A resin impregnation method and a method for preparing reconstituted bamboo.
By employing a three-stage impregnation method involving vacuum, pressure, and vacuum, the problem of uneven impregnation of reconstituted bamboo was solved, achieving uniform penetration of the adhesive into the bamboo fiber. This improved the mechanical properties and production efficiency of the reconstituted bamboo while reducing costs.
Patent Information
- Application Number
- CN202410764827.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-06-14
AI Technical Summary
In existing technologies, the uneven impregnation of reconstituted bamboo leads to low production efficiency, high costs, and significant waste of adhesives, making it difficult to achieve uniform penetration and high-strength bonding.
A three-stage impregnation method of vacuum-pressurization-vacuum is adopted. The vacuum stage removes air from the bamboo fiber, the pressurization stage promotes adhesive penetration, and the vacuum stage ensures uniform coverage. Combined with incremental pressure control, the penetration of adhesive is controlled to achieve uniform distribution of adhesive.
This method achieves uniform penetration of adhesives into bamboo fibers, improves the mechanical strength and internal bonding strength of reconstituted bamboo, reduces production costs and energy consumption, and increases production efficiency.
Smart Images

Figure CN118386345B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of artificial bamboo products, specifically a method for impregnating bamboo bundles or fibrous bamboo veneers with resin; this application also relates to a method for preparing reconstituted bamboo using this impregnation method. Background Technology
[0002] Reconstituted bamboo is a type of board made by assembling bamboo bundles or fiberized veneers as basic units, using phenolic resin as an adhesive, and then gluing and pressing them together along the grain. The density of reconstituted bamboo can reach 1.0-1.30 g / cm³. 3 It boasts superior performance compared to other bamboo-based composite materials, such as plywood, particleboard, or reconstituted wood. Furthermore, it is aesthetically pleasing, retains the advantages of natural bamboo, including its lightweight, high strength, and eco-friendliness, while eliminating the disadvantages of unstable performance and poor durability. It is a relatively ideal green, high-strength material with applications in various fields, including outdoor flooring, landscaping materials, building beams and columns, wind turbine blade substrates, all-bamboo container flooring, and train carriage flooring.
[0003] The impregnation process is a crucial step in the preparation of reconstituted bamboo. The efficiency and quality of the impregnation directly impact production costs and the final quality of the reconstituted bamboo. Most companies employ an intermittent hanging cage method, vertically placing large batches of bamboo bundles and immersing them in a phenolic resin adhesive (PF) with a solid content of 25-30% for 15 minutes to achieve an adhesive application rate of approximately 15-25%. Examples include the utility model patent CN213161604U, entitled "A Lifting Impregnation Tank for Reconstituted Bamboo Furniture Production," and the invention patent application CN105666631A, entitled "An Adhesive Application Method for Outdoor Reconstituted Bamboo." However, in these methods, the adhesive may not have penetrated to the center of the bamboo bundles or fiber veneer before the impregnation process is complete, resulting in uneven impregnation as the bamboo in the center may not be properly wetted. During the subsequent glue application process, glue from the top of the bamboo bundles will drip down along the bundles, potentially causing uneven glue application inside and at the ends. Furthermore, to save impregnation time, achieve a certain impregnation rate, and ensure uniform glue application, a higher solids content polyphenol (PF) is typically used for impregnation. This results in relatively long glue application and drying times, as well as wasted PF, reduced efficiency in reconstituted bamboo manufacturing, increased production costs, and high drying energy consumption.
[0004] To address this, existing technologies have proposed several technical solutions to improve the impregnation effect of bamboo bundles or fibrous bamboo veneers. For example, the rolling impregnation technique disclosed in the invention patent with publication number CN112372774B, entitled "A bamboo-based fiber composite material and its preparation method," can improve the uniformity of impregnation and save drying time and energy consumption, but the amount impregnated at one time is small, resulting in relatively low production efficiency.
[0005] For example, the invention patent application with publication number CN106965271A, entitled "An Outdoor Reconstituted Bamboo Product and Preparation Method", discloses a technical solution of first heat-treating bamboo bundles and then impregnating them with resin. This solution can improve the dimensional stability and internal bonding strength of the reconstituted bamboo bundles, but it cannot solve the problems of uneven PF distribution and penetration.
[0006] For example, the vacuum impregnation technology disclosed in the invention patent application with publication number CN101637932A entitled "Method for Impregnating Bamboo and Wood Strips with High Moisture Content" can improve the permeability of bamboo and wood strips. Under the premise of achieving the same amount of glue, adhesives with relatively low solid content can be used. However, in actual operation, good permeability can improve the bonding effect to a certain extent, reduce the solid content of the adhesive, and increase the bonding strength, but the degree of improvement is limited. Summary of the Invention
[0007] Through practice, the inventors discovered that the uniformity of the adhesive impregnation process—that is, the even coating of the adhesive onto the surface of the bamboo fibers (including bamboo filaments and / or fibrous bamboo veneer) within the bamboo fiber bundle—is crucial for improving the impregnation effect, and its effect far surpasses that of methods that improve the permeability of the bamboo fibers themselves. Therefore, this application provides an impregnation method that uses a vacuum-pressurization-vacuum approach to ensure that the adhesive can more evenly coat the surface of the bamboo fibers within the bamboo fiber bundle, thereby improving the uniformity of the impregnation.
[0008] One aspect of this application provides an impregnation method carried out in a vacuum-pressure vessel, comprising a pre-vacuum stage, a pressurization stage, and a post-vacuum stage, wherein the vacuuming time of the pre-vacuum stage is 3-5 min, the pressure of the pressurization stage is 0.5-1.5 MPa and the pressure holding time is 10-15 min, and the vacuuming time of the post-vacuum stage is 10-12 min.
[0009] By employing the above method, the pre-vacuum stage causes air to be expelled from the gaps and pores of the bamboo fiber bundle; the pressurization stage causes the adhesive to penetrate into the center of the bamboo fiber bundle, thereby allowing the bamboo fibers in the bundle to be more evenly wetted by the adhesive, and further penetrating into the cells of the bamboo fibers; the post-vacuum stage causes the adhesive to further evenly coat the surface of the bamboo fibers and penetrate into the cells of the bamboo fibers. Therefore, the impregnation method of this application allows the adhesive to penetrate more evenly into the center of the bamboo fiber bundle, and the bamboo fibers located in the center are also wetted by the adhesive. Simultaneously, the impregnation method of this application expels air from the gaps and pores of the bamboo fiber bundle under vacuum conditions, and forces the adhesive into the gaps and pores of the bamboo fiber bundle under pressurization conditions. Therefore, compared with the existing vacuum impregnation technology, the impregnation is more uniform and takes less time. Using bamboo fibers with similar sizing amounts, and ensuring that the surface of the bamboo fibers is uniformly coated with adhesive, it is possible to press reconstitute bamboo with lower hygroscopicity, higher mechanical strength, and higher internal bond strength. Furthermore, it is suitable for impregnating bundled bamboo fibers, thus allowing for a larger amount of bamboo fiber to be impregnated in a single process compared to existing rolling impregnation techniques.
[0010] Preferably, the moisture content of the bamboo fiber is 10-20% before impregnation.
[0011] Preferably, during the pressurization phase, the pressure is increased from 0.5 MPa to 1.5 MPa.
[0012] After impregnation, some adhesive adheres to the surface of the bamboo fibers, while some penetrates into the cells of the bamboo fibers; both together constitute the actual amount of adhesive applied. However, during the pressing process, the adhesive in the cells is squeezed out and, together with the adhesive originally attached to the surface of the bamboo fibers, solidifies to form an adhesive film. Furthermore, the material properties of bamboo vary considerably due to factors such as the variety, age, origin, and harvesting season of the raw bamboo. This means that even using the same impregnation process, the amount of adhesive entering and penetrating the bamboo fiber cells may differ, and in some cases, the deviation can be significant. This makes it difficult to control the actual amount of adhesive applied.
[0013] The inventors discovered that a three-stage process of vacuum-pressurization-vacuum can improve the uniformity of impregnation, which promotes the penetration of high-solids-content adhesives with poor flowability between bamboo fibers. Furthermore, the inventors found that when the pressure is applied in an incremental manner during the pressurization stage, it promotes the penetration of relatively high-solids-content adhesives into the gaps in the center of the bamboo fiber bundles, but not into the pores of the bamboo fiber cells. For example, it can evenly penetrate adhesives with a solids content exceeding 30%. This effectively avoids the problem of difficulty in controlling the actual amount of adhesive applied due to differences in bamboo properties, and improves the consistency of impregnation effects across different batches of bamboo. In practice, this can reduce the amount of adhesive applied, i.e., the actual amount of adhesive consumed. Using adhesives with higher solids content can also shorten the time and energy consumption of the drying process after impregnation. Preferably, the solids content of the adhesive used is 35-40%.
[0014] The pressure increase during the pressurization phase is preferably achieved through multiple pressure segments. For example, the pressurization phase includes multiple pressure segments, with the first segment having a pressure of 0.5-0.8 MPa and a pressure holding time of 3-5 minutes, and the last segment having a pressure of 1.2-1.5 MPa and a pressure holding time of 2-3 minutes.
[0015] Furthermore, the pressurization stage includes three pressure zones: the first pressure zone has a pressure of 0.7-0.8 MPa and a pressure holding time of 3-5 min; the middle pressure zone has a pressure of 1.0-1.1 MPa and a pressure holding time of 4-7 min; and the last pressure zone has a pressure of 1.3-1.5 MPa and a pressure holding time of 2-3 min.
[0016] Building upon the foregoing, the inventors further discovered that, since the actual amount of adhesive applied is controllable, only the same or slightly more adhesive as the actual amount applied (i.e., the actual amount of adhesive consumed) needs to be added to the vacuum-pressure vessel. The added adhesive is completely and evenly permeated between the bamboo fiber bundles and uniformly coated onto the surface of the bamboo fibers. This process allows the bamboo fiber bundles after impregnation to be directly dried without the need for desizing or adhesive recycling. This improvement eliminates the time required for desizing and avoids the problem of different adhesive amounts at the ends of the bamboo fibers caused by desizing. Preferably, the mass ratio of the amount of adhesive introduced into the vacuum-pressure vessel to the actual amount of adhesive consumed is (1.02-1.05):1.
[0017] The second aspect of this application provides a method for preparing reconstituted bamboo, including an impregnation process, a drying process, and a pressing process. The impregnation process involves impregnating bamboo fibers in a vacuum-pressure vessel, including a pre-vacuum stage, a pressurization stage, and a post-vacuum stage. The vacuuming time in the pre-vacuum stage is 3-5 minutes, the pressure in the pressurization stage is 0.5-1.5 MPa, and the pressure is maintained for 10-15 minutes. The vacuuming time in the post-vacuum stage is 10-12 minutes. The bamboo fibers after the impregnation process directly enter the drying process.
[0018] Preferably, the pressing process includes a blank assembly stage, a feeding stage, a pressing stage, and a discharging stage. The feeding stage involves feeding the assembled veneer into the hot press at room temperature. After the temperature of the hot press plate is raised to 150-160°C, the pressing stage begins. Timing starts from when the internal temperature of the assembled veneer reaches 130°C, and the pressing time is 10-12 minutes to obtain reconstituted bamboo. The discharging stage involves removing the reconstituted bamboo from the hot press after the temperature of the hot press plate has dropped to a temperature not exceeding 65°C.
[0019] By using the above method, before the pressing stage begins, the veneer of the assembly is brought to a relatively high temperature, preferably 130°C. At this temperature, pressure is applied to the veneer, which allows the adhesive to cure evenly and the density of the reconstituted bamboo to be relatively uniform throughout, thereby obtaining reconstituted bamboo with high mechanical strength.
[0020] Preferably, the time interval between the impregnation process and the drying process is no more than 10 minutes.
[0021] In summary, the impregnation method provided in this application can achieve uniform impregnation of the adhesive in a relatively short time, and can process a large volume at a time, significantly shortening the time required for glue extrusion and resulting in high production efficiency. This application also provides a method for preparing reconstituted bamboo using this impregnation method, which can produce reconstituted bamboo with lower hygroscopicity, higher mechanical strength, and higher internal bond strength. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a schematic diagram of the process flow for the preparation method of recombinant bamboo provided in the embodiments of this application.
[0024] Figure 2 This is a schematic diagram of the vacuum-pressure vessel used in the impregnation method of Embodiment 5 of this application.
[0025] Figure 3 Fluorescence micrographs of the cross-sectional and radial sections of the bonding interfaces of Comparative Examples 1 (a, b), 2 (c, d), and 2 (e, f) of this application.
[0026] Figure 4 The image shows the distribution of adhesive lines on the end faces of reconstituted bamboo prepared from bamboo fibers of Comparative Examples 1(a), 2(b), and 5(c) of this application. Detailed Implementation
[0027] To enable those skilled in the art to better understand the technical solutions in this application, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this application.
[0028] This application discloses a method for preparing reconstituted bamboo, which includes an impregnation process, a drying process, and a pressing process.
[0029] The impregnation process involves impregnating bamboo fibers with adhesive in a vacuum-pressure tank. Before impregnation, the bamboo fibers are dried or equilibrated using existing technologies to control their moisture content within the range of 10-20%. The drying process removes moisture and starch from the bamboo fiber cells, allowing the adhesive to penetrate more easily.
[0030] The impregnation process includes a pre-vacuum stage, a pressurization stage, and a post-vacuum stage. The pre-vacuum stage takes 3-5 minutes to evacuate, the pressurization stage takes 0.5-1.5 MPa and maintains the pressure for 10-15 minutes, and the post-vacuum stage takes 10-12 minutes to evacuate.
[0031] In implementations using a single-pressure process during the pressurization stage, adhesives with relatively low solids content can be used to achieve the target application rate. After the impregnation process, a 10-15 minute degreasing treatment is required to remove excess adhesive from the bamboo fiber bundles.
[0032] In some embodiments, the pressure is increased from 0.5 MPa to 1.5 MPa during the pressurization phase. In this embodiment, adhesives with a solid content higher than 30% are permitted, for example, adhesives with a solid content of 35-40%. After the impregnation process, a 5-10 minute desizing treatment is required to remove excess adhesive from the bamboo fiber bundles.
[0033] In other embodiments, the pressurization stage includes multiple pressure zones. The first pressure zone has a pressure of 0.5-0.8 MPa and a pressure holding time of 3-5 minutes, while the last pressure zone has a pressure of 1.2-1.5 MPa and a pressure holding time of 2-3 minutes. In this embodiment, adhesives with a solid content higher than 30% are permitted. Simultaneously, by controlling the mass ratio of adhesive introduced into the vacuum-pressure vessel to the actual adhesive consumption to be (1.02-1.05):1, the step of degreasing and the recycling of adhesive resulting from degreasing can be eliminated, allowing the bamboo fibers after the impregnation process to directly enter the drying process. To avoid altering the adhesive distribution on the bamboo fiber surface under gravity, preferably, the time interval between the impregnation and drying processes does not exceed 10 minutes.
[0034] The aforementioned actual adhesive consumption is the amount of adhesive used, calculated based on the target application amount, using the following formula:
[0035] Where: W is the actual amount of adhesive consumed; C' is the target amount of adhesive applied; m0 (kg) is the initial mass of bamboo fiber; w is the solid content of the adhesive; and x is the moisture content of the bamboo fiber before impregnation.
[0036] The adhesive content, i.e. the actual amount of adhesive applied, is calculated using the following formula:
[0037] Where: C is the glue content; m0 (kg) and m2 (kg) are the initial mass and the mass after glue impregnation of bamboo fiber, respectively; w is the solid content of the adhesive; and x is the moisture content of bamboo fiber before glue impregnation.
[0038] The drying process involves drying the sizing bamboo fiber at a temperature of 60-70℃ or other suitable temperature conditions until the moisture content is below 8-10%.
[0039] The pressing process includes the assembly stage, feeding stage, pressing stage, and discharging stage. The feeding stage involves feeding the assembled veneers into the hot press at room temperature. After the hot press plate temperature is raised to 150-160℃, the pressing stage begins. Timing starts when the internal temperature of the assembled veneer reaches 130℃, and the pressing time is 10-12 minutes, yielding reconstituted bamboo. The discharging stage involves removing the reconstituted bamboo from the hot press after the hot press plate temperature drops to no higher than 65℃.
[0040] Example 1: Using moso bamboo from Huangshan County, Anhui Province, the bamboo was processed into fibrous bamboo veneer through methods such as rolling and thinning. The initial moisture content of the bamboo fiber was 10-20%, with an average moisture content of 16.5%. A phenolic resin adhesive (PF) with a solid content of 52.98 wt%, a viscosity of 65 cps (25°C), and a pH of 9.74 was purchased from Guangdong Dena Chemical Co., Ltd. in China. The solid content of the phenolic resin adhesive (PF) was diluted with water to 25 wt%. The bamboo fiber was placed in a vacuum-pressure vessel, and after being filled with the phenolic resin adhesive (PF), an impregnation process was carried out.
[0041] The impregnation process is as follows: vacuuming for 3 minutes in the pre-vacuum stage, pressure of 0.5 MPa and pressure holding time of 12 minutes in the pressurization stage, vacuuming for 10 minutes in the post-vacuum stage, and then performing a 10-minute desizing process after the impregnation process.
[0042] In the drying process, the moisture content of the resin-impregnated bamboo fiber is dried to 8-10%.
[0043] In the pressing process, bamboo fiber is assembled into veneer blanks using existing technology; then, the assembled veneers are fed into a hot press at room temperature; the pressing plate temperature of the hot press is raised to 150℃ before the pressing stage begins. Timing starts from when the internal temperature of the assembled veneer reaches 130℃, and the pressing time is 10 minutes, resulting in a density of 1.15 g / cm³. 3 The reconstituted bamboo is then removed from the hot press after the temperature of the press plate has dropped to 60°C.
[0044] Finally, the reconstituted bamboo was placed in an environment of 20°C / 65%RH until its weight did not change, i.e., its mass was constant.
[0045] Example 2: The difference between Example 2 and Example 1 is that the impregnation process is as follows: vacuuming for 3 minutes in the pre-vacuum stage, pressure of 1.0 MPa and pressure holding time of 12 minutes in the pressurization stage, vacuuming for 10 minutes in the post-vacuum stage, and 10 minutes of desizing after the impregnation process is completed.
[0046] Example 3: The difference between Example 3 and Example 1 is that the impregnation process is as follows: vacuuming for 3 minutes in the pre-vacuum stage, pressure of 1.5 MPa and pressure holding time of 12 minutes in the pressurization stage, vacuuming for 10 minutes in the post-vacuum stage, and 10 minutes of desizing after the impregnation process is completed.
[0047] Example 4: The difference between Example 4 and Example 1 is that the solid content of the phenolic resin adhesive (PF) was diluted to 35 wt% with water.
[0048] The impregnation process is as follows: vacuuming for 3 minutes in the pre-vacuum stage; gradually increasing the pressure from 0.8 MPa to 1.2 MPa in the pressurization stage at a rate of 0.04 MPa / min, with a total pressurization time of 10 minutes; vacuuming for 10 minutes in the post-vacuum stage; and applying adhesive for 5 minutes after the impregnation process is completed.
[0049] Example 5: The difference between Example 4 and Example 1 is that the solid content of the phenolic resin adhesive (PF) was diluted with water to 38 wt%. Production practice has shown that an application rate of 25% is sufficient to form an ideal glue line and achieve the desired bonding effect; therefore, this example sets the target application rate at 25%. Simultaneously, the initial average moisture content of the bamboo fiber was measured to be 32%, and the adhesive was added at 1.05 times the calculated application rate. The calculated amount of adhesive added to the vacuum-pressure vessel was 0.47 kg of adhesive per kilogram of bamboo fiber. Of course, since the amount of adhesive added is relatively small, a relatively small vacuum-pressure vessel should be used, and a method such as... Figure 2 The shown adhesive injection device allows bamboo fibers to be immersed in adhesive. The adhesive injection device 1 is installed in a vacuum-pressure tank 2. The vacuum-pressure tank 2 has a bamboo fiber receiving box 21 with an open top. The adhesive injection device 1 includes a plurality of adhesive-spraying tubes 11 spaced apart along the length of the bamboo fiber receiving box 21. The bottom of each adhesive-spraying tube 11 has a plurality of adhesive-spraying ports 12. Each adhesive-spraying tube 11 is controlled to open and close by its own solenoid valve and is connected to a main adhesive injection tube 13 through a pipeline. The main adhesive injection tube 13 is connected to an external adhesive source through a main solenoid valve.
[0050] Of course, other feasible vacuum-pressure tank structures can also be used, as long as the adhesive can be applied evenly to all parts of the bamboo fiber bundle during the glue application process and the bundle can be immersed in the adhesive during the impregnation process. In the subsequent vacuum-pressure-vacuum treatment process, the adhesive can improve its fluidity under the action of vacuum-pressure and penetrate evenly into the gaps between the bamboo fibers.
[0051] The impregnation process is as follows: the pre-vacuum stage involves evacuating for 3 minutes; the pressurization stage includes three pressure zones: the first pressure zone has a pressure of 0.7 MPa and a pressure holding time of 3 minutes; the middle pressure zone has a pressure of 1.1 MPa and a pressure holding time of 5 minutes; and the last pressure zone has a pressure of 1.5 MPa and a pressure holding time of 3 minutes; the post-vacuum stage involves evacuating for 10 minutes.
[0052] After the impregnation process is completed, no glue-draining treatment is performed, and the bamboo fiber is sent to the drying device for drying within 10 minutes.
[0053] Example 6: The difference between Example 6 and Example 2 is that in the pressing process, bamboo fiber is assembled into a veneer blank using existing techniques, i.e., assembled veneer. After the temperature of the hot press plate is raised to 150°C, the assembled veneer is fed into the hot press, the press is closed, and the pressing stage begins. The pressing stage lasts for 10 minutes, resulting in reconstituted bamboo. Finally, after the temperature of the hot press plate drops to 60°C, the reconstituted bamboo is removed from the hot press. It was detected that the internal temperature of the assembled veneer was 68°C when entering the pressing stage.
[0054] Comparative Example 1: Fiberized bamboo veneer was used, with an initial moisture content of 10-20% and an average moisture content of 16.8%. A phenolic resin adhesive (PF) with a solid content of 52.98 wt%, a viscosity of 65 cps (25°C), and a pH of 9.74 was used. The solid content of the PF was diluted to 25 wt% with water. Impregnation was performed in a vacuum tank at a vacuum pressure of -0.08 MPa for 15 minutes. The drying and pressing processes were the same as in Example 1.
[0055] Comparative Example 2: Fiberized bamboo veneer was used, with an initial moisture content of 10-20% and an average moisture content of 16.3%. A phenolic resin adhesive (PF) with a solid content of 52.98 wt%, a viscosity of 65 cps (25°C), and a pH of 9.74 was used. The solid content of the PF was diluted to 25 wt% with water. Impregnation was performed under normal pressure for 15 minutes. The drying and pressing processes were the same as in Example 1.
[0056] After being pressed at high temperature, the phenolic resin adhesive cures and bonds with bamboo fiber (matrix) to form a band-shaped bond line. The sample was immersed in 0.5% toluidine blue for 30 minutes to observe the distribution of the bond line and phenolic resin adhesive in the reconstituted bamboo. Figure 2 Fluorescence micrographs of the cross-sectional and radial sections of the bonding interfaces of Comparative Examples 1 (a, b), 2 (c, d), and 2 (e, f). Figure 2As can be seen, in Comparative Examples 1 and 2, due to uneven impregnation, only discontinuous adhesive points exist, failing to form the ideal continuous and complete adhesive line. Furthermore, the adhesive points are irregularly distributed on the surface of the fibers and cells. In Example 3, because the vacuum-pressure-vacuum impregnation method allows the adhesive to penetrate evenly between the bamboo fibers, a complete and continuous adhesive line can be formed. This microscopically confirms that the impregnation method in Example 2 ensures that the adhesive is evenly impregnated in the bamboo fiber bundles and also evenly distributed in the pressed reconstituted bamboo.
[0057] Figure 4 The distribution of adhesive lines on the end faces of reconstituted bamboo prepared from bamboo fibers in Comparative Examples 1(a), 2(b), and 5(c) is shown. In the figures, no continuous brown adhesive lines are observed on the end faces of the reconstituted bamboo in Comparative Examples 1 and 2, while continuous, complete, and darker adhesive lines are clearly visible on the end faces of the reconstituted bamboo in Example 5. This confirms that the impregnation method of Example 5 ensures that the adhesive is uniformly impregnated in the bamboo fiber bundles and also uniformly distributed in the pressed reconstituted bamboo. In contrast, in the comparative examples, because the adhesive could not be uniformly impregnated in the bamboo fiber bundles during the impregnation process, nor could it be uniformly distributed in the reconstituted bamboo, no continuous adhesive lines were observed on the end faces of the reconstituted bamboo. The presence of continuous, complete adhesive lines macroscopically confirms that the reconstituted bamboo prepared by the impregnation method of Example 5 has lower hygroscopicity, higher mechanical strength, and higher internal bond strength.
[0058] The solid content of the adhesive directly affects the shape of the glue line. Only when the solid content of the adhesive is not less than 30% can a glue line be formed. Figure 2 The adhesive lines shown are continuous, complete, and of a certain thickness. In the impregnation methods of Examples 1-5, when a low solid content of the adhesive is used (e.g., 25% solid content commonly used in the prior art), the low solid content adhesive will penetrate too much into the cell wall, making it difficult to form an ideal adhesive line.
[0059] The thickness of the adhesive thread is related to the solid content of the adhesive, as obtained by the technical solution in Example 5. Figure 3 (c) The thickness of the adhesive line is 228.3 μm. The thickness of the adhesive line decreases accordingly with decreasing solid content. The technical solutions of Comparative Example 1 and Comparative Example 2 respectively obtained... Figure 3 (a) and Figure 3 The thickness of the glued lines in (b) is only 50.7 μm and 139.7 μm, and the thickness is not uniform.
[0060] Table 1 shows the physicochemical properties of reconstituted bamboo prepared from impregnated bamboo fibers in Examples 1-6 and Comparative Examples 1-2. The water absorption thickness swelling rate was determined according to GB / T 30364-2013 using a 28-hour treatment test: the sample was immersed in boiling water (100°C) for 4 hours, then dried in an oven at 63°C for 24 hours, and finally immersed again in boiling water (100°C) for 4 hours. Static bending strength (MOR), modulus of elasticity (MOE), and horizontal shear strength (HSS) were determined according to GB / T 30364-2013.
[0061] Table 1. Physicochemical properties of reconstituted bamboo in Examples 1-6 and Comparative Examples 1-2 Group Actual application rate / % Adhesive consumption / kg (per kilogram of bamboo fiber) Water absorption thickness swelling rate / % Static bending strength / MPa Elastic modulus / GPa Horizontal shear strength / MPa Example 1 23 0.74 4.5 183.7 20.8 24.1 Example 2 24 0.73 4.4 187.3 21.5 25.9 Example 3 25 0.78 4.2 190.5 22.3 26.2 Example 4 24 0.72 4.2 198.2 23.7 27.4 Example 5 24 0.58 4.0 209.5 24.5 28.1 Example 6 24 0.63 4.8 186.6 20.5 24.3 Compare with Example 1 19 1.30 8.9 156.7 19.6 19.3 Compare with Example 2 21 1.10 6.7 169.5 20.1 22.4 The above description is for illustrative purposes and not for limitation. Many embodiments and applications beyond the provided examples will become apparent to those skilled in the art upon reading the above description. Therefore, the scope of this teaching should not be determined by reference to the above description, but rather by reference to the appended claims and the full scope of their equivalents. For purposes of completeness, all articles and references, including patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject disclosed herein in the preceding claims is not an abandonment of that subject matter, nor should it be construed as an indication that the applicant has not considered that subject matter as part of the disclosed application subject matter.
Claims
1. A method for impregnating bamboo fibers in a vacuum-pressure tank, comprising a pre-vacuum stage, a pressurization stage, and a post-vacuum stage, characterized in that, The vacuuming time in the pre-vacuum stage is 3-5 min, the pressure in the pressurization stage is 0.5-1.5 MPa and the pressure holding time is 10-15 min, and the vacuuming time in the post-vacuum stage is 10-12 min. The pressurization stage includes three pressure zones: the first pressure zone has a pressure of 0.7-0.8 MPa and a pressure holding time of 3-5 min; the middle pressure zone has a pressure of 1.0-1.1 MPa and a pressure holding time of 4-7 min; and the last pressure zone has a pressure of 1.3-1.5 MPa and a pressure holding time of 2-3 min. The adhesive used has a solid content exceeding 30%; The mass ratio of the amount of adhesive introduced into the vacuum-pressure vessel to the actual amount of adhesive consumed is (1.02-1.05):
1.
2. The impregnation method according to claim 1, characterized in that, Before impregnation, the moisture content of the bamboo fiber is 10-20%.
3. A method for preparing reconstituted bamboo, characterized in that, The process includes impregnation, drying, and pressing. The impregnation process involves impregnating bamboo fiber with resin in a vacuum-pressure tank, and includes a pre-vacuum stage, a pressurization stage, and a post-vacuum stage. The vacuuming time in the pre-vacuum stage is 3-5 minutes, the pressure in the pressurization stage is 0.5-1.5 MPa and the pressure is maintained for 10-15 minutes, and the vacuuming time in the post-vacuum stage is 10-12 minutes. The pressurization stage includes three pressure zones: the first pressure zone has a pressure of 0.7-0.8 MPa and a pressure holding time of 3-5 min; the middle pressure zone has a pressure of 1.0-1.1 MPa and a pressure holding time of 4-7 min; and the last pressure zone has a pressure of 1.3-1.5 MPa and a pressure holding time of 2-3 min. The adhesive used has a solid content exceeding 30%; The bamboo fibers that have undergone the impregnation process directly enter the drying process.
4. The method for preparing reconstituted bamboo according to claim 3, characterized in that, The pressing process includes a blank assembly stage, a feeding stage, a pressing stage, and a discharging stage. The feeding stage involves feeding the assembled veneers into the hot press at room temperature. After the temperature of the hot press plate is raised to 150-160°C, the pressing stage begins. Timing starts from when the internal temperature of the assembled veneers reaches 130°C, and the pressing time is 10-12 minutes to obtain reconstituted bamboo. The discharging stage involves removing the reconstituted bamboo from the hot press after the temperature of the hot press plate has dropped to a temperature not exceeding 65°C.
5. The method for preparing reconstituted bamboo according to claim 3, characterized in that, The time interval between the impregnation process and the drying process shall not exceed 10 minutes.
Citation Information
Patent Citations
Gum leakage method of bamboo-wood rods with high water content
CN101637932A
Gluing method for recombined bamboo for outdoor use
CN105666631A
Outdoor reconsolidated bamboo product and preparation method
CN106965271A
Bamboo-based fiber composite materials and their continuous preparation methods
CN112372774B
Lifting type glue dipping pool for recombined bamboo furniture production
CN213161604U