A crystallizer and a design method thereof
By designing a mold with a curved surface structure that combines narrow-surface copper plates and wide-surface copper plates, combined with the arrangement of cooling water tanks and fastening holes, the problems of edge cracks in the narrow-surface cast slab and short life of the copper plates in the existing technology are solved, and the narrow-surface and large-surface mold is achieved. The production of cast slabs with curved surfaces, large concave amounts and defect-free corners improves production efficiency and the life of the copper plate.
Patent Information
- Application Number
- CN202410788229.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-19
AI Technical Summary
It is difficult for the existing mold to effectively control edge cracks when producing narrow-surface cast slabs, resulting in low yield and production efficiency, and short life of the copper plate. It cannot meet the requirements of narrow-surface large arcs, large concave amounts, and defect-free corners.
A crystallizer including two wide-faced copper plates and two narrow-faced copper plates was designed. The working surface of the narrow-faced copper plates is a curved surface. Through the taper compensation value and adjustment factor, a continuous smooth transition between the convex area in the middle and the flat area on the edge is achieved. , combined with the arrangement of the cooling water tank and fastening holes, to meet the solidification shrinkage characteristics of the cast billet and ensure that the cast billet adheres well to the copper plate during the entire process.
Significantly reduces the width of edge cracks during the rolling process of wide and thick plates, ensures high-temperature over-straightening of the corners of the billet, prevents cracks, improves the service life of the mold, and achieves narrow surfaces, large arc surfaces, and large concavities , the production of billets with nearly right-angled corners.
Smart Images

Figure CN118385484B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of metal casting, and specifically relates to a crystallizer and a design method thereof. Background Art
[0002] Edge cracks are a type of linear surface crack defect that occurs at the edge of medium and thick plates and is parallel to the rolling direction during the rolling process. This type of crack is generally located at the edge of the steel plate with a width of 40~120mm and is distributed in the form of several lines with a depth of 0.1~1mm. In the actual production process, wide and thick plates with high edge cracks are often widened and rolled to remove the edge cracks, or the corners of the wide and thick slabs are rounded off before they are rolled off the production line. However, this will greatly reduce the yield rate and production efficiency of the wide and thick plates, causing huge economic losses to users.
[0003] At present, it is generally believed that the formation of edge cracks is caused by the corner folding caused by the rapid drop in temperature of the intermediate billet corner during the rolling process of wide and thick plates. However, a large number of field practices have shown that the edge cracks of medium and thick plates are mainly caused by the formation of "drawing" defects and cracking on the narrow surface of the intermediate billet during the longitudinal rolling and stretching process, and then gradually flipping to the edge of the wide surface of the steel plate during the thinning and rolling process.
[0004] A large number of experiments have shown that under the current mainstream medium and thick plate and wide and thick plate production lines and their rolling processes at home and abroad, in order to effectively prevent the "drawing" crack defects on the narrow surface of the intermediate billet from flipping to the edge of the steel plate during the rolling process, the narrow surface of the ingot must have a large arc-shaped concave structure (concave arc span / ingot thickness ≥ 0.8, concave amount ≥ 10mm).
[0005] In order to prepare narrow-faced concave structure ingots, Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B proposed a crystallizer with a convex block structure in the middle of a narrow copper plate. In the above two prior arts, the middle convex block of the narrow copper plate is an arc structure, and the edge is a horizontal base surface, and the two are transitioned by tangency. However, in the actual implementation process, the arc convex block and the horizontal base surface of the edge cannot be tangent. To achieve a smooth tangent transition between the two interfaces, it is necessary to introduce a transition arc tangent to the two at the junction of the arc convex block and the horizontal base surface of the edge. Affected by the excessive width occupied by the transition arc and the horizontal base surface of the edge of the copper plate, the width of the arc convex block in the middle of the copper plate is greatly reduced, which cannot meet the requirement of effectively controlling the width of the edge crack of the narrow face of the ingot concave arc span / ingot thickness ≥ 0.8. At the same time, in the actual implementation process of the above two existing technologies, due to the combined effects of the large and rapid concave in the middle of the narrow surface of the ingot during the solidification process and the pressure reduction at the end of solidification, the middle of the narrow surface of the ingot presents an obvious nearly "triangular" concave structure, which causes the ingot to form double-strand shape defects on both sides of the thickness centerline during the actual rolling process, and even deep folding line defects in the middle of the thickness of the wide and thick plate.
[0006] In view of the defects of Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B, Chinese utility model patent CN214349470U and Chinese invention patent CN112846116A proposed a crystallizer with a narrow face as a full arc face. That is, the working surface of the narrow copper plate of the crystallizer is designed from top to bottom as an arc-shaped structure with the same radius in the horizontal direction, and the highest protrusion height of the arc surface is 10~20mm, so as to realize the preparation of the ingot with a narrow face, large arc surface and large inner concave structure. However, since the working surface of the narrow copper plate in the above two prior arts is the same arc-shaped structure from the upper mouth to the lower mouth, the corner of the ingot formed by the solidification of the molten steel in the crystallizer presents an obvious acute angle structure (the narrow face transverse arc copper plate and the wide face flat copper plate form an acute angle). Affected by this, on the one hand, the heat transfer rate of the corners of the ingot with the sharp-angle structure in the secondary cooling casting zone is significantly accelerated, so that when producing continuous casting ingots of micro-alloyed steel containing Nb, V, Al, etc., the ingot is prone to transverse crack defects at the corners due to the excessively low corner temperature when passing through the straightening zone; on the other hand, the narrow copper plate of the crystallizer adopts the same arc-shaped structure from top to bottom horizontally. Under the action of solidification shrinkage, the corners of the ingot with the sharp-angle structure separate from the copper plate prematurely to form a large gap, which causes the formation of coarse austenite grains at the corners of the ingot shell, which is also not conducive to the control of cracks at the corners of the ingot.
[0007] In view of the defects of Chinese utility model patent CN214349470U and Chinese invention patent CN112846116A, Chinese invention patent CN115815545A proposes a crystallizer with a transition structure in which the convex arc in the middle is directly connected to the straight edge area, thereby ensuring the preparation of a narrow-surface, large-arc, large-indentation, right-angled structure of a casting blank, significantly reducing the width of the edge crack, while also ensuring that the corner temperature of the casting blank during the solidification process in the casting stream in the second cooling zone is not lower than the corner of the traditional narrow-surface flat casting blank, effectively reducing the occurrence of cracks in the corner of the casting blank. However, since the middle arc surface and the straight edge area of the copper plate in the above-mentioned prior art are directly intersected to transition, the actual solidification process is affected by the surface tension of the molten steel and the liquid protective slag, and the solidified blank shell at the intersection transition zone cannot fit with the copper plate for heat transfer due to the sudden convexity of the middle arc surface, which easily leads to a steel leakage accident in the transition zone due to the thin solidified blank shell.
[0008] The crystallizer of Chinese invention patent CN117139575A, based on the crystallizer of Chinese invention patent CN115815545A, further introduces an arc transition zone at the junction of the central convex arc and the edge straight zone. The effect of this approach is reduced to the disadvantage of the crystallizer of Chinese utility model patent CN204997018U and Chinese invention patent CN106270433B, that is, the solidification process of the billet is prone to form a "triangular" concave structure in the middle of the narrow surface of the billet due to the excessive width occupied by the edge straight zone and the transition zone.
[0009] At the same time, the arc-shaped working surfaces of the crystallizers of Chinese utility model patent CN204997018U, Chinese invention patent CN106270433B, Chinese utility model patent CN214349470U, and Chinese invention patent CN112846116A do not take into account the shrinkage of the billet in the thickness direction in the crystallizer. In the actual slab continuous casting process, the billet solidifies in the crystallizer, and shrinks by 1 to 3 mm in the thickness direction. That is, the width of the narrow copper plate of the actual crystallizer from the upper mouth to the lower mouth is linearly reduced by 1 to 3 mm. In the above-mentioned developed crystallizers, whether the working surface is designed with the same convex block in the middle or the same arc structure, the actual solidification characteristics of the billet are not taken into account. The shrinkage of the billet in the thickness direction during the downward solidification process will "lock" the two sides of the convex block or arc in the middle of the crystallizer, thereby greatly wearing out the two sides of the arc surface in the middle and lower part of the copper plate and unable to serve for a long time. Although the copper plate of Chinese invention patent CN115815545A takes this problem into consideration, it converts all the solidification shrinkage of the ingot along the thickness direction into the reduction of the span of the middle arc, that is, it does not take into account the shrinkage of the straight edge area. This causes the concave arc surface of the ingot at the intersection of the straight edge area and the middle arc to separate from the arc side surface of the copper plate during the solidification process of the ingot, further aggravating the risk of steel leakage in the ingot in the junction area.
[0010] Chinese invention patent CN112118924A discloses a crystallizer for compensating for the shrinkage of the shell during solidification in the crystallizer. Although its narrow copper plate also proposes a convex arc structure, the height of the protrusion gradually decreases from the upper mouth to the lower mouth of the crystallizer, and is even reduced to a flat structure. That is, the crystallizer structure cannot produce a narrow concave slab.
[0011] In addition, the above-mentioned developed narrow-faced crystallizers with convex structures have not considered the nonlinear change in the height direction of the shrinkage of the billet along the width direction in the crystallizer, that is, the billet shrinks faster in the middle and upper part of the crystallizer toward the center of the width, and shrinks relatively slowly in the middle and lower part. In the narrow-faced concave billet prepared by the above-mentioned developed crystallizer, the billet cannot obtain efficient heat transfer from the copper plate during the solidification process in the middle and upper part, so the grains in the corners of the billet are often coarse, and the proportion of corner crack defects in the actual production process is high; in the middle and lower part of the crystallizer, the billet shell with slowed shrinkage and the copper plate form mutual extrusion, which aggravates the wear of the copper plate in the middle and lower part of the crystallizer.
[0012] To this end, taking into account the control effect of edge cracks on wide and thick plates, the quality of the corners of the ingot, and the service life of the crystallizer, it is urgent to develop a crystallizer that can simultaneously meet the requirements of narrow surface, large arc surface, large inner concave amount, corner-free defect-free ingot production, and long service life of copper plates. Summary of the invention
[0013] Therefore, the technical problem to be solved by the present application is to provide a crystallizer and a design method thereof, wherein the crystallizer has a long service life and can meet the production requirements of defect-free ingots with narrow faces, large arc surfaces, large inner concave amounts, and nearly right-angle structures at the corners.
[0014] In order to solve the above problems, the present application provides a crystallizer, comprising two relatively wide copper plates and two relatively narrow copper plates, which are combined to form a crystallizer cavity for solidifying molten steel into narrow concave ingots; the narrow copper plates include a top surface, a bottom surface and a working surface, and the working surface is convex toward the direction of the crystallizer cavity and contacts the ingots;
[0015] Among them, the working surface is a curved surface, and the curved surface conforms to the formula:
[0016]
[0017] Wherein, B1 is the taper compensation value of the working surface at each height from the top surface to the bottom surface of the narrow copper plate; D1 is the lateral morphology of the working surface at each height from the top surface in the width direction of the narrow copper plate;
[0018] Among them, in the width direction of the narrow copper plate, the lateral morphology D1 of the working surface at each height from the top surface conforms to the formula:
[0019]
[0020] In the formula, x is the horizontal distance from the transverse center line of the narrow copper plate; B2 is the raised height of the working surface at the height of the top surface of the narrow copper plate, and the value range is 10~18mm; B3 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate; B4 is the correction value of the taper compensation.
[0021] Optionally, the taper compensation value B1 of the working surface of the narrow copper plate from the top surface to the bottom surface conforms to the formula:
[0022]
[0023] In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface of the narrow copper plate;
[0024] The adjustment factor B3 of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate conforms to the formula:
[0025]
[0026] Where l1 is the height of the crystallizer;
[0027] The taper compensation correction value B4 conforms to the formula:
[0028]
[0029] Where l2 is the width of the top surface of the narrow copper plate; y0 is the y value when B1 takes the maximum value.
[0030] Optionally, in the height direction of the crystallizer, the width of the narrow copper plate decreases linearly by 1 to 3 mm from the top surface to the bottom surface.
[0031] Optionally, the side of the narrow copper plate facing away from the ingot is a cooling surface, and the cooling surface is provided with a fastening hole, a first cooling water trough, a second cooling water trough and a third cooling water trough;
[0032] At least two rows of fastening holes are provided, and at least two rows of fastening holes are symmetrically arranged along the transverse center line of the narrow copper plate;
[0033] At least two first cooling water grooves are provided, and the at least two first cooling water grooves are respectively provided on a side away from the transverse center line of the narrow copper plate of at least two rows of fastening holes;
[0034] At least two second cooling water tanks are provided, and the at least two second cooling water tanks are respectively provided on one side of at least two rows of fastening holes close to the transverse center line of the narrow copper plate;
[0035] A plurality of third cooling water grooves are provided, and the plurality of third cooling water grooves are provided between two adjacent rows of fastening holes and are located on a side of the second cooling water groove close to the transverse center line of the narrow copper plate;
[0036] Among them, at least two second cooling water tanks and a plurality of third cooling water tanks are arranged at equal intervals from each other.
[0037] Optionally, a plurality of thermocouple assembly holes are provided on the cooling surface of the narrow copper plate.
[0038] Optionally, the first cooling water trough and the second cooling water trough of the narrow copper plate are inclined water troughs, and the first cooling water trough and the second cooling water trough are inclined in a direction away from a transverse center line of the narrow copper plate.
[0039] Optionally, the angle between the first cooling water groove of the narrow copper plate and the cooling surface is A, 70°≤A≤80°;
[0040] The angle between the second cooling water trough of the narrow copper plate and the cooling surface is B, 80°≤B≤89°;
[0041] Among them, B>A.
[0042] Optionally, the bottoms of the plurality of third cooling water troughs are located on the same curved surface, and the convex arc of the cross section of the curved surface where the bottoms of the plurality of third cooling water troughs are located is parallel to the convex arc of the cross section of the working surface.
[0043] Optionally, the distance between the transverse center line of the bottom of the third cooling water tank and the cooling surface complies with the formula:
[0044]
[0045] Wherein, h0 is the initial thickness of the top surface of the narrow copper plate; h1 is the maximum use thickness of the working surface of the narrow copper plate, which is 10~20mm; h2 is the safe distance between the bottom of the water tank and the working surface under the maximum use thickness, which is 9~13mm;
[0046] Among them, the distance between the transverse center line of the bottom of the first cooling water trough and the second cooling water trough and the cooling surface is greater than the distance between the transverse center line of the bottom of the third cooling water trough and the cooling surface by 1-3 mm.
[0047] Another aspect of the present application provides a crystallizer design method for designing any one of the above crystallizers, the method comprising:
[0048] Step 1: Obtain high temperature thermal / mechanical properties of steel and thermal properties of the mold copper plate and cooling water;
[0049] Step 2: Using the direct fluid-solid coupling algorithm, calculate the solidification shrinkage of the corner of the ingot with a planar narrow surface in the direction toward the center of the wide surface in the crystallizer;
[0050] Step 3: Based on the distribution of the solidification shrinkage from the corner of the ingot with a planar narrow surface to the center of the wide surface of the crystallizer in the height direction of the crystallizer, determine the expression for the taper compensation value of the copper plate on the narrow surface of the crystallizer;
[0051] Step 4: Replace the narrow copper plate of the crystallizer with a planar working surface in step 1 with a narrow copper plate of the crystallizer with a curved working surface, and repeat step 2;
[0052] Step 5: Draw a temperature cloud diagram of the narrow copper plate of the crystallizer with a curved working surface to determine whether the designed crystallizer meets the requirements.
[0053] Beneficial effects:
[0054] An embodiment of the present invention provides a crystallizer and a design method thereof, wherein the crystallizer provides a protrusion on the working surface of a narrow copper plate to transition continuously and smoothly from the middle to the edge, thereby avoiding the need to set an additional transition zone between the middle protrusion of the working surface and the nearly straight area of the edge to occupy the width of the middle protrusion, and solving the problem that the additional introduction of the transition zone results in the lateral span of the middle protrusion being too small, thereby failing to effectively reduce the width of the edge cracks of the ingot during the rolling process and causing a double-strand shape defect at the edge. At the same time, it also avoids the problem of leakage of the solidified billet shell caused by no smooth transition zone between the convexity in the middle of the working surface and the straight area on the edge, ensuring that the crystallizer can prepare high-quality ingots with narrow faces, large arcs, large inner concavities, and nearly right-angle structures at the corners, significantly reducing the width of wide edge line cracks in wide and thick plate rolling, and ensuring that the ingots are over-straightened at high temperatures at the corners in the secondary cooling zone to prevent the generation of cracks at the corners of the ingots; in addition, by introducing an adjustment factor into the horizontal middle convex surface span of the working surface of the narrow copper plate, the adjustment of the middle convex span and the width of the nearly straight area on the edge with the downward solidification shrinkage characteristics of the ingot is achieved, ensuring that the concave surface of the narrow surface of the ingot is highly fitted with the narrow copper plate in the horizontal direction during the solidification process, while the ingots are efficiently and evenly solidified. , reducing the wear on both sides of the raised arc surface in the middle of the copper plate, and improving the service life of the crystallizer; at the same time, the working surface of the narrow copper plate introduces a curved surface taper compensation structure along the height direction that caters to the solidification shrinkage characteristics of the billet shell, which meets the characteristics of dynamic solidification of the ingot in the height direction, ensuring that the narrow surface of the ingot fits well with the copper plate during the entire solidification process, so that the heat transfer between the two is uniform; on this basis, the nearly straight area of the edge of the working surface of the narrow copper plate introduces a correction value of the taper compensation amount that takes into account wear, and the taper compensation value of the nearly straight area of the edge at a height below the maximum value of the taper compensation amount of the top surface gradually decreases, which solves the problem of severe wear of the edge in the middle and lower area of the crystallizer in the actual continuous casting process, and further ensures the long service life of the crystallizer. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a schematic structural diagram of a crystallizer of an optional embodiment of the present application;
[0056] Figure 2 This is a schematic structural diagram of a narrow copper plate of an optional embodiment of the present application;
[0057] Figure 3 A topographical diagram of a working surface of a narrow copper plate of an optional embodiment of the present application without considering B1;
[0058] Figure 4 This is a contour line diagram of a working surface at a height of 312 mm from the top surface of the narrow copper plate and at the lower mouth of the crystallizer of an optional embodiment of the present application;
[0059] Figure 5 This is a schematic structural diagram of a cooling surface of an optional embodiment of the present application;
[0060] Figure 6 A transverse cross-sectional view of a narrow copper plate of an optional embodiment of the present application;
[0061] Figure 7 This is a schematic structural diagram of a cooling water tank in an optional embodiment of the present application;
[0062] Figure 8 A flow chart of a crystallizer design method according to an optional embodiment of the present application;
[0063] Fig. 9 This is a flow chart of a crystallizer design method according to another optional embodiment of the present application.
[0064] The reference numerals are:
[0065] 100, wide copper plate; 200, narrow copper plate; 300, casting billet;
[0066] 1. Top surface; 2. Bottom surface; 3. Side surface; 4. Working surface; 5. Cooling surface; 6. Horizontal center line of narrow copper plate; 7. Fastening hole; 8. First cooling water trough; 9. Second cooling water trough; 10. Third cooling water trough; 11. Horizontal center line of cooling water trough bottom; 12. Thermocouple assembly hole. DETAILED DESCRIPTION
[0067] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0068] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0069] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0070] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0071] See also Figures 1 to 7 As shown, according to one aspect of an embodiment of the present application, a crystallizer is provided, comprising two relatively wide copper plates 100 and two relatively narrow copper plates 200, wherein a crystallizer inner cavity is formed between the two relatively wide copper plates 100 and the two relatively narrow copper plates 200 for solidifying molten steel into a casting 300; the narrow copper plate 200 comprises a top surface 1, a bottom surface 2 and a working surface 4, wherein the working surface 4 is connected to the casting 300, and the working surface 4 protrudes toward the direction of the crystallizer inner cavity;
[0072] Working surface 4 is a curved surface, and the curved surface conforms to the formula:
[0073] (1)
[0074] Wherein, B1 is the taper compensation value of the working surface 4 at each height from the top surface 1 to the bottom surface 2 of the narrow copper plate 200; D1 is the lateral morphology of the working surface 4 at each height from the top surface 1 in the width direction of the narrow copper plate 200;
[0075] In the width direction of the narrow copper plate 200, the lateral shape D1 of the working surface 4 at each height from the top surface 1 conforms to the formula:
[0076] (2)
[0077] In the formula, x is the horizontal distance from the transverse center line 6 of the narrow copper plate; B2 is the raised height of the working surface 4 at the height of the top surface 1 of the narrow copper plate 200, and the value range is 10~18mm; B3 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface 4 of the narrow copper plate 200; B4 is the correction value of the taper compensation amount.
[0078] The taper compensation value B1 of the working surface 4 of the narrow copper plate 200 from the top surface 1 to the bottom surface 2 conforms to the formula:
[0079] (3)
[0080] In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface 1 of the narrow copper plate 200;
[0081] The adjustment factor B3 of the transverse span of the middle raised area in the width direction of the working surface 4 of the narrow copper plate 200 conforms to the formula:
[0082] (4)
[0083] Where l1 is the height of the crystallizer;
[0084] The taper compensation correction value B4 conforms to the formula:
[0085] (5)
[0086] Wherein, l2 is the width of the top surface 1 of the narrow copper plate 200; y0 is the y value when B1 takes the maximum value.
[0087] Among them, the crystallizer provided in the embodiment of the present application can produce a narrow concave ingot 300 with a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner.
[0088] The crystallizer includes two wide copper plates 100 and two narrow copper plates 200. The two wide copper plates 100 are arranged in parallel and opposite to each other, and the two narrow copper plates 200 are also arranged in parallel and opposite to each other.
[0089] For details, see Figure 1 As shown, two wide copper plates 100 and two narrow copper plates 200 are combined to form a crystallizer cavity, which is used to solidify molten steel into a billet shell, and to continuously cast a narrow concave billet 300 with a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner. It can be understood that the transverse direction of the narrow copper plate 200 is the width direction of the narrow copper plate 200, and the width direction of the narrow copper plate 200 is the thickness direction of the billet 300, that is, the transverse direction of the narrow copper plate 200 is the thickness direction of the billet 300.
[0090] The wide copper plate 100 may be a flat copper plate, and the narrow copper plate 200 may be a convex curved copper plate.
[0091] The narrow copper plate 200 includes a top surface 1 and a bottom surface 2. The top surface 1 of the narrow copper plate 200 is flush with the upper opening of the crystallizer, and the bottom surface 2 of the narrow copper plate 200 is flush with the lower opening of the crystallizer. It can be understood that the upper opening of the crystallizer can be the end where the molten steel enters the inner cavity of the crystallizer, and the lower opening of the crystallizer can be the end where the cast billet leaves the inner cavity of the crystallizer.
[0092] The narrow copper plate 200 further includes a working surface 4 , which may be a wall surface of the narrow copper plate 200 facing the inner cavity of the crystallizer, that is, the working surface 4 is a wall surface of the narrow copper plate 200 in contact with the solidified ingot 300 .
[0093] Specifically, the working surface 4 is convex toward the inner cavity of the crystallizer, and the working surface 4 is a convex curved surface. The expression of the convex curved surface conforms to formula (1).
[0094] Among them, the working surface 4 includes a middle portion and two side portions, the two side portions are relatively arranged along the width direction of the narrow copper plate 200, one side portion is arranged on one side of the middle portion, and the other side portion is arranged on the other side of the middle portion. In the embodiment of the present application, the middle portion and the two side portions are integrally formed. It should be noted that the middle portion can also be used to characterize the area on the narrow copper plate 200 close to the transverse center line 6 of the narrow copper plate, that is, the middle portion can also be used to characterize the middle of the narrow copper plate 200; the side portion can be used to characterize the area on the narrow copper plate 200 away from the transverse center line 6 of the narrow copper plate, that is, the side portion can also be used to characterize the side of the narrow copper plate 200.
[0095] Specifically, the middle part can be a raised area, and the side part can be a nearly straight area. It can be understood that the middle part is a raised area toward the inner cavity of the crystallizer, and the side part changes more smoothly than the middle part, so that the crystallizer can prepare a casting 300 with a corner having a nearly right-angle structure. The corner of the casting 300 can be a casting 300 corresponding to the angle at the intersection of the wide copper plate 100 and the narrow copper plate 200. In the embodiment of the present application, the angle at the intersection of the wide copper plate 100 and the narrow copper plate 200 is close to a right angle. It should be noted that the working surface 4 conforms to formula (1), which can realize a smooth and continuous transition between the middle part and the two side sides, and can also realize that in the height and width direction of the narrow copper plate 200, the height and span of the raised part in the middle, and the height and width of the nearly straight area of the side are all continuous curved surface changes.
[0096] Among them, in the embodiment of the present application, in the height direction of the narrow copper plate 200, the span of the middle raised area of the working surface 4 gradually decreases from the top surface 1 to the bottom surface 2, that is, the lateral span of the middle raised area gradually decreases from the top surface 1 to the bottom surface 2.
[0097] Among them, in the embodiment of the present application, in the height direction of the narrow copper plate 200, the height of the middle protrusion of the working surface 4 first increases and then decreases, and the projection of the transverse center line 6 of the narrow copper plate on the working surface 4 is similar in shape to the transverse center line 11 of the bottom of the cooling water tank, that is, the projection of the transverse center line 6 of the narrow copper plate on the working surface 4 has a similar bending trend and undulating characteristics to the transverse center line 11 of the bottom of the cooling water tank. The shape of the transverse center line 11 of the bottom of the cooling water tank can be seen in FIG. Figure 7It should be noted that the convex height of the middle and upper area of the working surface 4 is greater than the convex height of the middle and lower area of the working surface 4 , and the middle and upper area of the working surface 4 may be an area more than 312 mm away from the top surface 1 of the narrow copper plate 200 .
[0098] The crystallizer provided in the embodiment of the present application, by setting the projection of the working surface 4 on the narrow copper plate 200 to transition continuously and smoothly from the middle to the edge, avoids the need to set an additional transition zone for the transition between the middle and the edge of the working surface 4, reduces the width of the middle occupied by the straight area of the edge, and thus solves the problem that the width of the edge crack of the ingot 300 during the rolling process cannot be effectively reduced due to the additional introduction of the transition zone, and the significant double-strand shape defect caused thereby, and can also avoid the problem of leakage of the solidified ingot shell if a smooth transition zone is not introduced between the middle and the edge of the working surface 4, and ensures that the crystallizer can prepare the ingot 300 with a narrow face, a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner with high quality, thereby significantly reducing the width of the wide edge crack of the wide and thick plate rolling, and ensuring that the ingot 300 is straightened at high temperature at the corner in the second cooling zone, to prevent the generation of cracks at the corner of the ingot 300; At the same time, an adjustment factor is introduced into the transverse span of the middle raised area in the width direction of the working surface 4 of the narrow copper plate 200, so as to realize the adjustment of the middle raised span and the width of the nearly straight area at the edge along with the downward solidification shrinkage characteristics of the ingot 300, thereby ensuring that the inner concave surface of the ingot 300 is highly fitted and solidified with the narrow copper plate 200 in the transverse direction during the entire solidification process. While the ingot 300 is efficiently and uniformly solidified, the wear on both sides of the raised arc surface in the middle of the copper plate is reduced, thereby improving the service life of the crystallizer; at the same time, the working surface 4 of the narrow copper plate 200 has a curved taper compensation structure along its height direction to cater to the solidification shrinkage characteristics of the ingot shell, which meets the characteristics of the dynamic solidification of the ingot 300 in the height direction, ensuring that the narrow surface of the ingot 300 is well fitted with the copper plate during the entire solidification process, so that the heat transfer between the two is uniform; in addition, a compensation correction value considering wear is introduced into the nearly straight area at the edge of the working surface 4 of the narrow copper plate 200, see Figure 4 As shown, the taper compensation value of the nearly straight area of the edge below 312 mm from the top surface 1 gradually decreases, solving the problem of severe wear of the edge in the lower area of the crystallizer in the actual continuous casting process.
[0099] In some possible embodiments provided in the present application, the side of the narrow copper plate 200 facing away from the ingot 300 is a cooling surface 5, and the cooling surface 5 is provided with fastening holes 7, a first cooling water trough 8, a second cooling water trough 9 and a third cooling water trough 10; the fastening holes 7 are arranged in at least two rows, and at least two rows of fastening holes 7 are symmetrically arranged along the transverse center line 6 of the narrow copper plate; at least two first cooling water troughs 8 are arranged, and at least two first cooling water troughs 8 are respectively arranged on the side of at least two rows of fastening holes 7 away from the transverse center line 6 of the narrow copper plate; at least two second cooling water troughs 9 are arranged, and at least two second cooling water troughs 9 are respectively arranged on the side of at least two rows of fastening holes 7 close to the transverse center line 6 of the narrow copper plate; a plurality of third cooling water troughs 10 are arranged, and a plurality of third cooling water troughs 10 are arranged between two adjacent rows of fastening holes 7, and are located on the side of the second cooling water trough 9 close to the transverse center line 6 of the narrow copper plate; at least two second cooling water troughs 9 and a plurality of third cooling water troughs 10 are arranged at equal intervals from each other.
[0100] The cooling surface 5 may be a wall surface of the narrow copper plate 200 away from the ingot 300 , and the cooling surface 5 is arranged opposite to the working surface 4 .
[0101] Among them, fastening holes 7 and cooling water troughs are opened on the cooling surface 5. The fastening holes 7 are bolt holes used to fix the narrow copper plate 200 and the cooling water tank; the cooling water trough extends along the height direction of the narrow copper plate 200, and the cooling water trough is used to cool the narrow copper plate 200, and then cool the ingot 300 in the inner cavity of the crystallizer.
[0102] Specifically, in the width direction of the narrow copper plate 200, the fastening holes 7 can be arranged in two to four rows, and the cooling water grooves can be arranged in multiple rows. It should be noted that when the fastening holes 7 are arranged in two rows, the distance between the fastening holes 7 and the adjacent cooling water grooves can be 3 to 6 mm; when the fastening holes 7 are arranged in more than two rows, the distance between the fastening holes 7 and the adjacent cooling water grooves can be 2 to 5 mm.
[0103] The widths of the plurality of cooling water grooves are the same, and the width of the cooling water grooves may be 4-7 mm.
[0104] Among them, the heights of the multiple cooling water troughs are the same, and the distance between the cooling water trough and the top surface 1 of the narrow copper plate 200 can be 20-25 mm, and the distance between the cooling water trough and the bottom surface 2 of the narrow copper plate 200 can also be 20-25 mm.
[0105] Among them, the multiple cooling water grooves are symmetrically arranged with the transverse center line 6 of the narrow copper plate as the symmetry center, and the multiple cooling water grooves include at least two first cooling water grooves 8, at least two second cooling water grooves 9 and several third cooling water grooves 10.
[0106] Specifically, in the embodiment of the present application, the fastening holes 7 are arranged in two rows, the first cooling water grooves 8 are arranged in two rows, the second cooling water grooves 9 are arranged in two rows, and the third cooling water grooves 10 are arranged in eight rows. The two first cooling water grooves 8 are respectively arranged on the side of the two rows of fastening holes 7 away from the transverse center line 6 of the narrow copper plate, the two second cooling water grooves 9 are respectively arranged on the side of the two rows of fastening holes 7 close to the transverse center line 6 of the narrow copper plate, and the eight third cooling water grooves 10 are all arranged between the two second cooling water grooves 9.
[0107] Specifically, the narrow copper plate 200 further includes two side surfaces 3, the two side surfaces 3 are planes, and the two side surfaces 3 are symmetrically arranged with the narrow copper plate transverse center line 6 as the symmetry center. Starting from the narrow copper plate transverse center line 6 in the direction toward the side surface 3, a plurality of cooling water troughs are numbered W6, W5, W4, W3, W2 and W1 in sequence, W6, W5, W4 and W3 are all third cooling water troughs 10, W2 is the second cooling water trough 9, and W1 is the first cooling water trough 8.
[0108] The cooling water grooves between the two rows of fastening holes 7 are spaced at the same distance from each other, that is, W2, W3, W4, W5, W6, W6, W5, W4, W3 and W2 are spaced at the same distance from each other in the width direction of the narrow copper plate 200, and the spacing range is 10-20 mm. By setting the cooling water grooves between the two fastening holes 7 to have the same spacing, uniform cooling of the ingot 300 in the inner cavity of the crystallizer can be achieved.
[0109] In the above embodiment, a plurality of thermocouple assembly holes 12 are also provided on the cooling surface 5 .
[0110] By providing the thermocouple assembly hole 12 on the cooling surface 5 , a stable installation position is provided for the thermocouple, so that the temperature monitoring of the narrow copper plate 200 can be realized.
[0111] The thermocouple assembly hole 12 may be a circular hole, and the diameter of the thermocouple assembly hole 12 may be 5-6 mm.
[0112] Among them, several thermocouple assembly holes 12 are arranged perpendicular to the cooling surface 5, and the distance between several thermocouple assembly holes 12 and the working surface 4 of the narrow copper plate 200 is the same. The distance between several thermocouple assembly holes 12 and the working surface 4 of the narrow copper plate 200 at the original thickness can be 20~26mm.
[0113] Specifically, a plurality of thermocouple assembly holes 12 may be arranged in 2 to 4 rows in the height direction of the narrow copper plate 200, and a plurality of thermocouple assembly holes 12 may be arranged in 1 to 2 columns in the width direction of the narrow copper plate 200. In the height direction of the narrow copper plate 200, the distance between the first row of thermocouple assembly holes 12 and the top surface 1 of the narrow copper plate 200 may be 200 to 240 mm, and the spacing between two adjacent rows of thermocouple assembly holes 12 may be 100 to 150 mm, and the spacing may be the same or different, and the present application does not make further limitations. For example, when a plurality of thermocouple assembly holes 12 are arranged in a row in the width direction of the narrow copper plate 200, each of the thermocouple assembly holes 12 coincides with the transverse center line 6 of the narrow copper plate; when a plurality of thermocouple assembly holes 12 are arranged in two rows in the width direction of the narrow copper plate 200, the two rows of thermocouple assembly holes 12 are symmetrically arranged with the transverse center line 6 of the narrow copper plate as the symmetry center. At this time, the spacing between the two rows of thermocouple assembly holes 12 and the transverse center line 6 of the narrow copper plate can be 13% to 23% of the width of the top surface 1 of the narrow copper plate 200.
[0114] In the above embodiment, the first cooling water trough 8 and the second cooling water trough 9 are inclined troughs, and the first cooling water trough 8 and the second cooling water trough 9 are inclined in a direction away from the transverse center line 6 of the narrow copper plate.
[0115] By setting the first cooling water trough 8 and the second cooling water trough 9 as inclined troughs and tilting the first cooling water trough 8 and the second cooling water trough 9 in a direction away from the transverse center line 6 of the narrow copper plate, uniform heat transfer of the narrow copper plate 200 in the width direction can be ensured to achieve uniform cooling of the cast billet 300 in the inner cavity of the crystallizer.
[0116] Among them, the first cooling water trough 8 and the second cooling water trough 9 are inclined water troughs, and the first cooling water trough 8 and the second cooling water trough 9 are set at an angle to the cooling surface 5; the third cooling water trough 10 is a straight water trough, and the third cooling water trough 10 is perpendicular to the cooling surface 5.
[0117] Specifically, the first cooling water trough 8 is inclined in a direction away from the transverse center line 6 of the narrow copper plate, and the first cooling water trough 8 is used to cool the edge of the working surface 4; the second cooling water trough 9 is inclined in a direction away from the transverse center line 6 of the narrow copper plate, and the second cooling water trough 9 is used to cool the area corresponding to the projection of the fastening hole 7 on the working surface 4.
[0118] In the above embodiment, the angle between the first cooling water trough 8 and the cooling surface 5 is A, 70°≤A≤80°; the angle between the second cooling water trough 9 and the cooling surface 5 is B, 80°≤B≤89°; wherein B>A.
[0119] By setting the angle between the first cooling water trough 8 and the cooling surface 5 to be greater than the angle between the second cooling water trough 9 and the cooling surface 5, it is possible to ensure uniform lateral temperature distribution on the working surface 4, ensure high-temperature over-straightening of the corners of the ingot 300 in the second cooling zone, and prevent the occurrence of cracks at the corners of the ingot 300.
[0120] In the above embodiment, the bottoms of several third cooling water troughs 10 are located on the same curved surface; at the same height, the convex arc of the cross section of the curved surface where the bottoms of several third cooling water troughs 10 are located is parallel to the convex arc of the cross section of the working surface 4.
[0121] By arranging a plurality of third cooling water troughs 10 whose bottoms are located so that the convex arc of the cross section is parallel to the convex arc of the cross section of the working surface 4, it is possible to ensure uniform heat transfer in the middle of the working surface 4 in the width direction of the narrow copper plate 200, so as to achieve uniform cooling of the ingot 300 in the inner cavity of the crystallizer.
[0122] The curved surfaces where the bottoms of the third cooling water tanks 10 are located may conform to formula (1).
[0123] Specifically, at the same height, the convex arc of the cross section of the curved surface where the bottoms of the third cooling water grooves 10 are located can be obtained by translating the convex arc of the cross section of the middle part of the working surface 4 .
[0124] In the above embodiment, the distance between the transverse center line of the bottom of the third cooling water tank 10 and the cooling surface 5 conforms to the formula:
[0125] (6)
[0126] In the formula, h0 is the initial thickness of the top surface 1 of the narrow copper plate 200; h1 is the maximum use thickness of the working surface side of the narrow copper plate 200, which is 10~20mm; h2 is the safe distance between the bottom of the cooling water trough and the working surface 4 under the maximum use thickness, which is 9~13mm; wherein, the distance between the bottom of the first cooling water trough 8 and the second cooling water trough 9 and the cooling surface 5 is greater than the distance between the bottom of the third cooling water trough 10 and the cooling surface 5 by 1~3mm. It should be noted that, since the fastening hole 7 is provided between the first cooling water trough 8 and the second cooling water trough 9, the distance between the first cooling water trough 8 and the second cooling water trough 9 is greater than the distance between two adjacent third cooling water troughs 10. If the distances between the bottom of the first cooling water trough 8, the bottom of the second cooling water trough 9 and the bottom of the third cooling water trough 10 and the working surface 4 are the same, the temperature at the position on the working surface 4 relative to the first cooling water trough 8 and the second cooling water trough 9 will be higher than the temperature at the position on the working surface 4 relative to the third cooling water trough 10. In the embodiment of the present application, by setting the distance between the transverse center line of the bottom of the first cooling water trough 8 and the second cooling water trough 9 and the cooling surface 5 to be greater than the distance between the transverse center line of the bottom of the third cooling water trough 10 and the cooling surface 5 by 1~3mm, so that the bottom of the first cooling water trough 8 and the second cooling water trough 9 is closer to the working surface 4 than the bottom of the third cooling water trough 10, it can be ensured that the temperature of each area of the working surface 4 is consistent, so as to achieve uniform cooling of the cast billet 300 in the inner cavity of the crystallizer.
[0127] By setting the distance between the bottom of the third cooling water trough 10 and the cooling surface 5 to conform to the formula (6), the depth of the third cooling water trough 10 changes in a curve in the height direction of the narrow copper plate 200.
[0128] The structure of the narrow copper plate 200 is further described below in conjunction with specific values and drawings.
[0129] Among them, see Figure 1 As shown, the crystallizer is composed of two flat wide copper plates 100 and two convex narrow copper plates 200, and is used to produce narrow concave ingots 300 with a cross-sectional size of 250 mm×1800 mm.
[0130] Among them, see Figure 2 As shown, the height l1 of the narrow copper plate 200 is 900 mm, and the narrow copper plate 200 is a structure that is wide at the top and narrow at the bottom, with the transverse center line 6 of the narrow copper plate as the symmetry center.
[0131] Specifically, in the height direction of the crystallizer, the width of the narrow copper plate 200 decreases linearly by 1 to 3 mm from the top surface 1 to the bottom surface 2. It should be noted that during the actual slab continuous casting process, the ingot 300 solidifies in the crystallizer, and the thickness direction of the ingot 300 shrinks by 1 to 3 mm. In the present application, by setting the width of the narrow copper plate 200 to decrease linearly by 1 to 3 mm from the top surface 1 to the bottom surface 2, it is possible to prevent the ingot 300 from detaching from the wide copper plate 100 due to shrinkage in the thickness direction during the downward solidification process.
[0132] In the above embodiment, the width of the narrow copper plate 200 decreases linearly by 2 mm from the top surface 1 to the bottom surface 2, the width l2 of the top surface 1 is 266 mm, and the width of the bottom surface 2 is 264 mm.
[0133] In the above embodiment, the protrusion height B2 of the working surface 4 at the height of the top surface 1 of the narrow copper plate 200 is 14 mm.
[0134] Among them, in the above embodiment, the transverse middle raised area of the working surface 4 is the middle of the working surface 4, and the nearly straight areas on both sides of the middle are the edges of the working surface 4. In the height and width directions of the narrow copper plate 200, the raised height and span of the middle part, and the raised height and width of the edge part all show continuous curved surface changes, and the middle part and the two side edges have an integrated smooth and continuous transition.
[0135] Among them, in the height direction of the narrow copper plate 200, the taper compensation value of the working surface 4 is determined according to the following method: first, the shrinkage of the corner of the ingot 300 along the width direction is calculated, and then the curve expression of the taper compensation value of the height below the meniscus of the narrow copper plate 200 is obtained by fitting a seventh-order polynomial, with the meniscus as the coordinate origin, the height of the narrow copper plate 200 and the compensation value as the horizontal and vertical coordinates respectively. On this basis, the fitted expression curve is further rotated clockwise with the bottom surface 2 of the narrow copper plate 200 as the origin until the curve at the top surface 1 of the narrow copper plate 200 intersects with the horizontal axis, and the origin of the coordinate system is translated to the intersection, thereby obtaining the taper compensation value expression (3) of the working surface 4 of the narrow copper plate 200 from the top surface 1 to the bottom surface 2.
[0136] Among them, in the above embodiment, the steel type produced is AH36 steel, and its meniscus is located at a height of 100mm below the top surface 1 of the narrow copper plate 200. The shrinkage of the corner of the ingot 300 along the width direction in the meniscus and in each height direction below it is calculated, and then the seventh-order polynomial fitting coefficients shown in formula (3) are obtained by rotating the expression curve and translating the coordinate system: A0=0; A1=0.01677; A2=-2.805E-05; A3=-4.687E-08; A4=2.114E-10; A5=-3.114E-13; A5=2.206E-16; A6=-6.320E-20. That is, the expression of formula (3) is:
[0137] B1=0.01677y-2.805E-05y 2 -4.687E-08y 3 +2.114E-10y 4 -3.114E-13y 5 +2.206E-16y 6 -6.320E-20y 7 (7)
[0138] According to formula (7), the maximum value of the taper compensation of the working surface 4 in the height direction is 2.35 mm, which is located 312 mm below the top surface 1 of the narrow copper plate 200, that is, y0 is 312 mm. The taper compensation values of the working surface 4 at different heights of the narrow copper plate 200 are determined, as shown in Table 1.
[0139] Table 1
[0140]
[0141] Furthermore, in the above embodiment, according to the convex height of 14 mm of the working surface 4 at the height of the top surface 1 of the narrow copper plate 200 and the edge wear degree of the working surface 4 of the narrow copper plate 200, the lateral morphology of the working surface 4 of the narrow copper plate 200 is designed to be the curve shown in formula (8). Wherein, the expressions of B3 and B4 are shown in formulas (9) and (10).
[0142] (8)
[0143] Wherein, 14 is the protrusion height of the working surface 4 at the height where the top surface 1 of the narrow copper plate 200 is located.
[0144] (9)
[0145] (10)
[0146] The taper compensation value of the working surface 4 along the height direction of the narrow copper plate 200 and the lateral morphology along the width direction of the narrow copper plate 200 are combined to determine the surface expression (8) of the narrow copper plate 200 in the embodiment of the present application with the working surface 4 of the edge of the top surface 1 as the reference. Its morphology is as follows: Figure 3 As shown. As can be seen from Figure 3, due to the introduction of the span adjustment factor on the raised surface in the middle of the working surface 4, the raised span in the middle and the width of the nearly straight area on the edge gradually decrease toward the transverse center line 6 of the narrow copper plate as the ingot 300 solidifies and shrinks downward, ensuring that the concave surface of the ingot 300 is highly fitted and evenly solidified with the narrow copper plate 200 in the width direction throughout the solidification process, avoiding the phenomenon of the ingot 300 shrinking and locking onto the raised surface or detaching from the raised surface, and ensuring the long service life of the crystallizer. At the same time, in the embodiment of the present application, since the compensation correction value considering wear is introduced into the nearly straight area on the edge of the narrow copper plate 200, the taper compensation value of the nearly straight area on the edge at a height of 312 mm below the top surface 1 gradually decreases, as shown in FIG. Figure 4 As shown. In the embodiment of the present application, the edge thickness of the narrow copper plate 200 is thinned by about 0.85mm from a height of 312mm below the top surface 1 to the bottom surface 2 compared to the straight area of the edge. In the embodiment of the present application, the two side surfaces 3, the top surface 1 and the bottom surface 2 of the narrow copper plate 200 are all planar structures. Among them, the initial thickness h0 of the edge of the top surface 1 of the narrow copper plate 200 is 40mm, the top surface 1 is arranged parallel to the bottom surface 2, and the two side surfaces 3 are symmetrically arranged with the horizontal center line 6 of the narrow copper plate as the symmetry center. In the embodiment of the present application, see Figure 5 and Figure 6 As shown, the cooling surface 5 of the narrow copper plate 200 is designed with twelve cooling water grooves, two rows of fastening holes 7 fixedly and sealedly connected to the cooling water tank, and one row of thermocouple assembly holes 12.
[0147] Among them, multiple cooling water grooves are symmetrically arranged with the transverse center line 6 of the narrow copper plate as the symmetry center and are arranged parallel to the side 3. In the embodiment of the present application, multiple cooling water grooves are numbered W1 to W6 in sequence from the edge of the narrow copper plate 200 to the transverse center line 6 of the narrow copper plate. The transverse width of the multiple cooling water grooves is 6mm, and the grooves are opened from 25mm below the top surface 1 to 25mm above the bottom surface 2, that is, the height of the cooling water groove is 850mm.
[0148] Combination Figure 6The transverse morphology of the cooling water trough is further described. The cooling water troughs W1 and W2 on the two side surfaces 3 close to the narrow copper plate 200 are at angles of 78° and 88° to the cooling surface 5, respectively. The cooling water troughs W3, W4, W5 and W6 are all designed perpendicular to the cooling surface 5. The morphology of the curved surface where the bottom of the multiple cooling water troughs is located is consistent with the morphology of the working surface 4 in the height direction of the narrow copper plate 200. The distances of the transverse center lines 11 of the bottom of the multiple cooling water troughs relative to the transverse center line 6 of the narrow copper plate are 111.9mm, 83.2mm, 64.7mm, 46.2mm, 27.7mm, and 9.3mm, respectively. In terms of the grooving depth of the cooling water trough, the maximum use thickness h1 on the side of the working surface 4 of the narrow copper plate 200 in the embodiment of the present application is 15mm, and the safety distance h2 of the transverse center line of the bottom of the cooling water trough from the working surface 4 under the maximum use thickness is 10mm. Based on this, the distance between the transverse center line 11 of the bottom of each cooling water trough and the cooling surface 5 at each height can be determined by formula (6), that is, the depth of each cooling water trough can be determined by formula (6). Among them, the distance between the transverse center line 11 of the bottom of the W1 and W2 cooling water troughs located on both sides of the fastening hole 7 and the cooling surface 5 is increased by 1 mm on the basis of the distance determined by formula (6), as shown in Table 2.
[0149] Table 2
[0150]
[0151] Among them, the fastening holes 7 are arranged between the cooling water tanks W1 and W2, and eight fastening holes are designed with equal vertical spacing from the top surface 1 to the bottom surface 2. The diameter of the fastening hole 7 is 16 mm and the depth is 15 mm. It is used to pass through bolts with a specification of M16×1.5. In the height direction of the narrow copper plate 200, the distance between the center of the fastening hole 7 and the top surface 1 of the narrow copper plate 200 is 50 mm, 165 mm, 280 mm, 395 mm, 510 mm, 625 mm, 740 mm, and 855 mm from top to bottom respectively; the distance between the center of the fastening hole 7 and the horizontal center line 6 of the narrow copper plate is 98.5 mm.
[0152] Among them, the thermocouple assembly holes 12 are arranged on the horizontal center line of the copper plate, and there are two rows in total. The diameter of the thermocouple assembly holes 12 is 5 mm, and the distance between the bottom surface 2 of the thermocouple assembly holes 12 and the working surface 4 of the narrow copper plate 200 is 22 mm. The distances between the upper and lower rows of thermocouple assembly holes 12 and the top surface 1 of the narrow copper plate 200 are 210 mm and 325 mm respectively.
[0153] Another aspect of the present application embodiment is shown in Figure 8 and Fig. 9 As shown, a crystallizer design method is provided, which is used to design any one of the above crystallizers, and the method comprises:
[0154] Step 1: Use JMatPro software to calculate the high-temperature thermal / mechanical physical properties of AH36 steel; consult the standard manual to obtain the thermal physical properties of the crystallizer copper plate and cooling water, and finally import all physical property parameter relationship curves into the corresponding commercial software material database.
[0155] Specifically, referring to the actual AH36 steel composition shown in Table 3, the JMatPro software was used to calculate the thermal conductivity, density, elastic modulus, enthalpy, Poisson's ratio, yield limit, linear thermal expansion coefficient that change with temperature at high temperature, and the liquidus temperature of 1798.15K and the solidus temperature of 1738.15K. On this basis, the thermal conductivity, specific heat and density physical properties of the crystallizer copper plate and cooling water were obtained by consulting the standard tool manual as shown in Table 4. The relationship curves between the physical properties of each material and the temperature were respectively imported into the material database of the corresponding commercial software for calculation.
[0156] Table 3
[0157]
[0158] Table 4
[0159]
[0160] Step 2: Direct fluid-solid coupling algorithm is used to access ANSYS Fluent and MSC.Marc commercial software using the multi-physics coupling interface MPCCI, and the three-dimensional thermal / mechanical finite element analysis of the ingot-crystallizer system and the copper plate-cooling water thermal / flow analysis are coupled to calculate the dynamic solidification heat transfer and deformation shrinkage behavior of the traditional narrow plane ingot 300 in the crystallizer, as follows:
[0161] Step 201: According to the actual copper plate drawing and the actual taper of the narrow surface, a three-dimensional solid model of a crystallizer consisting of two wide-surface and two narrow-surface copper plates 200, a casting slab 300 and cooling water in a cooling water tank is created.
[0162] Specifically, according to the actual wide copper plate drawings, narrow copper plate drawings, and narrow surface taper process of the crystallizer, a three-dimensional solid model of the crystallizer consisting of two wide copper plates 100 and two narrow copper plates 200, a three-dimensional solid model of the ingot 300, and a three-dimensional solid model of cooling water in the copper plate cooling water tank are established. Among them, in the embodiment of the present application, the height of the wide copper plate 100 and the narrow copper plate 200 of the crystallizer are both 900mm, the thickness is both 40mm, the top surface 1 of the narrow copper plate 200 is 266mm wide, the bottom surface 2 is 264mm wide, and the narrow surface taper is 1.0%.
[0163] Step 202: Import the mold copper plate, the ingot 300 and the cooling water model into ICEM-CFD for meshing, and execute different meshing strategies, while defining the contact surface between the cooling water and the copper plate as a coupling surface.
[0164] Specifically, the three-dimensional solid models of the crystallizer copper plate, the ingot 300 and the cooling water are respectively imported into the meshing software ICEM CFD for hexahedral meshing. The mesh size of the crystallizer copper plate is 10 mm, and the mesh size of the ingot 300 is 2 mm; the outermost mesh of the cooling water in the water tank is further processed with super-dense processing, and the mesh size is set to 0.02 mm, and the surface in contact with the copper plate in the cooling water model is defined as a coupling surface during meshing.
[0165] Step 203: Import the meshed copper plate and the ingot 300 into MSC.Marc, use unit type 7 to perform thermal / structural analysis, and assign physical property parameters to the corresponding model.
[0166] Specifically, the meshed copper plate and ingot 300 models are imported into MSC.Marc software, and the mesh units of the model are set to unit type 7 for performing thermal / structural analysis, and the physical property parameters imported into the material database in step 1 are assigned to the copper plate and ingot 300 respectively.
[0167] Step 204: According to the actual production situation of a steel plant, the position of the meniscus of the crystallizer is set and the area below the meniscus is defined as the effective height, and the downward direction of the ingot 300 is defined as the ingot drawing direction.
[0168] Specifically, based on the actual continuous casting production crystallizer liquid level height of 800mm, the meniscus position in the embodiment of the present application is defined as a height of 100mm from the upper mouth of the crystallizer, and the height below the meniscus is set as the effective height of the crystallizer, and the downward direction of the ingot 300 is defined as the billet drawing direction.
[0169] Step 205: define the cooling water tank wall surface of the copper plate model as a coupling surface for coupling calculation with the copper plate-cooling water heat / flow model.
[0170] Specifically, in the MSC.Marc software, the cooling water tank wall of the copper plate model is defined as a coupling surface for coupling calculation with the copper plate-cooling water thermal / fluid model.
[0171] Step 206: Establish a heat flow model of the shell-crystallizer interface that takes into account the dynamic changes of the interface gap between the shell and the copper plate, the protective slag film and the air gap.
[0172] Specifically, a heat flow model of the shell-crystallizer interface is established, which takes into account the dynamic changes of the interface gap between the shell and the copper plate, the protective slag film and the air gap. The calculation of the interface heat flow is determined by solving the simultaneous equations of Eqs. (11) to (20).
[0173] (11)
[0174] Where q is the interface heat flux density; T shell is the surface temperature of the ingot 300, which is calculated by a three-dimensional thermal / mechanical finite element model of the ingot-crystallizer system; T mold is the hot surface temperature of the copper plate, which is also calculated by the three-dimensional thermal / mechanical finite element model of the ingot-crystallizer system; R is the comprehensive thermal resistance of the interface, which is determined by formula (12).
[0175] (12)
[0176] In the formula, h rad is the comprehensive radiation heat transfer coefficient, determined by formula (13); h cond is the comprehensive conduction heat transfer coefficient, which is determined by formula (14).
[0177] (13)
[0178] (14)
[0179] In the formula, σ SB is the Stefan-Boltzmann constant; is the emissivity of the solidified shell; is the emissivity of the copper plate of the crystallizer; T melt is the melting temperature of the protective slag; R int is the thermal resistance of the crystallizer-solid slag layer interface, determined by formula (15); d liq is the thickness of the liquid protective slag layer, determined by formula (16); d sol is the thickness of the solid protective slag layer, determined by formula (17); d air is the air gap thickness, determined by formula (18); k liq k is the thermal conductivity of liquid mold slag; sol k is the thermal conductivity of solid mold slag; air is the thermal conductivity of air.
[0180] (15)
[0181] (16)
[0182] (17)
[0183] (18)
[0184] d gap is the total thickness of the interface gap between the billet shell and the copper plate of the crystallizer. Based on the principle of equal heat flow through each heat transfer medium layer in the interface, according to the surface temperature Tshell The melting temperature of the mold slag T melt Relationship, the above formulas can be substituted into the following equation group to solve the interface heat flux q.
[0185] (19)
[0186] or
[0187] (20)
[0188] Among them, q melt is the heat flux density of the liquid protective slag layer; q sol is the heat flux density of the solid protective slag layer; q air is the heat flux density of the air gap layer; q int is the interface heat flux density between the solid protective slag and the copper plate of the crystallizer. The corresponding parameters in the above formulas are detailed in Table 5.
[0189] Table 5
[0190]
[0191] Step 207: Setting the initial temperature conditions of the copper plate and the casting slab 300.
[0192] Specifically, based on the actual continuous casting of AH36 steel on site and its casting temperature, the initial temperatures of the copper plates 100 and 200 are set to 395K, and the initial temperature of the ingot 300 is set to 1823.2K.
[0193] Step 208: According to step 216, dynamically set the heat transfer boundary conditions of the copper plate cooling water trough, the heat transfer boundary conditions between the ingot 300 and the copper plate determined by step 206, the downward displacement constraint of the ingot 300, the fixed constraint of the bolt hole, and the static pressure of the molten steel applied to the solidification front of the ingot 300.
[0194] Specifically, the temperature boundary conditions and mechanical boundary conditions of the copper plate and the ingot 300 are set. The heat transfer boundary conditions of the copper plate cooling water tank are dynamically set by the coupling interface based on the flow and heat transfer calculation results of the cooling water in step 216; the heat transfer boundary conditions between the ingot 300 and the copper plate are dynamically determined by the shell-crystallizer interface heat flow model in step 206; a downward displacement constraint equivalent to a pulling speed of 1.1 m / min is applied to the ingot 300, and a completely fixed displacement constraint is set for the fastening bolt holes on the back of the copper plate. The interaction force boundary between the ingot 300 and the copper plate is set using the "rigid body-deformable body" contact pair analysis setting. The molten steel static pressure boundary condition is applied to the solidification front of the ingot 300, and the value of the molten steel static pressure is determined by formula (21).
[0195] (twenty one)
[0196] Where P is the static pressure of molten steel, Pa; ρ s (T) is the density of the ingot 300 at temperature T; g is the acceleration due to gravity, which is 9.81 m / s²; h is the vertical height from the meniscus.
[0197] Step 209: Select a constitutive equation that reflects the high temperature deformation characteristics of the ingot 300.
[0198] Specifically, a constitutive equation reflecting the high temperature deformation characteristics of the ingot 300 unit is selected. In the embodiment of the present application, considering that creep, elastic deformation and plastic deformation occur simultaneously during the solidification process of the ingot 300, the equations shown in equations (22) to (25) are selected as the mechanical constitutive equations of the ingot 300.
[0199] (twenty two)
[0200] In the formula, is the equivalent strain rate; is the equivalent stress; t is the current time; C is the pre-exponential factor, given by formula (23); Q is the ratio of the viscoplastic deformation activation energy to the gas constant, which is 17160K in the embodiment of the present application. -1 ; n and m are the exponents of stress and time, respectively, given by equations (24) and (25).
[0201] (twenty three)
[0202] In the formula, w c is the mass fraction of carbon in AH36 steel, see Table 3.
[0203] (twenty four)
[0204] (25)
[0205] Step 210: Set the analysis type between the ingot 300 and the crystallizer to transient thermal / structural analysis.
[0206] Step 211: Determine the model calculation time and time step based on the actual production pulling speed and the effective height of the crystallizer.
[0207] Specifically, based on the actual pulling speed of 1.1 m / min of AH36 steel produced by a steel plant, the calculation time of the model is determined to be 43.64 s, and the time step is set to 0.01 s.
[0208] Step 212: Using the unit birth and death function, set the participation status of the ingot 300 unit in the transient thermal / structural calculation of the crystallizer copper plate.
[0209] Specifically, the unit life and death function of the Marc software is used to set whether the slab 300 unit participates in the transient thermal / structural calculation between it and the copper plate of the crystallizer according to whether the slab 300 unit is located in the effective height area below the meniscus of the crystallizer. If the slab 300 unit is located at or below the meniscus of the crystallizer, the transient thermal / structural calculation of the slab 300 and the copper plate of the crystallizer is performed; otherwise, the slab 300 unit is frozen so that it does not participate in the transient thermal / structural calculation of the two.
[0210] Step 213: Import the cooling water model mesh into Fluent, turn on the energy equation option and select the k-epsilon turbulence model.
[0211] Step 214: Set the physical parameters of the cooling water and the water tank wall, set the cooling water inlet velocity, initial temperature, initial temperature of the coupling surface, turbulent kinetic energy and turbulent dissipation rate.
[0212] Specifically, the physical properties of the cooling water and copper plate imported into the material database in step 1 are assigned to the cooling water and the water tank wall respectively, and the cooling water inlet velocity, cooling water temperature, initial contact temperature of the coupling surface, and turbulent kinetic energy are set to 7.5 m / s, 305 K, 305 K, and 0.3528 m 2 / s 2 and turbulent dissipation rate 1115.087 m 2 / s 3 .
[0213] Step 215: The thermal / mechanical model of the ingot-crystallizer copper plate and the thermal / flow model of the copper plate-cooling water are coupled through the MPCCI interface.
[0214] Specifically, the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system and the thermal / fluid coupling calculation model of the copper plate-cooling water system are connected to the coupling calculation interface MPCCI.
[0215] Step 216: The thermal / mechanical model of the ingot-crystallizer copper plate and the thermal / flow model of the copper plate-cooling water are coupled through the MPCCI interface to achieve a two-way exchange of heat flux density and temperature data to update the respective heat transfer boundary conditions.
[0216] Specifically, the heat flux density calculated by the thermal / fluid coupling calculation model of the copper plate-cooling water system is applied to the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system as the heat transfer boundary condition of the copper plate cooling surface 5. At the same time, the thermal / mechanical coupling finite element model of the ingot-crystallizer copper plate system returns the calculated temperature and heat flux density to the thermal / fluid coupling calculation model of the copper plate-cooling water system, and updates the heat transfer boundary condition of the cooling water in the thermal / fluid coupling calculation model of the copper plate-cooling water system.
[0217] Step 217: Set parallel computing.
[0218] Specifically, parallel calculation is set, and model calculation is executed until the calculation is completed, and the solidification shrinkage of the corners of the ingot 300 at various heights below the meniscus of the crystallizer along the wide surface direction is extracted.
[0219] Step 3: Using the result of step 217, determine the shrinkage of the ingot 300 at each height below the meniscus of the crystallizer through polynomial fitting, and then determine the curve expression B1 of the copper plate taper compensation value.
[0220] Specifically, according to step 217, the shrinkage of the corner of the ingot 300 at each height below the meniscus of the crystallizer is calculated along the width center direction, and the copper plate height and the compensation value are respectively the horizontal and vertical coordinates, and the meniscus height is taken as the origin of the coordinate system. The curve expression of the taper compensation value of the working surface 4 at the height below the meniscus of the copper plate is obtained by seventh-order polynomial fitting. On this basis, the curve at the height of the bottom surface 2 of the narrow copper plate 200 is further taken as the origin, and the curve is rotated clockwise until the curve at the top surface 1 of the copper plate intersects with the horizontal axis, and the origin of the coordinate system is translated to the intersection, and then the seventh-order polynomial fitting is performed according to the function of formula (3) to obtain the coefficients A i value, establish the B1 expression.
[0221] Step 4: According to the crystallizer proposed in the embodiment of the present application, a model is established and the copper plate with a flat working surface 4 in step 1 is replaced with a copper plate with a convex curved working surface 4, and the operation of step 2 is repeated.
[0222] Specifically, according to the crystallizer structure in the embodiment of the present application, a narrow copper plate 200 with a convex curved surface is designed, and the narrow copper plate 200 with a flat working surface 4 in step 1 is replaced with a narrow copper plate 200 with a convex curved surface as designed, and step 2 is repeated.
[0223] Step 5: Extract the temperature field of the narrow copper plate 200 and draw a temperature cloud map of the working surface 4 of the narrow copper plate 200 to determine whether the designed crystallizer meets the requirements.
[0224] Specifically, the temperature field of the narrow copper plate 200 is extracted and a temperature cloud map of the working surface 4 of the narrow copper plate 200 is drawn. If the overall temperature distribution or change of the narrow copper plate 200 is uniform, it is determined that the designed crystallizer meets the requirements and the crystallizer design is completed; otherwise, the spacing and size of the cooling water troughs, the spacing between the fastening holes 7 and the cooling water troughs, and the depth of the cooling water troughs on both sides of the fastening holes 7 are adjusted, and steps 2 to 4 are repeated until a crystallizer that satisfies uniform heat transfer and a curved working surface 4 of the narrow copper plate 200 is obtained.
[0225] An embodiment of the present invention provides a crystallizer and a design method thereof, wherein the crystallizer continuously and smoothly transitions from the middle to the edge by setting a protrusion on the working surface 4 on the narrow copper plate 200, thereby avoiding the problem that the middle width is occupied by setting an additional transition zone between the middle and the edge of the working surface 4, resulting in a small middle span, thereby failing to effectively reduce the problem of significant width edge line crack defects and significant double-strand shape defects formed in the billet 300 during the rolling process. It can also avoid the problem of liquid leakage of the solidified billet shell caused by the lack of a smooth transition zone between the middle and the edge of the working surface 4, so that the crystallizer can prepare the billet 300 with a narrow face, a large arc surface, a large inner concave amount, and a nearly right-angle structure at the corner with high quality, thereby significantly reducing the width of the wide edge line crack during the rolling of the wide and thick plate, and ensuring that the billet 300 is over-straightened at high temperature at the corner in the secondary cooling zone to prevent the billet 300 from cracking at the corner. The production of lines; at the same time, an adjustment factor is introduced into the span of the raised curved surface in the middle of the working surface 4 of the narrow copper plate 200, so that the span of the raised curved surface in the middle and the width of the nearly straight area at the edge can be adjusted along with the downward solidification shrinkage characteristics of the ingot 300, ensuring that the concave surface of the ingot 300 is highly fitted and solidified with the narrow copper plate 200 in the horizontal direction during the solidification process. While the ingot 300 is efficiently and uniformly solidified, the service life of the crystallizer is improved; in addition, the working surface 4 of the narrow copper plate 200 has a curved surface taper compensation structure along the height direction to cater to the solidification shrinkage characteristics of the ingot shell, which meets the characteristics of the dynamic solidification of the ingot 300 in the height direction, ensuring that the narrow surface of the ingot 300 is well fitted with the copper plate during the entire solidification process, so that the heat transfer between the two is uniform; at the same time, a compensation correction value considering wear is introduced into the nearly straight area at the edge of the working surface 4 on the narrow copper plate 200, see Figure 4 As shown, the taper compensation value of the nearly straight area of the edge below 312 mm from the top surface 1 gradually decreases, which solves the problem of severe wear of the edge in the lower area of the crystallizer in the actual continuous casting process.
[0226] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned advantageous methods can be freely combined and superimposed.
[0227] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application. The above are only preferred implementations of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present application, and these improvements and variations should also be regarded as the protection scope of the present application.
Claims
1. A crystallizer, characterized in that: It comprises two wide copper plates and two narrow copper plates which are arranged opposite to each other, and the two wide copper plates and the two narrow copper plates are combined to form a crystallizer cavity, which is used to solidify molten steel into a casting billet; the narrow copper plates comprise a top surface, a bottom surface and a working surface, and the working surface is convex toward the direction of the crystallizer cavity and contacts with the casting billet; Among them, the working surface is a curved surface, and the curved surface conforms to the formula: Wherein, B1 is the taper compensation value of the working surface at each height from the top surface to the bottom surface of the narrow copper plate; D1 is the lateral morphology of the working surface at each height from the top surface in the width direction of the narrow copper plate; Among them, in the width direction of the narrow copper plate, the lateral morphology D1 of the working surface at each height from the top surface conforms to the formula: Wherein, x is the horizontal distance from the transverse center line of the narrow copper plate; B2 is the raised height of the working surface at the height of the top surface of the narrow copper plate, and the value range is 10~18mm; B3 is the adjustment factor of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate; B4 is the correction value of the taper compensation; The taper compensation value B1 of the working surface of the narrow copper plate at each height from the top surface to the bottom surface conforms to the formula: In the formula, A i is the fitting coefficient of the seventh-order polynomial; y is the distance from the top surface of the narrow copper plate; The adjustment factor B3 of the transverse span of the middle raised area in the width direction of the working surface of the narrow copper plate conforms to the formula: Where l1 is the height of the crystallizer; The taper compensation correction value B4 conforms to the formula: Where l2 is the width of the top surface of the narrow copper plate; y0 is the y value when B1 takes the maximum value.
2. The crystallizer according to claim 1, characterized in that In the height direction of the crystallizer, the width of the narrow copper plate decreases linearly by 1 to 3 mm from the top surface to the bottom surface.
3. The crystallizer according to claim 1, characterized in that The side of the narrow copper plate facing away from the ingot is a cooling surface, and fastening holes, a first cooling water trough, a second cooling water trough and a third cooling water trough are provided on the cooling surface; At least two rows of fastening holes are provided, and at least two rows of fastening holes are symmetrically arranged along the transverse center line of the narrow copper plate; At least two first cooling water grooves are provided, and the at least two first cooling water grooves are respectively provided on a side away from the transverse center line of the narrow copper plate of at least two rows of fastening holes; At least two second cooling water tanks are provided, and the at least two second cooling water tanks are respectively provided on one side of at least two rows of fastening holes close to the transverse center line of the narrow copper plate; A plurality of third cooling water grooves are provided, and the plurality of third cooling water grooves are provided between two adjacent rows of fastening holes and are located on a side of the second cooling water groove close to the transverse center line of the narrow copper plate; Among them, at least two second cooling water tanks and a plurality of third cooling water tanks are arranged at equal intervals from each other.
4. The crystallizer according to claim 3, characterized in that A plurality of thermocouple assembly holes are also provided on the cooling surface of the narrow copper plate.
5. The crystallizer according to claim 3, characterized in that The first cooling water trough and the second cooling water trough of the narrow copper plate are inclined water troughs, and the first cooling water trough and the second cooling water trough are inclined in a direction away from the transverse center line of the narrow copper plate.
6. The crystallizer according to claim 5, characterized in that The angle between the first cooling water tank of the narrow copper plate and the cooling surface is A, 70°≤A≤80°; The angle between the second cooling water trough of the narrow copper plate and the cooling surface is B, 80°≤B≤89°; Among them, B>A.
7. The crystallizer according to claim 3, characterized in that The bottoms of the plurality of third cooling water grooves are located on the same curved surface, and the convex arc of the cross section of the curved surface where the bottoms of the plurality of third cooling water grooves are located is parallel to the convex arc of the cross section of the working surface.
8. The crystallizer according to claim 7, characterized in that The distance between the transverse centerline of the bottom of the third cooling water tank and the cooling surface conforms to the formula: Wherein, h0 is the initial thickness of the top surface of the narrow copper plate; h1 is the maximum use thickness of the working surface of the narrow copper plate, which is 10~20mm; h2 is the safe distance between the bottom of the water tank and the working surface under the maximum use thickness, which is 9~13mm; Among them, the distance between the transverse center line of the bottom of the first cooling water trough and the second cooling water trough and the cooling surface is greater than the distance between the transverse center line of the bottom of the third cooling water trough and the cooling surface by 1-3 mm.
9. A crystallizer design method, characterized in that: For designing a crystallizer according to any one of claims 1 to 8, the method comprises: Step 1: Obtain high temperature thermal / mechanical properties of steel and thermal properties of the mold copper plate and cooling water; Step 2: Using the direct fluid-solid coupling algorithm, calculate the solidification shrinkage of the corner of the ingot with a planar narrow surface in the direction toward the center of the wide surface in the crystallizer; Step 3: Based on the distribution of the solidification shrinkage from the corner of the ingot with a planar narrow surface to the center of the wide surface of the crystallizer in the height direction of the crystallizer, determine the expression for the taper compensation value of the copper plate on the narrow surface of the crystallizer; Step 4: Replace the narrow copper plate of the crystallizer with a planar working surface in step 1 with a narrow copper plate of the crystallizer with a curved working surface, and repeat step 2; Step 5: Draw a temperature cloud diagram of the narrow copper plate of the crystallizer with a curved working surface to determine whether the designed crystallizer meets the requirements.