperature quenching. On the basis of grain refinement by normalizing, low-temperature quenching prevents excessive grain growth during quenching and holding, further refining the grains. 3. The present invention adopts a long-term tempering and accelerated cooling process after tempering. Through long-term tempering, a large number of dispersed carbides precipitate in the steel. The large number of dispersed carbide precipitates inhibit the propagation of impact cracks and improve the toughness of the steel plate. The accelerated cooling process after long-term tempering prevents the formation of large-particle carbide precipitates during tempering and cooling, suppresses temper brittleness, and improves the toughness of the steel plate. Attached Figure Description
[0014] Figure 1 The image shows the metallographic structure of the chromium-molybdenum steel plate in Example 1. Detailed Implementation
[0015] The present invention will be further described in detail below with reference to specific embodiments.
[0016] Examples 1-8 A heat treatment method for chromium-molybdenum steel plates includes normalizing, reheating and low-temperature quenching, tempering, and long-time tempering with accelerated cooling. The specific process steps are as follows: 1) Normalizing: The steel plate is heated to 910-930℃ with a heating coefficient of 3-3.5 min / mm, held at that temperature for 60-80 min, and then air-cooled to room temperature. 2) Reheating and low-temperature quenching: The steel plate is heated to 870-890℃ with a heating coefficient of 3-3.5 min / mm. After holding at this temperature for 30-40 minutes, it is removed from the furnace and water-cooled to room temperature.
[0017] 3) Tempering: Heating temperature 650~680℃, heating coefficient 3.5~5min / mm, hold for 50~60min, then remove from the furnace and let cool to room temperature.
[0018] 4) Long-term tempering and accelerated cooling: heating temperature 690~710℃, heating coefficient 3.5~5min / mm, holding temperature for 480~600min, and then cooling to room temperature at a rate of ≥15℃ / s after taking it out of the furnace.
[0019] The production process parameters for each embodiment are shown in Table 1, the chemical composition and mass percentage of the steel plate are shown in Table 2, and the specifications and properties of the steel plate after heat treatment are shown in Table 3.
[0020]
[0021]
[0022] The remaining components in Table 2 are Fe and unavoidable impurities.
[0023]
[0024] Appendix Figure 1 The image shows the metallographic structure of the chromium-molybdenum steel plate from Example 1. Figure 1 It can be seen that the microstructure of the steel plate is bainitic (the figures for the other embodiments are similar, and the valley is omitted).
[0025] The above embodiments are only used to illustrate and not limit the technical solutions of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the present invention without departing from the spirit and scope of the present invention. Any modifications or partial substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A heat treatment method for chromium-molybdenum steel plates, characterized in that, The heat treatment method includes normalizing, reheating and low-temperature quenching, tempering, and long-time tempering with accelerated cooling; the specific control parameters are as follows. 1) In the normalizing process, the steel plate is heated to 910-930℃ with a heating coefficient of 3-3.5 min / mm, and after holding at that temperature, it is removed from the furnace and air-cooled to room temperature; 2) In the reheating and low-temperature quenching process, the steel plate is heated to 870-890℃ with a heating coefficient of 3-3.5 min / mm, and then cooled to room temperature after being taken out of the furnace. 3) In the tempering process, the heating temperature is 650-680℃, the heating coefficient is 3.5-5 min / mm, and after holding at the temperature, the furnace is allowed to cool to room temperature. 4) The long-term tempering and accelerated cooling process involves heating at a temperature of 690–710°C, with a heating coefficient of 3.5–5 min / mm, followed by accelerated cooling to room temperature at a rate of ≥15°C / s after being taken out of the furnace; the holding time is 480–600 min. The chemical composition and mass percentage of the steel plate are as follows: C: 0.11-0.14%, Si: 0.50-0.65%, Mn: 0.40-0.65%, P≤0.009%, S≤0.0014%, Cr: 1.15-1.45%, Al: 0.02-0.04%, Mo: 0.50-0.62%, with the balance being Fe and unavoidable impurities; The steel plate has a yield strength ≥434MPa, a tensile strength ≥578MPa, an elongation ≥28%, and an average transverse impact energy ≥300J at -30℃. The metallographic structure of the steel plate is bainite.
2. The heat treatment method for a chromium-molybdenum steel plate according to claim 1, characterized in that, The holding time in the normalizing process is 60-80 minutes.
3. The heat treatment method for a chromium-molybdenum steel plate according to claim 1, characterized in that, The holding time in the reheating low-temperature quenching process is 30 to 40 minutes.
4. The heat treatment method for a chromium-molybdenum steel plate according to claim 1, characterized in that, The holding time in the tempering process is 50 to 60 minutes.
5. The heat treatment method for a chromium-molybdenum steel plate according to claim 1, characterized in that, The thickness of the steel plate is 30-40mm.
Citation Information
Patent Citations
Heat treatment method of low-carbon bainite steel
CN117721274A