A device and method for preparing POE elastomer

By using equipment such as jet reactor, flash tank and twin screw descent machine during the preparation of POE elastomer, the problem of unstable quality of POE elastomer in the prior art is solved, and uniform molecular weight and VOCs content are achieved. The low effect improves the processing performance and application prospects of the product.

CN118384522BActive Publication Date: 2024-12-06广东众和工程设计有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410399920.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-12-06
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

The quality of the products prepared by the prior art POE elastomers is unstable, the VOCs content is high and the molecular weight distribution is uneven, resulting in high gel content and poor devolatilization effect.

Method used

Using sequentially connected feeding system, jet reactor, termination kettle, first flash tank, second flash tank, twin screw desolator, centrifugal dewaterer and drying fluidization system, through mixing injectors and horizontal push flow Agitator, multiple flash evaporation and devolatilization treatments control the catalyst activity and polymerization reaction conditions, and achieve uniform molecular weight distribution of polymer and low VOCs content.

Benefits of technology

It improves the conversion rate of polymerization reaction and catalyst activity, reduces the gel content and VOCs content of POE elastomers, significantly improves product quality, and has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118384522B_ABST
    Figure CN118384522B_ABST
Patent Text Reader

Abstract

The invention discloses a device and method for preparing a POE elastomer, belonging to the technical field of polymer materials, the device for preparing a POE elastomer comprises a feeding system, a jet reactor, a stop kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidized system connected in sequence; a drying fluidized bed and a cooling fluidized bed connected in sequence in the drying fluidized system; a mixing ejector is provided inside the jet reactor; and a plug flow agitator is provided inside the stop kettle. The polymer molecular weight synthesized by the present invention is uniformly distributed, the gel content of the POE elastomer is low, the devolatilization effect is good, and the VOCs content of POE is as low as below 50ppm, the product quality is high, and it has a wide range of application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a device and a method for preparing a POE elastomer. Background Art

[0002] POE elastomer, or polyolefin elastomer, is a material with a special molecular structure, similar to that of ethylene propylene diene monomer (EPDM). Therefore, POE elastomer also exhibits excellent properties such as aging resistance, ozone resistance, and chemical resistance. Compared with traditional polymer materials, POE elastomer has better processing and molding properties, and no plasticizer needs to be added during molding. POE elastomer has been widely used in many fields such as the automotive industry, wire and cable sheathing, and plastic toughening agents. In the automotive industry, it can be used to improve the performance and durability of automotive parts; in the field of wire and cable sheathing, its aging resistance and chemical resistance make it an ideal sheath material; in terms of plastic toughening agents, POE elastomer can significantly improve the toughness and impact resistance of plastics.

[0003] The POE product prepared by the existing technology has unstable quality, high VOCs content and uneven molecular weight distribution. In view of this, the present application is proposed. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a device and a method for preparing a POE elastomer. The synthesized polymer has a uniform molecular weight distribution, the gel content of the POE elastomer is low, the devolatilization effect is good, and the VOCs content of the POE is as low as below 50ppm. The product quality is high and has broad application prospects.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A device for preparing POE elastomer, comprising a feeding system, a jet reactor, a termination kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidization system connected in sequence;

[0007] The drying fluidized bed and the cooling fluidized bed are sequentially connected to the drying fluidized bed;

[0008] A mixing ejector is provided inside the jet reactor;

[0009] A plug flow agitator is arranged inside the termination kettle.

[0010] Preferably, the jet reactor is also connected to an external circulation cooler.

[0011] Preferably, a first static mixer, a first filter and a second static mixer are sequentially provided between the termination kettle and the first flash tank; a second filter and a first preheater are sequentially provided between the first flash tank and the second flash tank.

[0012] Preferably, the feeding system includes an ethylene tank, a comonomer tank, a solvent tank, a hydrogen tank, a co-catalyst tank, a main catalyst tank, and an impurity-breaking agent tank; the comonomer tank, solvent tank, and impurity-breaking agent are connected to a premixing kettle, the co-catalyst tank and the main catalyst tank are connected to a third static mixer, the third static mixer, the ethylene tank, and the premixing kettle are connected to a fourth static mixer, and the fourth static mixer is connected to the jet reactor.

[0013] Preferably, at least one of the following (a) to (f) is satisfied:

[0014] (a) further comprising a terminator tank, wherein the terminator tank is connected to the terminator;

[0015] (b) further comprising an antioxidant tank, wherein the antioxidant tank is connected to the second static mixer;

[0016] (c) further comprising an anti-caking agent tank, wherein the anti-caking tank is connected to the drying fluidized bed;

[0017] (d) further comprising a nitrogen tank connected to the jet reactor;

[0018] (f) further comprises an ethylene recycling tank, wherein the ethylene recycling tank is connected to the premixer via a compressor.

[0019] Preferably, the centrifugal dehydrator forms a water circulation loop through the first buffer tank, the circulation pump and the twin-screw devolatilizer.

[0020] The present invention also provides a method for preparing a POE elastomer, based on the above-mentioned device for preparing a POE elastomer, comprising the following steps:

[0021] (1) premixing a main catalyst and a cocatalyst to obtain a premixed catalyst; premixing a comonomer, a breaker and a solvent to obtain a premix; premixing ethylene, the premix and the premixed catalyst and adding them to a jet reactor to perform a polymerization reaction;

[0022] (2) The material after the polymerization reaction enters the termination kettle, and the terminator is added to terminate the reaction. After the termination reaction, it is premixed again, then filtered, and premixed with an antioxidant. The premixed material enters the first flash tank for the first flash evaporation. The material after the first flash evaporation is filtered and preheated, and enters the second flash tank for flash evaporation. The material after the second flash evaporation is preheated and enters a twin-screw devolatilizer for devolatilization. The devolatilized material enters a centrifugal dehydrator for centrifugal dehydration, and finally enters a drying fluidization system, where an anti-caking agent is added for drying fluidization to obtain a POE elastomer.

[0023] Preferably, the main catalyst includes at least one of dimethylsilyl tert-butylamine tetramethylcyclopentadiene titanium dichloride, a constrained geometry metallocene catalyst, dibenzhydryl cyclopentadiene (2,7-di-tert-butyl-fluorenyl) zirconium dichloride, dimethylsilyl bridge-tetramethylcyclopentadienyl-tert-butylamino-dimethyltitanium, diphenyl carbon bridge-cyclopentadienyl-(2-dimethylamino-hutyl) zirconium dichloride and [N-(3,5-di-tert-butyl salicylidene)-2-diphenylphosphinophenylimine] titanium trichloride.

[0024] Preferably, the cocatalyst includes at least one of methylaluminoxane, modified methylaluminoxane, tri(perfluorophenyl)borane, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate and N,N-dicetylanilinium tetrakis(pentafluorophenyl)borate.

[0025] Preferably, the solvent includes at least one of isobutane, n-pentane, isopentane, n-hexane, methylcyclopentane, n-heptane, methylcyclohexane, isooctane and toluene.

[0026] Preferably, the comonomer includes at least one of 1-butene, 1-hexene, 1-octene and 1-decene.

[0027] Preferably, the impurity destroying agent includes at least one of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride and ethylaluminum dichloride.

[0028] Preferably, the terminator includes at least one of isooctyl alcohol, 1,3-propylene glycol and ethanol.

[0029] Preferably, the antioxidant includes at least one of antioxidant 168, antioxidant 1076, antioxidant 1010, antioxidant 3114, and antioxidant B225.

[0030] Preferably, the anti-caking agent includes at least one of calcium stearate emulsion, aluminosilicate, talc and oleamide.

[0031] Preferably, the polymerization reaction temperature is 80-160° C., the polymerization reaction time is 15-60 min, and the polymerization reaction pressure is 1.5-5 MPa.

[0032] Preferably, the pressure in the termination kettle is 6-10 MPa and the temperature is 130-140°C.

[0033] Preferably, the first flash evaporation pressure is 0.1-0.5 MPa, and the flash evaporation temperature is 68-85°C.

[0034] Preferably, the second flash evaporation pressure is 0.05-0.5 MPa, and the flash evaporation temperature is 170-200°C.

[0035] Preferably, the total length of the twin-screw devolatilizer is 2.5m, with four devolatilizer ports, the devolatilizer port pressure is controlled at 30Kpa, the temperature of each section of the devolatilizer is controlled at 115-200°C, the pressure is controlled at -10-30Kpa, and the twin-screw operating speed is 250-350r / min.

[0036] Preferably, the mass ratio of the solvent to ethylene is (5-6):1.

[0037] Preferably, the mass ratio of ethylene to comonomer is (1.5-3):1.

[0038] Preferably, the molar ratio of the main catalyst to the co-catalyst is (1.2-2):1.

[0039] Preferably, the mass of the main catalyst is 0.28 to 0.35‰ of the total mass of ethylene and comonomers.

[0040] Preferably, the molar ratio of the terminator to the co-catalyst is (1.2-1.8):1.

[0041] Preferably, the mass of the hydrogen is 0.2 to 0.4‰ of the total mass of ethylene and the comonomer.

[0042] The beneficial effects of the present invention are as follows: the present invention adopts a feeding system, a jet reactor, a termination kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidized system which are connected in sequence to prepare a POE elastomer, which can effectively improve the mixing effect of the rubber solution, has high activity of the catalyst, high conversion rate of polymerization reaction monomers, uniform molecular weight distribution of the polymer, low gel content of the POE elastomer, good devolatilization effect, and the VOCs content of the POE is as low as below 50 ppm, the product quality is high, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a schematic structural diagram of the device for preparing POE elastomer of the present invention.

[0044] Figure 2 It is a schematic structural diagram of the drying fluidization system of the present invention.

[0045] Markings in the figure: 1, jet reactor; 101, mixing ejector; 2, termination kettle; 201, plug flow agitator; 3, first flash tank; 301, first agitator; 4, second flash tank; 402, second agitator; 5, twin-screw devolatilizer; 6, centrifugal dehydrator; 7, drying fluidized system; 701, drying fluidized bed; 702, cooling fluidized bed; 8, external circulation cooler; 9, first static mixer; 10, first filter; 11, second static mixer; 12, second filter; 13, first preheater; 14. Second preheater; 15. First buffer tank; 16. Circulation pump; 17. Second buffer tank; 18. Ethylene recycling tank; 19. Compressor; 20. Silo; 21. Exhaust fan; 22. Ethylene tank; 23. Comonomer tank; 24. Solvent tank; 25. Hydrogen tank; 26. Co-catalyst tank; 27. Main catalyst tank; 28. Impurity destroyer tank; 29. ​​Premixing kettle; 30. Third static mixer; 31. Fourth static mixer; 32. Antioxidant tank; 33. Terminator tank; 34. Anti-caking agent tank; 35. Nitrogen tank. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.

[0047] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0048] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0049] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.

[0050] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.

[0051] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0052] like Figure 1 , Figure 2 As shown, the embodiment of the present application provides a device for preparing POE elastomer, including a feeding system, a jet reactor, a termination kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidization system connected in sequence;

[0053] The drying fluidized bed and the cooling fluidized bed are sequentially connected to the drying fluidized bed;

[0054] A mixing ejector is provided inside the jet reactor;

[0055] A plug flow agitator is arranged inside the termination kettle.

[0056] The present invention creatively adopts a feeding system, a jet reactor, a termination kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidized system which are connected in sequence to prepare a POE elastomer, which can effectively improve the mixing effect of the rubber solution, has high catalyst activity, high conversion rate of polymerization reaction monomers, uniform polymer molecular weight distribution, low gel content of the POE elastomer, good devolatilization effect, and the VOCs content of the POE is as low as below 50 ppm. The product quality is high and has broad application prospects.

[0057] The present invention adopts a jet reactor with a mixing ejector inside, so that the gas and liquid can achieve a full polymerization reaction, improve the polymerization reaction conversion rate, and increase the catalyst activity. The catalytic activity in the production process is about 230,000 Kg (POE) / Kg (cat.), which is higher than the catalytic activity of 200,000 Kg (POE) / Kg (cat.) in the existing production process. The polymerization reaction monomer conversion rate reaches more than 80% during the production process.

[0058] The present invention adopts a termination kettle with a plug flow agitator inside to effectively control the reaction end point, and can effectively control the polymerization reaction time, while making the molecular weight distribution of the polymer uniform, reducing the gel content of the product, and improving the product stability and processing performance.

[0059] The present invention creatively adopts the first flash tank and the second flash tank for flash evaporation, which increases the gas-liquid separation area and helps to improve the flash evaporation effect. The amount of ethylene flashed out of the flash tank during the production process is measured to reach more than 85% (wt) of the total amount of unreacted converted ethylene. This is higher than the existing production process in which the amount of ethylene flashed out of the flash tank can only reach 78% (wt) of the total amount of unreacted converted ethylene.

[0060] The flash temperature of the second flash tank is greater than the flash temperature of the first flash tank.

[0061] In one embodiment, the jet reactor is further connected to an external circulation cooler.

[0062] In one embodiment, the number of the external circulation coolers is two, and the two external circulation coolers are connected in series.

[0063] In one embodiment, the effective volume of the jet reactor is 200 L. The inner cavity aspect ratio is 1.5, the maximum working pressure of the reactor is 10 MPa, the maximum working temperature is 125 ° C, the mixing ejector 2 is a Venturi type mixing ejector, the jet port of the mixing ejector 2 is inserted into the lower part of the jet reactor, located at 30% of the liquid level, the inner wall of the jet reactor is mirror polished, and the jet reactor is provided with a liquid level transmitter, a pressure gauge, a safety valve, a pressure sensor, a temperature probe, a temperature transmitter, an emergency pressure relief valve, and is connected to the DCS system to monitor the changes in pressure and temperature in the reactor at any time.

[0064] In one embodiment, the termination kettle is provided with a plug flow agitator, which is provided with nine layers of plug slurry and is divided into three zones, and each zone can selectively add the terminator into one of the zones according to the polymerization reaction conditions. The effective volume of the termination kettle is 80L, the stirring speed is 58r / min, the inner cavity aspect ratio is 1.4, the maximum working pressure of the reactor is 15Mpa, the maximum working temperature is 230°C, and the inner wall of the termination kettle is mirror polished. The kettle is provided with a stirring current, a pressure gauge, a safety valve, a pressure sensor and a temperature probe, and is connected to the DCS system to monitor the changes in pressure and temperature in the kettle at any time.

[0065] In one embodiment, the effective volume of the first flash tank is 480L, the tank is provided with two first agitators, each agitator has three layers of turbine paddles, the stirring speed is 68r / min, the inner cavity aspect ratio is 1.2, the maximum working pressure of the first-stage flash tank is 1Mpa, the maximum working temperature is 180°C, the liquid level control range is 50%, and the tank is provided with a liquid level transmitter, a stirring current, a pressure gauge, a safety valve, a pressure sensor and a temperature probe, and is connected to the DCS system to monitor the changes in the liquid level, pressure and temperature in the tank at any time.

[0066] In one embodiment, the effective volume of the second flash tank is 180L, and the tank is provided with a second agitator, the agitator has three layers of turbine paddles, the stirring speed is 55r / min, the inner cavity aspect ratio is 1.5, the maximum working pressure of the secondary flash tank is 1Mpa, the maximum working temperature is 250°C, the liquid level control range is 50%, and the glue concentration is 53%. The tank is provided with a liquid level transmitter, a stirring current, a pressure gauge, a safety valve, a pressure sensor and a temperature probe, and is connected to the DCS system to monitor the changes in the liquid level, pressure and temperature in the tank at any time.

[0067] In one embodiment, the cooling fluidized bed is further connected to a silo.

[0068] In one embodiment, the drying fluidized bed, cooling fluidized bed and silo are all connected to an exhaust fan.

[0069] In one embodiment, the twin-screw devolatilizer is equipped with a motor current, a pressure gauge, a thermal heating system temperature and flow transmitter, a pressure sensor and a screw machine temperature transmitter, a pelletizer cutter speed transmitter, and a pelletizing water flow controller, and is connected to a DCS system to monitor the operation of the twin-screw devolatilizer at any time.

[0070] In one embodiment, the length of the drying fluidized bed is 6m, the temperature of the warm air is controlled at 30-45°C, and the amplitude of the fluidized bed is controlled at 5-20mm / s. The length of the cooling fluidized bed is 4.5m, the temperature of the cold air is controlled at 10-15°C, the amplitude of the fluidized bed is controlled at 7-18mm / s, and the temperature of the POE elastomer granules at the outlet of the cooling fluidized bed is controlled at 20°C before being sent to the rear silo. The gas from the drying fluidized bed, the cooling fluidized bed and the silo is sent to the RTO for treatment through an exhaust fan.

[0071] In one embodiment, the twin-screw devolatilizer is further connected to a second buffer tank.

[0072] In one embodiment, a first static mixer, a first filter and a second static mixer are sequentially arranged between the termination kettle and the first flash tank; a second filter and a first preheater are sequentially arranged between the first flash tank and the second flash tank.

[0073] In one embodiment, the feeding system includes an ethylene tank, a comonomer tank, a solvent tank, a hydrogen tank, a co-catalyst tank, a main catalyst tank, and an impurity-breaking agent tank; the comonomer tank, the solvent tank, and the impurity-breaking agent are connected to a premixing kettle, the co-catalyst tank and the main catalyst tank are connected to a third static mixer, the third static mixer, the ethylene tank, and the premixing kettle are connected to a fourth static mixer, and the fourth static mixer is connected to a jet reactor.

[0074] In one embodiment, at least one of the following (a) to (f) is satisfied:

[0075] (a) further comprising a terminator tank, wherein the terminator tank is connected to the terminator;

[0076] (b) further comprising an antioxidant tank, wherein the antioxidant tank is connected to the second static mixer;

[0077] (c) further comprising an anti-caking agent tank, wherein the anti-caking tank is connected to the drying fluidized bed;

[0078] (d) further comprising a nitrogen tank connected to the jet reactor;

[0079] (f) further comprises an ethylene recycling tank, wherein the ethylene recycling tank is connected to the premixer via a compressor.

[0080] The nitrogen tank does not work when the equipment is in normal operation, but when an emergency occurs in the device, the nitrogen tank is activated and nitrogen is introduced to terminate the reaction.

[0081] In one embodiment, the centrifugal dehydrator forms a water circulation loop through a first buffer tank, a circulation pump and a twin-screw devolatilizer.

[0082] The present invention also provides a method for preparing a POE elastomer, based on the above-mentioned device for preparing a POE elastomer, comprising the following steps:

[0083] (1) premixing a main catalyst and a cocatalyst to obtain a premixed catalyst; premixing a comonomer, a breaker and a solvent to obtain a premix; premixing ethylene, the premix and the premixed catalyst and adding them to a jet reactor to perform a polymerization reaction;

[0084] (2) The material after the polymerization reaction enters the termination kettle, and the terminator is added to terminate the reaction. After the termination reaction, it is premixed again, then filtered, and premixed with an antioxidant. The premixed material enters the first flash tank for the first flash evaporation. The material after the first flash evaporation is filtered and preheated, and enters the second flash tank for flash evaporation. The material after the second flash evaporation is preheated and enters a twin-screw devolatilizer for devolatilization. The devolatilized material enters a centrifugal dehydrator for centrifugal dehydration, and finally enters a drying fluidization system, where an anti-caking agent is added for drying fluidization to obtain a POE elastomer.

[0085] In one embodiment, the main catalyst includes at least one of dimethylsilyl tert-butylamine tetramethylcyclopentadiene titanium dichloride, a constrained geometry metallocene catalyst, dibenzhydryl cyclopentadiene (2,7-di-tert-butyl-fluorenyl) zirconium dichloride, dimethylsilyl bridge-tetramethylcyclopentadienyl-tert-butylamino-dimethyl titanium, diphenyl carbon bridge-cyclopentadienyl-(2-dimethylamino-hutyl) zirconium dichloride and [N-(3,5-di-tert-butyl salicylidene)-2-diphenylphosphinophenylimine] titanium trichloride.

[0086] In one embodiment, the co-catalyst includes at least one of methylaluminoxane, modified methylaluminoxane, tri(perfluorophenyl)borane, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate and N,N-di(hexadecyl)anilinium tetrakis(pentafluorophenyl)borate.

[0087] Preferably, the solvent includes at least one of isobutane, n-pentane, isopentane, n-hexane, methylcyclopentane, n-heptane, methylcyclohexane, isooctane and toluene.

[0088] In one embodiment, the comonomer includes at least one of 1-butene, 1-hexene, 1-octene, and 1-decene.

[0089] In one embodiment, the impurity destroying agent includes at least one of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride, and ethylaluminum dichloride.

[0090] In one embodiment, the terminator includes at least one of isooctyl alcohol, 1,3-propylene glycol, and ethanol.

[0091] In one embodiment, the antioxidant includes at least one of antioxidant 168, antioxidant 1076, antioxidant 1010, antioxidant 3114, and antioxidant B225.

[0092] In one embodiment, the anti-caking agent includes at least one of calcium stearate emulsion, aluminosilicate, talc, and oleamide.

[0093] In one embodiment, the polymerization reaction temperature is 80-160° C., the polymerization reaction time is 15-60 min, and the polymerization reaction pressure is 1.5-5 MPa.

[0094] In one embodiment, the pressure in the termination kettle is 6-10 MPa and the temperature is 130-140°C.

[0095] In one embodiment, the first flash evaporation pressure is 0.1-0.5 MPa, and the flash evaporation temperature is 68-85°C.

[0096] In one embodiment, the second flash evaporation pressure is 0.05-0.5 MPa, and the flash evaporation temperature is 170-200°C.

[0097] In one embodiment, the total length of the twin-screw devolatilizer is 2.5m, and there are four devolatilization ports in total. The pressure of the devolatilization ports is controlled at 30Kpa, the temperature of each section of the devolatilizer is controlled at 115-200°C, the pressure is controlled at -10-30Kpa, and the twin-screw operates at a speed of 250-350r / min.

[0098] In one embodiment, the mass ratio of the solvent to ethylene is (5-6):1.

[0099] In one embodiment, the mass ratio of ethylene to comonomer is (1.5-3):1.

[0100] In one embodiment, the molar ratio of the main catalyst to the co-catalyst is (1.2-2):1.

[0101] In one embodiment, the mass of the main catalyst is 0.28 to 0.35‰ of the total mass of ethylene and comonomers.

[0102] In one embodiment, the molar ratio of the terminator to the co-catalyst is (1.2-1.8):1.

[0103] In one embodiment, the mass of the hydrogen is 0.2 to 0.4‰ of the total mass of ethylene and the comonomer.

[0104] The amount of the antioxidant added is 2-8‰ of the material in the previous step (the material after the reaction is terminated, premixed and filtered).

[0105] The amount of impurity remover added is 1.1 to 1.5 times the molar amount of impurities in the system.

[0106] Wherein, the addition amount of the anti-caking agent is 3‰ to 6‰ of the centrifugally dehydrated material.

[0107] Optionally, the raw materials in the solvent tank can be pressurized by a pump and selectively passed through one or more of a deoxygenation bed, a drying bed, a desulfurization bed, a dechlorination bed, a carbon monoxide removal bed, and a carbon dioxide removal bed for refining according to the impurity situation. After the raw materials are refined, they enter the refined solvent tank for storage. An online water and oxygen detection probe is installed after the refining bed. If the water and oxygen in the refined raw materials are greater than 3ppm, they can be returned to the raw material tank through the reflux pipeline for re-refining.

[0108] Optionally, the raw materials in each gas and raw material tank (ethylene tank, co-catalyst tank, main catalyst tank, terminator tank, hydrogen tank, nitrogen tank, comonomer tank, impurity-breaking agent tank, anti-caking agent tank, antioxidant tank) can be pressurized and selectively refined through one or more of the deoxygenation bed, drying bed, desulfurization bed, dechlorination bed, carbon monoxide removal bed, and carbon dioxide removal bed according to the impurity situation, and directly used for the polymerization system. An online water and oxygen detection probe is installed behind the refining bed. If the water and oxygen in the refined gas raw material are >3ppm, the spare bed can be switched to ensure that the gas raw material meets the control index.

[0109] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.

[0110] Example 1

[0111] like Figure 1 , Figure 2 As shown, an embodiment of the present application provides a device for preparing POE elastomer, comprising a feeding system, a jet reactor, a stop kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidized system connected in sequence; the drying fluidized system comprises a drying fluidized bed and a cooling fluidized bed connected in sequence; a mixing ejector is provided inside the jet reactor; and a plug flow agitator is provided inside the stop kettle.

[0112] Wherein, the jet reactor is also connected to two external circulation coolers, and the two external circulation coolers are connected in series.

[0113] Wherein, the cooling fluidized bed is also connected to a silo.

[0114] Wherein, the drying fluidized bed, cooling fluidized bed and silo are all connected to the exhaust fan.

[0115] The twin-screw devolatilizer is equipped with motor current, pressure gauge, thermal heating system temperature and flow transmitter, pressure sensor and screw machine temperature transmitter, pelletizer cutter speed transmitter, pelletizer water flow controller, and is connected to the DCS system to monitor the operation of the twin-screw devolatilizer at any time.

[0116] Wherein, the twin-screw devolatilizer is also connected to the second buffer tank.

[0117] Among them, a first static mixer, a first filter and a second static mixer are arranged in sequence between the termination kettle and the first flash tank; a second filter and a first preheater are arranged in sequence between the first flash tank and the second flash tank.

[0118] Wherein, the feeding system includes an ethylene tank, a comonomer tank, a solvent tank, a hydrogen tank, a co-catalyst tank, a main catalyst tank, and an impurity-breaking agent tank; the comonomer tank, the solvent tank, and the impurity-breaking agent are connected to a premixing kettle, the co-catalyst tank and the main catalyst tank are connected to a third static mixer, the third static mixer, the ethylene tank, and the premixing kettle are connected to a fourth static mixer, and the fourth static mixer is connected to a jet reactor.

[0119] It also includes a terminator tank, an antioxidant tank, an anti-caking agent tank, a nitrogen tank, and an ethylene recycling tank. The terminator tank is connected to the terminator; the antioxidant tank is connected to the second static mixer; the anti-caking tank is connected to the dry fluidized bed; the nitrogen tank is connected to the jet reactor; and the ethylene recycling tank is connected to the premixer via a compressor.

[0120] Wherein, the centrifugal dehydrator forms a water circulation loop through the first buffer tank, the circulation pump and the twin-screw devolatilizer.

[0121] The method for preparing POE elastomer based on the above-mentioned device for preparing POE elastomer comprises the following steps:

[0122] (1) premixing dimethylsilyl tert-butylamine tetramethylcyclopentadiene titanium dichloride and methylaluminoxane to obtain a premixed catalyst; premixing l-octene, triethylaluminum and n-hexane to obtain a premix; premixing ethylene, the premix and the premixed catalyst and adding them to a jet reactor to perform a polymerization reaction;

[0123] (2) The material after the polymerization reaction enters the termination kettle, isooctyl alcohol is added to terminate the reaction, and is premixed again after the termination reaction, and then filtered and premixed with an antioxidant. The premixed material enters the first flash tank for the first flash distillation. The material after the first flash distillation is filtered, preheated to 170° C., and enters the second flash tank for flash distillation. The material after the second flash distillation is preheated to 130° C. and then enters a twin-screw devolatilizer for devolatilization. The devolatilized material enters a centrifugal dehydrator for centrifugal dehydration, and finally enters a drying fluidization system, an anti-caking agent is added for drying fluidization, and a POE elastomer is obtained.

[0124] The polymerization reaction temperature is 135° C., the polymerization reaction time is 20 min, and the polymerization reaction pressure is 2.5 MPa.

[0125] Wherein, the pressure in the termination kettle is 8Mpa and the temperature is 135°C.

[0126] Wherein, the first flash evaporation pressure is 0.2Mpa, and the flash evaporation temperature is 80°C.

[0127] Wherein, the second flash evaporation pressure is 0.1Mpa, and the flash evaporation temperature is 175°C.

[0128] In one embodiment, the twin-screw devolatilizer has a total length of 2.5 m, is provided with four devolatilization ports, the devolatilization port pressure is controlled at 30 KPa, the temperature of each section of the devolatilizer is controlled at 130° C., the pressure is controlled at 10 KPa, and the twin-screw operates at a speed of 300 r / min.

[0129] In one embodiment, the mass ratio of the solvent to ethylene is 5.5:1.

[0130] In one embodiment, the mass ratio of ethylene to comonomer is 2:1.

[0131] In one embodiment, the molar ratio of the main catalyst to the co-catalyst is 1.4:1.

[0132] In one embodiment, the mass of the main catalyst is 0.32‰ of the total mass of ethylene and comonomers.

[0133] In one embodiment, the molar ratio of the terminator to the co-catalyst is 1.2:1.

[0134] In one embodiment, the mass of the hydrogen is 0.3‰ of the total mass of ethylene and comonomer.

[0135] The amount of impurity remover added is 1.2 times the molar amount of impurities in the system.

[0136] The antioxidant is compounded by antioxidant 168 and antioxidant 1010 in a weight ratio of 1:2, wherein the amount of the antioxidant added is 4‰ of the material in the previous step (the material after the reaction is terminated, premixed and filtered).

[0137] Wherein, the addition amount of the anti-caking agent calcium stearate emulsion is 4.5‰ of the centrifugally dehydrated material.

[0138] In this embodiment, sampling was performed after the termination reaction was completed, and the collected gel solution was analyzed and calculated. The catalytic activity was about 230,000 Kg (POE) / Kg (cat.), the polymerization reaction monomer conversion rate was 80%, and no gel was detected in the product.

[0139] The amount of ethylene flashed out of the first flash tank in this embodiment is calculated to be 85% of the total amount of unreacted converted ethylene.

[0140] Among them, the VOCs content of the POE elastomer synthesized in this embodiment is 50ppm.

[0141] The molecular weight of the POE elastomer synthesized in this embodiment is 85,000, the molecular weight distribution is 1.86, and the octene insertion rate is 28.6%.

[0142] Comparative Example 1

[0143] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses a pipeline static mixer to replace the termination kettle (that is, this comparative example terminates in the pipeline), and the rest is the same.

[0144] Among them, sampling was carried out after the termination reaction of this comparative example, and the collected gel solution was analyzed and calculated. The catalytic activity was about 2120000Kg (POE) / Kg (cat.), the polymerization reaction monomer conversion rate was 76%, and a small amount of gel was detected in the product.

[0145] Among them, the amount of ethylene flashed out of the first flash tank in this comparative example was measured and calculated to reach 80% of the total amount of unreacted converted ethylene.

[0146] Among them, the VOCs content of the POE elastomer synthesized in this comparative example is 88 ppm.

[0147] The molecular weight of the POE elastomer synthesized in this comparative example is 103,000, the molecular weight distribution is 1.93, and the octene insertion rate is 27.6%.

[0148] Comparative Example 2

[0149] The difference between Comparative Example 2 and Example 1 is that only the first flash evaporation is performed in this comparative example, and the others are the same.

[0150] Among them, sampling was carried out after the termination reaction of this comparative example, and the collected gel solution was analyzed and calculated. The catalytic activity was about 230000Kg (POE) / Kg (cat.), the polymerization reaction monomer conversion rate was 80%, and no gel was detected in the product.

[0151] Among them, the amount of ethylene flashed out of the first flash tank in this comparative example was measured and calculated to reach 85% of the total amount of unreacted converted ethylene.

[0152] Among them, the VOCs content of the POE elastomer synthesized in this comparative example is 105 ppm.

[0153] The molecular weight of the POE elastomer synthesized in this comparative example is 88,000, the molecular weight distribution is 1.91, and the octene insertion rate is 27.3%.

[0154] Comparative Example 3

[0155] The difference between Comparative Example 3 and Example 1 is that only the first flash evaporation is performed in this comparative example, and the second flash evaporation is not used, and the other conditions are the same.

[0156] Among them, sampling was carried out after the termination reaction of this comparative example, and the collected gel solution was analyzed and calculated. The catalytic activity was about 228000Kg (POE) / Kg (cat.), the polymerization reaction monomer conversion rate was 80.2%, and no gel was detected in the product.

[0157] Among them, the amount of ethylene flashed out of the first flash tank of this comparative example was measured and calculated to reach 84.6% of the total amount of unreacted converted ethylene.

[0158] Among them, the VOCs content of the POE elastomer synthesized in this comparative example is 6350 ppm.

[0159] The molecular weight of the POE elastomer synthesized in this comparative example is 87,800, the molecular weight distribution is 1.89, and the octene insertion rate is 28.6%.

[0160] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a POE elastomer, characterized in that: The device for preparing POE elastomer comprises the following steps: (1) premixing a main catalyst and a cocatalyst to obtain a premixed catalyst; premixing a comonomer, a breaker and a solvent to obtain a premix; premixing ethylene, the premix and the premixed catalyst and adding them to a jet reactor to perform a polymerization reaction; (2) the material after the polymerization reaction enters the termination kettle, a terminator is added to terminate the reaction, the material is premixed again after the termination reaction, then filtered, premixed with an antioxidant, the premixed material enters the first flash tank for the first flash evaporation, the material after the first flash evaporation is filtered, preheated, and enters the second flash tank for flash evaporation, the material after the second flash evaporation is preheated and enters a twin-screw devolatilizer for devolatilization treatment, the devolatilized material enters a centrifugal dehydrator for centrifugal dehydration, and finally enters a drying fluidization system, an anti-caking agent is added for drying fluidization, and a POE elastomer is obtained; The device for preparing POE elastomer comprises a feeding system, a jet reactor, a termination kettle, a first flash tank, a second flash tank, a twin-screw devolatilizer, a centrifugal dehydrator and a drying fluidization system connected in sequence; The drying fluidized bed and the cooling fluidized bed are sequentially connected to the drying fluidized bed; A mixing ejector is provided inside the jet reactor; A plug flow agitator is provided inside the termination kettle; The feeding system includes an ethylene tank, a comonomer tank, a solvent tank, a hydrogen tank, a co-catalyst tank, a main catalyst tank, and an impurity-breaking agent tank; the comonomer tank, the solvent tank, and the impurity-breaking agent are connected to a premixing kettle, the co-catalyst tank and the main catalyst tank are connected to a third static mixer, the third static mixer, the ethylene tank, and the premixing kettle are connected to a fourth static mixer, and the fourth static mixer is connected to a jet reactor.

2. The method for preparing a POE elastomer according to claim 1, characterized in that: The main catalyst comprises at least one of dimethylsilyl tert-butylamine tetramethylcyclopentadiene titanium dichloride, a constrained geometry metallocene catalyst, dibenzylidene cyclopentadiene (2,7-di-tert-butyl-fluorenyl) zirconium dichloride, dimethylsilyl bridge-tetramethylcyclopentadienyl-tert-butylamino-dimethyl titanium, diphenyl carbon bridge-cyclopentadienyl-(2-dimethylamino-hutyl) zirconium dichloride and [N-(3,5-di-tert-butyl salicylidene)-2-diphenylphosphinophenylimine] titanium trichloride; and / or The cocatalyst comprises at least one of methylaluminoxane, modified methylaluminoxane, tri(perfluorophenyl)borane, triphenylcarbon tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate and N,N-dicetylanilinium tetrakis(pentafluorophenyl)borate; and / or The solvent comprises at least one of isobutane, n-pentane, isopentane, n-hexane, methylcyclopentane, n-heptane, methylcyclohexane, isooctane and toluene; and / or The comonomer comprises at least one of 1-butene, 1-hexene, 1-octene and 1-decene; and / or The impurity destroying agent comprises at least one of triethylaluminum, triisobutylaluminum, trihexylaluminum, trioctylaluminum, diethylaluminum chloride and ethylaluminum dichloride; and / or The terminator comprises at least one of isooctyl alcohol, 1,3-propylene glycol and ethanol; and / or The antioxidant comprises at least one of antioxidant 168, antioxidant 1076, antioxidant 1010, antioxidant 3114, and antioxidant B225; and / or The anti-caking agent includes at least one of calcium stearate emulsion, aluminosilicate, talc and oleamide.

3. The method for preparing a POE elastomer according to claim 1, characterized in that: The polymerization reaction temperature is 80-160° C., the polymerization reaction time is 15-60 min, and the polymerization reaction pressure is 1.5-5 MPa; and / or The pressure in the termination kettle is 6-10 MPa and the temperature is 130-140° C.; and / or The first flash evaporation pressure is 0.1-0.5 MPa, and the flash evaporation temperature is 68-85° C.; and / or The second flash evaporation pressure is 0.05-0.5 MPa, and the flash evaporation temperature is 170-200° C.; and / or The total length of the twin-screw devolatilizer is 2.5m, and it is equipped with four devolatilizer ports. The pressure of the devolatilizer ports is controlled at 30Kpa, the temperature of each section of the devolatilizer is controlled at 115-200°C, the pressure is controlled at -10-30Kpa, and the twin-screw operating speed is 250-350r / min.

4. The method for preparing a POE elastomer according to claim 1, characterized in that: The mass ratio of the solvent to ethylene is (5-6):1; and / or The mass ratio of ethylene to comonomer is (1.5-3):1; and / or The molar ratio of the main catalyst to the co-catalyst is (1.2-2):1; and / or The mass of the main catalyst is 0.28-0.35‰ of the total mass of ethylene and comonomers; and / or The molar ratio of the terminator to the co-catalyst is (1.2-1.8):1; and / or The mass of the hydrogen is 0.2 to 0.4‰ of the total mass of ethylene and the comonomer.

5. The method for preparing a POE elastomer according to claim 1, characterized in that: The jet reactor is also connected to an external circulation cooler.

6. The method for preparing a POE elastomer according to claim 1, characterized in that: A first static mixer, a first filter and a second static mixer are sequentially arranged between the termination kettle and the first flash tank; a second filter and a first preheater are sequentially arranged between the first flash tank and the second flash tank.

7. The method for preparing a POE elastomer according to claim 1, characterized in that: Satisfy at least one of the following (a) to (f): (a) further comprising a terminator tank, wherein the terminator tank is connected to the terminator; (b) further comprising an antioxidant tank, wherein the antioxidant tank is connected to the second static mixer; (c) further comprising an anti-caking agent tank, wherein the anti-caking agent tank is connected to the drying fluidized bed; (d) further comprising a nitrogen tank connected to the jet reactor; (f) further comprises an ethylene recycling tank, wherein the ethylene recycling tank is connected to the premixer via a compressor.

8. The method for preparing a POE elastomer according to claim 1, characterized in that: The centrifugal dehydrator forms a water circulation loop through the first buffer tank, the circulation pump and the twin-screw devolatilizer.