Environmentally friendly and degradable masterbatch and preparation method thereof
By using materials such as carboxyl functionalized polylactic acid and modified chitosan in the masterbatch, the problems of poor degradability and flammability of polylactic acid in traditional masterbatch are solved, and a product with excellent degradable, flame retardant and antibacterial properties is solved. Environmentally friendly masterbatch meets higher environmental protection and safety requirements.
Patent Information
- Application Number
- CN202410824651.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-06-25
AI Technical Summary
Traditional masterbatch uses polyethylene or polypropylene resin which has poor degradability and is difficult to meet environmental protection requirements. At the same time, polylactic acid has a low oxygen index and is flammable, and requires antibacterial properties in applications such as milk tea packaging and straws. It is difficult for existing technology to provide flame retardant, Antibacterial and degradable color masterbatch.
Carboxyl functionalized polylactic acid, modified chitosan, catalyst and lubricant are melted and blended in a twin-screw extruder to prepare an environmentally friendly and degradable color masterbatch. The modified chitosan is obtained through a specific chemical reaction to improve its Flame retardant, antibacterial and compatibility.
The prepared masterbatch has excellent degradability, mechanical properties, flame retardancy and antibacterial properties, has long-term and stable performance, and is suitable for environmentally friendly masterbatch applications.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of masterbatch preparation, and in particular relates to an environmentally friendly and degradable masterbatch and a preparation method thereof. Background Art
[0002] As people's living standards improve, they are more demanding on the aesthetics of plastic products. Traditional plastic coloring is to directly mix powdered pigments with resins. The disadvantages are that the pigments have poor compatibility with plastics, the pigments are easily scattered when added, causing environmental pollution, and endangering the health of operators.
[0003] In order to overcome the above shortcomings, masterbatches came into being. Masterbatches are pigments pre-dispersed in carrier resins. On the one hand, they can make the pigments have better dispersibility in plastics, and on the other hand, they can keep the pigments chemically stable and ensure the color stability of the products. Moreover, compared with traditional coloring methods, masterbatch coloring has the advantages of uniform coloring dispersion, excellent quality, no dye dust and excellent operating environment. It has quickly become one of the important materials in the plastic processing industry and is used in various industrial fields. However, with the increasingly prominent problems of environmental deterioration and energy shortage, traditional masterbatches usually use polyethylene or polypropylene resins. These materials have poor degradability and are difficult to meet people's environmental protection requirements. Therefore, environmentally friendly degradable materials are becoming more and more popular.
[0004] Common degradable materials include PBAT, PLA, PBS, etc. Among them, polylactic acid (PLA) is a polyester polymer obtained by polymerization with lactic acid as the main raw material. Its raw material is made of starch raw materials from renewable plant resources. After use, it can be completely degraded by microorganisms in nature, and finally generate carbon dioxide and water. Its source and post-treatment are extremely environmentally friendly, and it is an ideal green polymer material. In addition, polylactic acid has high strength and good rigidity, which makes it can be used to prepare hard plastic products. However, polylactic acid has a low oxygen index and is easy to burn when encountering open flames, which poses a safety hazard. Not only that, polylactic acid materials are used in milk tea packaging and straws, which are in direct contact with the human body and must have certain antibacterial properties. Therefore, it is urgent to invent a flame-retardant, antibacterial, and degradable masterbatch to meet the higher demands in the field of masterbatch preparation technology. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an environmentally friendly and degradable masterbatch and a preparation method thereof.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A method for preparing an environmentally friendly and degradable masterbatch, characterized in that it comprises the following steps:
[0008] The carboxyl functionalized polylactic acid, color powder, modified chitosan, catalyst and lubricant are mixed, added into a twin-screw extruder, melt blended, extruded and granulated to obtain an environmentally friendly and degradable masterbatch.
[0009] Furthermore, the raw materials are calculated in parts by weight as follows: 80-100 parts of carboxyl functionalized polylactic acid, 12-16 parts of color powder, 5-15 parts of modified chitosan, 0.1-0.3 parts of catalyst, and 2-4 parts of lubricant.
[0010] Furthermore, the catalyst is stannous chloride or stannous oxide.
[0011] Furthermore, the lubricant is epoxidized soybean oil or paraffin.
[0012] With carboxyl functionalized polylactic acid as the matrix, it has the properties of polylactic acid, giving the masterbatch excellent degradability and mechanical properties.
[0013] Furthermore, the modified chitosan is prepared by the following steps:
[0014] S1. In a three-necked flask equipped with a stirring device, tris(hydroxymethyl)aminomethane hydrochloride, triethylamine and N,N-dimethylformamide (DMF) were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 minutes. Then, phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 110°C and kept for reaction for 8 hours. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed three times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1; the ratio of tris(hydroxymethyl)aminomethane hydrochloride, triethylamine, DMF, and phosphorus oxychloride was 18.1g:15mL:100mL:15.3g;
[0015] Tris(hydroxymethyl)aminomethane hydrochloride reacts with phosphorus oxychloride to obtain intermediate 1; the reaction process is as follows:
[0016]
[0017] S2. In a three-necked flask equipped with a stirring device at room temperature, add intermediate 1, diethylene glycol dimethyl ether and N,N-diisopropylethylamine, mix well, add cyanuric chloride, control the reaction temperature to 55°C, react for 8 hours, filter, remove part of the solvent by rotary evaporation, and purify by column chromatography (the eluent is a mixed solvent of chloroform / ethyl acetate, the volume ratio of the two is 2:7), remove the eluent by rotary evaporation, and vacuum dry to obtain intermediate 2; the ratio of the amount of intermediate 1, diethylene glycol dimethyl ether, N,N-diisopropylethylamine, and cyanuric chloride is 32.9g:150mL:25.8g:19.4g;
[0018] Under the catalysis of N,N-diisopropylethylamine, intermediate 1 reacts with cyanuric chloride. By controlling the molar ratio of the two to be close to 2:1 and the cyanuric chloride to be slightly excessive, intermediate 2 is obtained. The reaction process is as follows:
[0019]
[0020] S3. In a three-necked flask equipped with a stirring device, add intermediate 2, sodium hydroxide, triethylamine and toluene in sequence, stir at room temperature for 30 minutes, add 3,5-dihydroxybenzaldehyde, control the reaction temperature to 70°C, keep the reaction for 6 hours, and filter after the reaction is completed. The filtrate is washed with saturated brine 3 times, dried with anhydrous magnesium sulfate, filtered again, and purified by column chromatography (the eluent is a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two is 2:5), and the eluent is removed by rotary evaporation to obtain intermediate 3; the ratio of the amount of intermediate 2, sodium hydroxide, triethylamine, toluene, and 3,5-dihydroxybenzaldehyde is 44.1g:3.9g:15mL:100mL:15.1g;
[0021] Sodium hydroxide reacts with the hydroxyl group on 3,5-dihydroxybenzaldehyde to form sodium phenolate with stronger nucleophilicity. Sodium phenolate, as a nucleophilic reagent, attacks the carbon atom connected to the chlorine atom on intermediate 2, so that the chlorine atom is replaced, thereby generating an ether bond; by controlling the molar ratio of 3,5-dihydroxybenzaldehyde to intermediate 2 to be close to 1:1 and 3,5-dihydroxybenzaldehyde to be slightly excessive, only one hydroxyl group on 3,5-dihydroxybenzaldehyde participates in the reaction, and triethylamine removes the hydrogen chloride generated by the reaction to obtain intermediate 3; the specific reaction process is as follows:
[0022]
[0023] S4. Add chitosan (relative molecular weight 1000) to a mixed solution of acetic acid and toluene (mass fraction of acetic acid is 12%), stir until it is completely dissolved, then add intermediate 3 and piperidine (condensation agent), stir and react at room temperature for 2 hours, drop sodium hydroxide solution to adjust the pH to 5.5, continue to react for 2 hours, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan; the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 3, and piperidine is 100mL:10g:15g:10mL;
[0024] Under the action of the condensation agent, the aldehyde group on the intermediate 3 condenses with the amino group on the chitosan to form an imine group (C=N Schiff base structure) to obtain modified chitosan; the specific reaction process is as follows:
[0025]
[0026] Chitosan is a polysaccharide with biodegradability and certain antibacterial properties. In addition, a large number of hydroxyl groups in the molecule can promote the dehydration of the matrix into carbon, convert the matrix into a high-concentration carbon layer, and improve the flame retardant properties of the matrix. Moreover, by modifying chitosan, its hydrophobicity is improved, the compatibility of chitosan and polylactic acid is improved, and the dispersion of modified chitosan in the matrix is promoted, so that the antibacterial and flame retardant properties of chitosan are fully exerted. In addition, the modified chitosan molecular chain also contains caged phosphonate structure, Schiff base structure and triazine structure, among which the caged phosphonate structure is a green and environmentally friendly flame retardant with strong stability. When burning, it will promote the formation of carbon layer, inhibit smoke release, and improve the flame retardant and smoke suppression properties of the matrix. In addition, the Schiff base structure can not only improve the flame retardancy of the matrix, but also improve the antibacterial properties of the matrix. Finally, the triazine structure will produce nitrogen-containing gas when burning, dilute and reduce the smoke density, and self-condense at high temperature to form melem to make the carbon layer compact, giving the matrix flame retardant and smoke suppression properties.
[0027] It should be noted that one end of the modified chitosan contains a hydroxyl group, which can produce a chemical bond with the carboxyl-functionalized polylactic acid under the action of a catalyst, thereby enhancing the interaction between the modified chitosan and the matrix, thereby improving the long-term stability of the modified chitosan performance.
[0028] Beneficial effects of the present invention:
[0029] 1. The masterbatch prepared by the present invention uses carboxyl functionalized polylactic acid as a matrix, which gives the masterbatch excellent degradability and mechanical properties.
[0030] 2. The introduction of chitosan is biodegradable and also gives the masterbatch certain flame retardancy and antibacterial properties. By modifying chitosan, compared with ordinary chitosan, the hydrophobicity is enhanced, the compatibility with polylactic acid is improved, and the effect on the mechanical properties of the masterbatch is small; it can also significantly enhance the flame retardancy and antibacterial properties of the masterbatch, and the performance is long-lasting and stable.
[0031] Therefore, the masterbatch prepared by the present invention has stable and efficient flame retardancy and antibacterial properties, and has excellent degradability and mechanical properties, is environmentally friendly, and has important application value in the field of masterbatch preparation technology. DETAILED DESCRIPTION
[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] Preparation of modified chitosan:
[0035] S1. In a three-necked flask equipped with a stirring device, 18.1 g of tris(hydroxymethyl)aminomethane hydrochloride, 15 mL of triethylamine and 100 mL of N,N-dimethylformamide were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 min. Then, 15.3 g of phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 110°C and kept for reaction for 8 h. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed three times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1.
[0036] S2. In a three-necked flask equipped with a stirring device, 32.9 g of intermediate 1, 150 mL of diethylene glycol dimethyl ether and 25.8 g of N, N-diisopropylethylamine were added at room temperature, and after mixing evenly, 19.4 g of cyanuric chloride was added, and the reaction temperature was controlled to 55 ° C. The reaction was carried out for 8 hours. After the reaction was completed, it was filtered, and part of the solvent was removed by rotary evaporation. Then, it was purified by column chromatography (the eluent was a mixed solvent of chloroform / ethyl acetate, and the volume ratio of the two was 2:7), the eluent was removed by rotary evaporation, and vacuum drying was performed to obtain intermediate 2;
[0037] S3. In a three-necked flask equipped with a stirring device, 44.1 g of intermediate 2, 3.9 g of sodium hydroxide, 15 mL of triethylamine and 100 mL of toluene were added in sequence, and the mixture was stirred at room temperature for 30 min. Then, 15.1 g of 3,5-dihydroxybenzaldehyde was added, and the reaction temperature was controlled to 70°C. The reaction was kept warm for 6 h. After the reaction was completed, the mixture was filtered, and the filtrate was washed with saturated brine 3 times, dried with anhydrous magnesium sulfate, filtered again, and purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 2:5), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0038] S4. Add 10 g of chitosan (relative molecular weight 1000) to a mixed solution of 100 mL of acetic acid and toluene (the mass fraction of acetic acid is 12%), stir until it is completely dissolved, then add 15 g of intermediate 3 and 10 mL of piperidine, stir and react at room temperature for 2 h, add sodium hydroxide solution dropwise to adjust the pH to 5.5, continue the reaction for 2 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.
[0039] Example 2
[0040] Preparation of modified chitosan:
[0041] S1. In a three-necked flask equipped with a stirring device, 36.2 g of tris(hydroxymethyl)aminomethane hydrochloride, 30 mL of triethylamine and 200 mL of N,N-dimethylformamide were mixed at room temperature, placed in an ice-water bath at 5°C, and stirred for 30 min. Then, 30.6 g of phosphorus oxychloride was slowly added dropwise, and the temperature was controlled not to exceed 20°C during the addition. After the addition was completed, the temperature was raised to 110°C and kept for reaction for 8 h. After the reaction was completed, the solvent was removed by filtration under reduced pressure, and the filter cake was washed three times with anhydrous ethanol, vacuum dried, and ground to obtain intermediate 1.
[0042] S2. In a three-necked flask equipped with a stirring device, 65.8 g of intermediate 1, 300 mL of diethylene glycol dimethyl ether and 51.6 g of N, N-diisopropylethylamine were added at room temperature, and the mixture was evenly mixed. Then, 38.8 g of cyanuric chloride was added, and the reaction temperature was controlled to 55 ° C. The reaction was carried out for 8 hours. After the reaction was completed, the mixture was filtered, and some solvents were removed by rotary evaporation. The mixture was purified by column chromatography (the eluent was a mixed solvent of chloroform / ethyl acetate in a volume ratio of 2:7), the eluent was removed by rotary evaporation, and the mixture was dried in vacuo to obtain intermediate 2.
[0043] S3. In a three-necked flask equipped with a stirring device, 88.2 g of intermediate 2, 7.8 g of sodium hydroxide, 30 mL of triethylamine and 200 mL of toluene were added in sequence, and the mixture was stirred at room temperature for 30 min. Then, 30.2 g of 3,5-dihydroxybenzaldehyde was added, and the reaction temperature was controlled to 70°C. The reaction was kept warm for 6 h. After the reaction was completed, the mixture was filtered, and the filtrate was washed 3 times with saturated brine, dried over anhydrous magnesium sulfate, filtered again, and purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 2:5), and the eluent was removed by rotary evaporation to obtain intermediate 3;
[0044] S4. Add 20 g of chitosan (relative molecular weight 1000) to a mixed solution of 200 mL of acetic acid and toluene (the mass fraction of acetic acid is 12%), stir until it is completely dissolved, then add 30 g of intermediate 3 and 20 mL of piperidine, stir and react at room temperature for 2 h, add sodium hydroxide solution dropwise to adjust the pH to 5.5, continue the reaction for 2 h, and after the reaction is completed, let it stand and precipitate, filter, wash with ethanol and water in turn, and dry in an oven to obtain modified chitosan.
[0045] The chemicals used in Examples 1 and 2 are as follows:
[0046] Tris(hydroxymethyl)aminomethane hydrochloride (McLean's reagent, MDL number: MFCD00012590), triethylamine (McLean's reagent, MDL number: MFCD00145448), N,N-dimethylformamide (McLean's reagent, MDL number: MFCD00003284), diethylene glycol dimethyl ether (McLean's reagent, MDL number: MFCD00008503), N,N-diisopropylethylamine (McLean's reagent, MDL number: MFCD00008868), cyanuric chloride (McLean's reagent, MDL number: MFCD00006046), 3,5-dihydroxybenzaldehyde (McLean's reagent, MDL number: MFCD00016611), chitosan McLean's reagent, MDL number: MFCD00161512, Mw: 1000).
[0047] Example 3
[0048] 80 g of carboxyl functionalized polylactic acid (produced by Shenzhen Meiluo Technology Co., Ltd.), 12 g of phthalocyanine red, 5 g of modified chitosan prepared in Example 1, 0.1 g of stannous chloride and 2 g of epoxy soybean oil were mixed and added to a twin-screw extruder, melt blended, extruded and granulated to obtain an environmentally friendly and degradable masterbatch.
[0049] Example 4
[0050] 90 g of carboxyl functionalized polylactic acid (produced by Shenzhen Meiluo Technology Co., Ltd.), 14 g of phthalocyanine green, 10 g of modified chitosan prepared in Example 2, 0.2 g of stannous oxide and 3 g of paraffin were mixed and added to a twin-screw extruder, melt blended, extruded and granulated to obtain an environmentally friendly and degradable masterbatch.
[0051] Example 5
[0052] 100 g of carboxyl functionalized polylactic acid (produced by Shenzhen Meiluo Technology Co., Ltd.), 16 g of phthalocyanine blue, 15 g of modified chitosan prepared in Example 2, 0.3 g of stannous oxide and 4 g of paraffin were mixed and added to a twin-screw extruder, melt blended, extruded and granulated to obtain an environmentally friendly and degradable masterbatch.
[0053] The chemicals used in Examples 3 to 5 are as follows:
[0054] Phthalocyanine red, phthalocyanine green and phthalocyanine blue were all produced by Meikelun Pigment Company; stannous oxide (McLean's reagent, MDL No.: MFCD00011243) and paraffin (McLean's reagent, MDL No.: MFCD00131611).
[0055] Comparative Example 1
[0056] The modified chitosan in Example 5 was replaced by ordinary chitosan (McLean reagent, MDL No.: MFCD00161512, Mw: 1000) of the same mass, and the remaining steps were the same as in Example 5.
[0057] Comparative Example 2
[0058] Commercially available PLA masterbatch produced by Dongguan Jinsuyan Plastic Technology Co., Ltd. was used.
[0059] Examples 3-5 and comparative examples 1-2 were made into corresponding shapes according to different test standards and subjected to the following performance tests:
[0060] The biodegradation rate was determined using the national standard GB / T 19811-2005;
[0061] The tensile properties are determined using the national standard GB / T 1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics";
[0062] The national standard GB / T 2406-2008 "Test method for combustion performance of plastics" is used to determine the limiting oxygen index;
[0063] The antibacterial properties before and after 30 days of storage were determined using QB / T 2591-2003A "Test methods and antibacterial effects of antibacterial plastics";
[0064] The measured results are shown in the following table:
[0065]
[0066] As can be seen from the above table, the flame retardancy and antibacterial properties of the masterbatch prepared in the embodiment of the present invention are better than those of the comparative example, and the degradability is excellent, and the addition of modified chitosan has little effect on the mechanical properties of the masterbatch. Therefore, the masterbatch of the present invention has important application value in the field of masterbatch preparation technology.
[0067] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0068] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A masterbatch, It is characterized in that The method comprises the following raw materials in parts by weight: 80-100 parts of carboxyl functionalized polylactic acid, 12-16 parts of color powder, 5-15 parts of modified chitosan, 0.1-0.3 parts of catalyst and 2-4 parts of lubricant; Wherein, the modified chitosan is prepared by the following steps: S1. Mix tris(hydroxymethyl)aminomethane hydrochloride, triethylamine and N,N-dimethylformamide, place in an ice-water bath at 5°C, stir thoroughly for 30 minutes, then add phosphorus oxychloride dropwise, the temperature does not exceed 20°C during the addition, react at 110°C for 8 hours, and after the reaction is complete, filter under reduced pressure, wash, vacuum dry, and grind to obtain intermediate 1 ; S2. After mixing intermediate 1, diethylene glycol dimethyl ether and N,N-diisopropylethylamine evenly, add cyanuric chloride, react at 55°C for 8h, and after the reaction is completed, filter, rotary evaporate, purify by column chromatography, rotary evaporate, and vacuum dry to obtain intermediate 2 ; S3, intermediate 2, sodium hydroxide, triethylamine and toluene were mixed, stirred at room temperature for 30 minutes, 3,5-dihydroxybenzaldehyde was added, and the reaction was carried out at 70°C for 6 hours. After the reaction was completed, the mixture was filtered, the filtrate was washed, dried, filtered again, purified by column chromatography, and rotary evaporated to obtain intermediate 3 ; S4. Add chitosan to the mixed solution of acetic acid and toluene, stir until it is completely dissolved, then add intermediate 3 and piperidine, stir and react at room temperature for 2 hours, adjust the pH to 5.5, continue to react for 2 hours, and after the reaction is completed, let it stand and precipitate, filter, wash, and dry to obtain modified chitosan. 。 2. A masterbatch according to claim 1, It is characterized in that In step S1, the ratio of tris(hydroxymethyl)aminomethane hydrochloride, triethylamine, DMF and phosphorus oxychloride is 18.1 g:15 mL:100 mL:15.3 g.
3. A masterbatch according to claim 1, It is characterized in that In step S2, the ratio of the amount of intermediate 1, diethylene glycol dimethyl ether, N,N-diisopropylethylamine, and cyanuric chloride is 32.9 g: 150 mL: 25.8 g: 19.4 g.
4. A masterbatch according to claim 1, It is characterized in that In step S3, the ratio of the amount of intermediate 2, sodium hydroxide, triethylamine, toluene, and 3,5-dihydroxybenzaldehyde is 44.1 g: 3.9 g: 15 mL: 100 mL: 15.1 g.
5. A masterbatch according to claim 1, It is characterized in that In step S4, the ratio of the mixed solution of acetic acid and toluene, chitosan, intermediate 3, and piperidine is 100 mL: 10 g: 15 g: 10 mL.
6. A masterbatch according to claim 1, It is characterized in that The catalyst is stannous chloride or stannous oxide.
7. A masterbatch according to claim 1, It is characterized in that The lubricant is epoxidized soybean oil or paraffin.
8. A method for preparing the masterbatch according to any one of claims 1 to 7, It is characterized in that The following steps are involved: The carboxyl functionalized polylactic acid, color powder, modified chitosan, catalyst and lubricant are mixed, added into a twin-screw extruder, melt blended, extruded and granulated to obtain an environmentally friendly and degradable masterbatch.
Citation Information
Patent Citations
Colored degradable anti-bacterial polylactic acid elastic fiber and preparation method thereof
CN106884226A
EVA environment-friendly color master batch
CN110982165A
Green environment-friendly degradable polylactic acid flame-retardant master batch and preparation method thereof
CN114539748A
Degradable environment-friendly plastic and preparation method thereof
CN116218177A
Anti-aging polyethylene color master batch and preparation method thereof
CN118006026A