A high wear-resistant flux-cored welding wire for drill pipe joints and its preparation method

By using high wear-resistant flux-cored wire on drill pipe joints, especially by adding elements such as Cr, Ti, and Nb to the flux core, the problem of severe wear on drill pipe joints has been solved, achieving high wear resistance and crack resistance, and extending service life.

CN118385814BActive Publication Date: 2026-11-17SHANGHAI UNIV OF ENG SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410468299.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2026-11-17
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

Existing drill pipe joints suffer from severe wear during downhole operations, resulting in a short service life, increased maintenance costs, and potential accidents. Existing wear-resistant belt materials are also unable to simultaneously possess high hardness, high wear resistance, and excellent strength and toughness.

Method used

High wear-resistant flux-cored welding wire is used, which contains a flux core and outer sheath with specific components. The wear resistance of the drill pipe joint is improved by additive manufacturing. The addition of elements such as Cr, Ti, Nb and RE in the flux core improves the performance of the weld overlay. The outer sheath is made of low carbon steel strip. The process includes cleaning, drying, mixing, rolling, filling and drawing.

Benefits of technology

It improves the wear resistance and crack resistance of drill pipe joints, with weld hardness reaching HRC70 or higher. After welding, it exhibits excellent wear resistance and crack resistance, extending the service life of drill pipe joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004798131700000051
    Figure BDA0004798131700000051
Patent Text Reader

Abstract

This invention discloses a high wear-resistant flux-cored welding wire for drill pipe joints and its preparation method, comprising an outer sheath and a flux-cored welding wire; the outer sheath is made of low-carbon steel strip; the flux core is composed of the following components by mass percentage: C: 0.3%–0.9%, Cr: 7%–18%, Mo: 0.5%–1.6%, B: 0.2%–1.5%, Si: 0.5%–1.2%, Mn: 0.5%–1.6%, Ni: 0.5%–4.5%, Ti: 0.2%–0.6%, Nb: 1.5%–6.0%, V: 0.3%–1.5%, RE: 0.15%–0.8%, with the balance being iron powder, and RE being one or more of Ce, Y, and La. Welds produced using this flux-cored welding wire have aesthetically pleasing weld formations, with an average macroscopic hardness exceeding HRC70, exhibiting excellent wear resistance and crack resistance, and are suitable for repairing or manufacturing drill pipe joints using arc or high-energy beam heat sources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of welding materials, specifically relating to a high wear-resistant flux-cored welding wire for drill pipe joints and its preparation method. Background Technology

[0002] In recent years, my country's oil and gas exploration industry has developed rapidly, and oil companies have continuously increased their requirements for the service life of drilling equipment. During downhole operations, drill pipe joints not only experience abrasive wear from broken shale and quartz sand, but also rub against the inner wall of the casing. The wear has also changed from single wear from shale and quartz sand to dual wear from shale and casing, accelerating the wear of the joint. Sometimes, the joints need to be scrapped and replaced after only one use, increasing maintenance costs and even causing accidents such as joint disengagement and partial well section failure, resulting in serious economic losses and resource waste.

[0003] Wear-resistant bands are one or more layers of high-hardness, high-wear-resistant hardened layers fixed to the drill pipe. By welding the wear-resistant band onto the surface of the drill pipe joint, wear between the drill pipe joint and the rock can be effectively prevented, while simultaneously separating the drill pipe from the casing wall, reducing wear on the drill pipe joint. Currently, commonly used manufacturing techniques include surfacing, thermal spraying, laser additive manufacturing, and plasma arc spraying. Among these, wear-resistant bands prepared by surfacing not only achieve high bonding strength with the drill pipe joint, but also have simple equipment, high production efficiency, strong scalability, and wide application. However, some problems also exist: it is difficult for wear-resistant band materials to simultaneously possess high hardness, high wear resistance, and excellent strength and toughness. Developing a welding material suitable for wear-resistant bands is of great significance. Summary of the Invention

[0004] To address the problems existing in the prior art, the main objective of this invention is to provide a high wear-resistant flux-cored welding wire for drill pipe joints, which has excellent welding performance. When used for welding drill pipe joints, the hardness of the wear-resistant band is greatly improved, resulting in good wear resistance and crack resistance.

[0005] Another objective of this invention is to provide a method for preparing the above-mentioned high wear-resistant flux-cored welding wire for drill pipe joints, which has a simple process.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A first aspect of the present invention provides a high wear-resistant flux-cored welding wire for drill pipe joints, comprising an outer sheath and a flux core; the outer sheath is made of low-carbon steel strip; the flux core is composed of the following components in weight percentage: C: 0.3%–0.9%, Cr: 7%–18%, Mo: 0.5%–1.6%, B: 0.2%–1.5%, Si: 0.5%–1.2%, Mn: 0.5%–1.6%, Ni: 0.5%–4.5%, Ti: 0.2%–0.6%, Nb: 1.5%–6.0%, V: 0.3%–1.5%, RE: 0.15%–0.8%, with the balance being iron powder.

[0008] Preferably, the outer skin is made of low-carbon steel strip with a width of 12-16 mm and a thickness of 0.4-1.0 mm.

[0009] Preferably, the outer sheath is made of low-carbon steel strip composed of the following components by mass percentage: C: 0.06%–0.08%, Si: 0.01%–0.03%, Mn: 0.35%–0.55%, S: 0.001%–0.025%, P: 0.0015%–0.025%, Cr: 0.001%–0.15%, Ni: 0.001%–0.3%, Cu: 0.01%–0.15%, with the balance being Fe and unavoidable impurities.

[0010] Preferably, the filling rate of the core is controlled at 25% to 30%.

[0011] Preferably, the particle size of the core components is 60-80 mesh, and the diameter is 1.2-2.0 mm.

[0012] Preferably, RE is a mixture of one or more of Ce, Y, and La, and satisfies the following: when RE is a mixture of two elements, the element content satisfies X1:X2=1; when RE is a mixture of three elements, La+Ce:Y=1:3.

[0013] Preferably, the component content of the core material satisfies the following condition: the content of impurity elements S and P is less than 0.025%.

[0014] Preferably, the component content of the core material satisfies the following ratio: Ti:Nb = 1:7~10.

[0015] Preferably, the component content of the core material satisfies the following conditions: when the C content is 0.6% to 0.9%, the Nb content does not exceed 6%, preferably 3% to 6%, thus possessing good mechanical properties.

[0016] Preferably, the composition of the core material satisfies the following conditions: when the Si content is 0.5% to 0.6%, the Mn content does not exceed 1.1%, preferably 0.9% to 1.1%, thus possessing good mechanical properties.

[0017] The high wear-resistant flux-cored wire for drill pipe joints of this invention improves the relative wear resistance of the joint through additive manufacturing. The weld overlay alloy exhibits good wear resistance. The design concept is as follows: adding a certain amount of carbon (C) to the flux core increases the weld strength; adding chromium (Cr) improves the high-temperature performance, hardenability, and wear resistance of the weld overlay; adding nitrogen (Ni) increases the toughness of the weld overlay; adding boron (B) increases the hardness of the cemented carbide phase and strengthens grain boundaries; Si and Mn deoxidize and increase the strength of the weld overlay; Ti refines the grains; adding Nb and Mo increases the strength and hardness of the weld; adding v promotes grain refinement and increases strength; and adding refractive acid (RE) refines the grains of the cladding layer and improves its hardness and wear resistance. The functions of each component are as follows:

[0018] C: It can react with alloying elements in the weld overlay to generate a high-hardness hard phase, which plays a role in solid solution strengthening of the weld.

[0019] Cr: Solid solution strengthening, promotes martensite formation, and improves the high-temperature performance, hardenability, and wear resistance of the weld overlay.

[0020] Mo has a solid solution strengthening effect, which can improve the strength and hardness of ferrite. When the content is about 0.5%, it can reduce or inhibit temper brittleness caused by other elements.

[0021] B: It can form more boride hard phases, which enhances the wear resistance of weld metal.

[0022] Si: Solid solution strengthening, which can eliminate the influence of oxygen in the weld.

[0023] Mn: Improves the strength and hardness of the weld, refines the acicular ferrite and coarse grain regions of the weld, and plays a role in deoxidation.

[0024] Ni can refine ferrite grains and improve the plasticity and toughness of steel.

[0025] Ti: Promotes the formation of acicular ferrite and refines grain size.

[0026] Nb: Refines grain size and improves the wear resistance of drill pipe joints.

[0027] V: It can increase the tempering stability of steel and has a strong secondary hardening effect, refine the grains, and improve mechanical strength.

[0028] RE: It can react with inclusions in steel, modify impurities, refine the structure of the weld overlay, refine the grains, and improve the wear resistance of the weld overlay.

[0029] A second aspect of the present invention also provides a method for preparing the high wear-resistant flux-cored wire for the drill pipe joint, comprising the following steps:

[0030] Step 1: Clean and remove rust from the low-carbon steel strip, and dry it;

[0031] Step 2: Weigh the raw materials according to the formula, put them in a drying oven at 200-300℃ for 4 hours, mix them evenly, and obtain the core powder;

[0032] Step 3: The pretreated low-carbon steel strip in Step 1 is first rolled by a roller press to form a U-shaped groove. Then, the core powder obtained in Step 2 is filled into the U-shaped groove by a powder feeder. The U-shaped groove is then closed by a forming machine and then drawn multiple times by a wire drawing machine until the specifications are met.

[0033] A third aspect of the invention also provides a high wear-resistant flux-cored wire for drill pipe joints for use in repairing or manufacturing drill pipe joints using arc or high-energy beam heat sources.

[0034] Compared with the prior art, the present invention has the following superior effects:

[0035] I. The addition of appropriate rare earth elements to the high wear-resistant flux-cored wire for the drill pipe joint of the present invention can improve the hardness of the weld overlay. The addition of rare earth elements to the weld overlay helps Cr and Ti elements to dissolve in the matrix structure, playing a role in solid solution strengthening. Their oxides can be reduced to rare earth elements by C elements to form a multiphase composite structure.

[0036] II. The weld seam of the drill pipe joint with an appropriate amount of rare earth elements added in this invention is aesthetically pleasing and has good wear resistance. The average macro hardness can reach HRC70 or above. At the same time, it has good crack resistance and is suitable for welding drill pipe joints. Detailed Implementation

[0037] To further clarify the purpose and technical solution of the present invention, the present invention will be further described in detail below with reference to the embodiments, but the scope of protection of the present invention is not limited to the following embodiments.

[0038] Example 1

[0039] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.45%, Cr: 7.50%, Mo: 0.55%, B: 0.25%, Si: 0.55%, Mn: 0.80%, Ni: 0.80%, Ti: 0.20%, Nb: 1.60%, V: 0.30%, RE: 0.15%, with the balance being iron powder.

[0040] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0041] Example 2

[0042] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.50%, Cr: 8.50%, Mo: 0.75%, B: 0.45%, Si: 0.65%, Mn: 1.00%, Ni: 1.00%, Ti: 0.30%, Nb: 2.3%, V: 0.40%, RE: 0.30%, with the balance being iron powder.

[0043] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0044] Example 3

[0045] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.60%, Cr: 9.50%, Mo: 0.90%, B: 0.80%, Si: 0.70%, Mn: 0.90%, Ni: 1.50%, Ti: 0.40%, Nb: 3.2%, V: 0.55%, RE: 0.45%, with the balance being iron powder.

[0046] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0047] Example 4

[0048] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.65%, Cr: 10.45%, Mo: 0.80%, B: 0.65%, Si: 0.60%, Mn: 1.20%, Ni: 2.00%, Ti: 0.45%, Nb: 3.5%, V: 0.75%, RE: 0.60%, with the balance being iron powder.

[0049] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0050] Example 5

[0051] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.70%, Cr: 12.80%, Mo: 1.25%, B: 0.95%, Si: 0.75%, Mn: 1.35%, Ni: 2.50%, Ti: 0.55%, Nb: 4.3%, V: 0.95%, RE: 0.70%, with the balance being iron powder.

[0052] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0053] Example 6

[0054] This embodiment provides a high wear-resistant flux-cored welding wire for oil drill pipe, the composition of which is as follows by mass percentage: C: 0.85%, Cr: 14.95%, Mo: 1.10%, B: 1.05%, Si: 0.90%, Mn: 1.55%, Ni: 3.00%, Ti: 0.60%, Nb: 6.0%, V: 1.20%, RE: 0.80%, with the balance being iron powder.

[0055] The flux-cored welding wire is prepared by the following method: The above raw materials are weighed and mixed evenly, then dried in a drying oven at 230℃ for 4 hours to obtain flux-cored powder. A low-carbon steel strip is placed on the feeding machine of a welding wire forming machine. The forming machine's pressing groove rolls the low-carbon steel strip into a U-shaped groove. The dried flux-cored powder is filled into the U-shaped groove, with a filling rate of 27%. The forming machine then closes the U-shaped groove. After wiping clean with anhydrous alcohol, the wire is drawn to a diameter of 1.6 mm. Finally, the oil on the welding wire is wiped off with a cotton cloth soaked in anhydrous alcohol.

[0056] The flux-cored welding wires prepared in Examples 1 to 6 were selected and welding experiments were conducted with conventional commercial flux-cored welding wires for oil drill pipes (Comparative Example 1 and Comparative Example 2). Gas metal arc welding was used, the shielding gas was 80% Ar + 20% CO2, the base material was Q235 steel, and the welding process parameters are shown in Table 1.

[0057] Table 1: Welding process parameters

[0058]

[0059] After welding, the weld overlay surface was ground smooth, and its macroscopic hardness was measured using an HR-150 Rockwell hardness tester with a load of 1.5 kN held for 15 seconds. Abrasive wear testing was performed using an MLS-255 wet sand rubber wheel abrasion tester under the following conditions: rubber wheel diameter 180 mm, rubber wheel speed 240 r / min, slurry ratio of 1.5 kg quartz sand and 1 kg water, and 2.5 kg of added weights. The sample was pre-ground for 1000 revolutions, rinsed and dried, and its initial mass M0 was measured. Then, it underwent fine grinding for 4000 revolutions, and the weight M1 of the fine-ground sample was measured. The mechanical properties of the weld metal are shown in Table 2.

[0060] Table 2: Mechanical properties of weld metal

[0061] Serial Number Hardness HRC <![CDATA[M0 before wear / g]]> <![CDATA[M1 / g after wear]]> Wear amount ΔM / g Example 1 72.8 83.7892 81.8112 1.978 Example 2 73.2 85.4743 83.5193 1.935 Example 3 75.1 82.9217 81.1547 1.767 Example 4 78.1 84.2715 82.5985 1.673 Example 5 74.3 83.9203 82.0663 1.854 Example 6 73.5 83.5820 81.6740 1.908 Comparative Example 1 61.5 85.2008 81.6528 3.548 Comparative Example 2 62.1 83.6680 80.2930 3.375

[0062] As can be seen from Table 2, the hardness of Examples 1 to 6 is greater than that of Comparative Examples 1 and 2, and the wear is less than that of Comparative Examples 1 and 2. It can be concluded that the performance of the flux-cored welding wire of the present invention is better than that of the comparative examples, and the drill pipe joint with added rare earth elements has better wear resistance.

[0063] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A high wear-resistant flux-cored welding wire for drill pipe joints, characterized in that, It includes an outer sheath and a core; the outer sheath is made of low-carbon steel strip; the core is composed of the following components in mass percentage: C: 0.3%~0.9%, Cr: 7%~18%, Mo: 0.5%~1.6%, B: 0.2%~1.5%, Si: 0.5%~1.2%, Mn: 0.5%~1.6%, Ni: 0.5%~4.5%, Ti: 0.2%~0.6%, Nb: 1.5%~6.0%, V: 0.3%~1.5%, RE: 0.15%~0.8%, with the balance being iron powder; RE is a mixture of one or more of Ce, Y, and La, and satisfies the following: when RE is a mixture of two elements, the element content satisfies X1:X2=1; when RE is a mixture of three elements, La+Ce:Y=1:

3. The component content of the core material meets the following requirement: the content of impurity elements S and P is less than 0.025%; The component content of the core material satisfies the following condition: Ti:Nb = 1:7~10; The component content of the core meets the following requirements: when the C content is 0.6%~0.9%, the Nb content is 3%~6%; The component content of the core meets the following requirements: when the Si content is 0.5%~0.6%, the Mn content does not exceed 1.1%.

2. The high wear-resistant flux-cored welding wire for drill pipe joints according to claim 1, characterized in that, The outer skin uses low-carbon steel strips with a width of 12~16mm and a thickness of 0.4~1.0mm.

3. The high wear-resistant flux-cored welding wire for drill pipe joints according to claim 1 or 2, characterized in that, The outer sheath is made of low-carbon steel strip composed of the following components by mass percentage: C: 0.06%~0.08%, Si: 0.01%~0.03%, Mn: 0.35%~0.55%, S: 0.001%~0.025%, P: 0.0015%~0.025%, Cr: 0.001%~0.15%, Ni: 0.001%~0.3%, Cu: 0.01%~0.15%, with the balance being Fe and unavoidable impurities.

4. The high wear-resistant flux-cored welding wire for drill pipe joints according to claim 1, characterized in that, The filling rate of the core is controlled at 25% to 30%.

5. The high wear-resistant flux-cored welding wire for drill pipe joints according to claim 1, characterized in that, The particle size of the core components is 60-80 mesh, and the diameter is 1.2-2.0 mm.

6. The method for preparing the high wear-resistant flux-cored wire for drill pipe joints according to any one of claims 1 to 5, characterized in that, Includes the following steps: Step 1: Clean and remove rust from the low-carbon steel strip, and dry it; Step 2: Weigh the raw materials according to the formula, put them in a drying oven at 200~300℃ for 4 hours, mix them evenly, and obtain the core powder; Step 3: The pretreated low-carbon steel strip in Step 1 is first rolled by a roller press to form a U-shaped groove. Then, the core powder obtained in Step 2 is filled into the U-shaped groove by a powder feeder. The U-shaped groove is then closed by a forming machine and then drawn multiple times by a wire drawing machine until the specifications are met.

7. The high wear-resistant flux-cored wire for drill pipe joints as described in any one of claims 1 to 5 is used for repairing or manufacturing drill pipe joints using arc or high-energy beam heat sources.

Citation Information

Patent Citations

  • Flux-cored wire for rail wagon wheel additive manufacturing and preparation method of flux-cored wire

    CN114871624A

  • Flux-cored wire for surfacing parts subject to high abrasive wear

    RU206282U1