A kind of ecological composite board based on graphene and preparation method thereof
By using graphene and modified lignin stearate in the adhesive of ecological composite boards to form epoxidized lignin stearate and aminated graphene, the bonding problems of traditional adhesives in humid and high-temperature environments are solved. Insufficient performance and formaldehyde release issues have been achieved, achieving the effect of a formaldehyde-free, water-resistant, and high-temperature-resistant adhesive.
Patent Information
- Application Number
- CN202410406624.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-07
AI Technical Summary
In the process of preparing ecological composite boards, traditional urea-formaldehyde resin adhesives use formaldehyde as raw materials, which causes the products to release formaldehyde for a long time and cause harm to the human body. The adhesive has insufficient bonding performance in humid and high-temperature environments.
A composite epoxy resin adhesive based on graphene is used to react lignin with stearyl chloride to generate hydrophobic segments, and then react with epichlorohydrin to introduce epoxy groups to form epoxidized lignin stearate, and Aminated graphene is added to form a dense graphene layer to improve adhesion and anti-corrosion properties.
The preparation of formaldehyde-free green adhesive has been achieved, with good water resistance and adhesion effect. It can maintain the bonding of the board layers in humid and high-temperature environments, avoid degumming, and enhance the anti-corrosion performance.
Smart Images

Figure BDA0004777637080000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite board materials, and in particular to a graphene-based ecological composite board and a preparation method thereof. Background Art
[0002] Ecological composite board is also called melamine board. It is a composite material with particle board and blockboard as the base material and paper of different colors and texture patterns as the surface. It is prepared by soaking paper of different colors and texture patterns in melamine resin adhesive and then curing, hot pressing and other processes. Ecological board has the characteristics of beautiful appearance, convenient construction, scratch resistance and wear resistance. Compared with traditional sticker furniture, it also has the characteristics of high temperature resistance, acid and alkali resistance, moisture resistance, fire resistance, etc., and the surface is not easy to change color and peel, and it is easy to be processed into veneers of different styles and strong texture. Therefore, it is loved and recognized by consumers in the market. Panel furniture processed with ecological board as raw material is also widely welcomed and widely used in home decoration, panel furniture, cabinet wardrobe, bathroom cabinet and other fields.
[0003] However, the use of adhesives is inevitable in the process of preparing ecological boards. Traditional urea-formaldehyde resin adhesives have a simple production process and high bonding strength, but since formaldehyde is often used as a raw material in its preparation process, ecological composite boards with urea-formaldehyde resin as a binder often release formaldehyde for a long time, causing great harm to the human body. Summary of the invention
[0004] The object of the present invention is to provide a graphene-based ecological composite board and a preparation method thereof to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0006] Step 1:
[0007] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 10-11 with stirring, stirring continuously for 0.5-1h, and standing for 2-3h; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 2.5-3.5, standing for 10-12h, filtering with suction, washing with water, and drying to obtain purified lignin;
[0008] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 90-100° C., adding stearyl chloride and stirring to mix, reacting for 2-3 hours, pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate;
[0009] S13: dispersing lignin stearate in N,N-dimethylformamide, adding hydrobromic acid, using hexadecyl tributyl phosphonium bromide as a catalyst, catalytically reacting at 100-120° C. for 6-8 hours, distilling off the solvent under reduced pressure, removing N,N-dimethylformamide and hydrobromic acid by pressurized evaporation, extracting with anhydrous ether and acetone, washing with deionized water until neutral, and drying to obtain phenolic lignin stearate;
[0010] S14: dispersing phenolic lignin stearate in N,N-dimethylformamide, dropping into sodium hydroxide solution, adding epichlorohydrin and heating to 75-85° C., reacting for 2-3 hours, and removing impurities by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0011] Step 2:
[0012] S21: mixing epoxidized lignin stearate and bisphenol A epoxy resin to obtain a composite epoxy resin; adding a polyurethane prepolymer and amino graphene to the composite epoxy resin, stirring and reacting at 75-85° C. for 2-4 hours to obtain material A; mixing a curing agent and a curing agent accelerator to obtain material B, and mixing material A and material B evenly according to a ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and vacuum degassing to obtain a graphene adhesive;
[0013] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer in sequence from top to bottom, and bonding the layers together by curing the graphene adhesive to obtain a semi-finished product;
[0014] S23: The melamine facing paper is laminated on both sides of the semi-finished product by a hot pressing process to obtain a graphene-based ecological composite board.
[0015] Furthermore, in step S12, lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:(3.5-4.5).
[0016] Furthermore, in step S13, lignin stearate and hydrobromic acid are reacted in a mass ratio of (8-10):1.
[0017] Furthermore, in S14, the amounts of the components are, by weight, 5 to 8 g of phenolic lignin stearate, 30 to 35 g of sodium hydroxide solution, and 8 to 10 g of epichlorohydrin; wherein the mass fraction of the sodium hydroxide solution is 5 to 6%.
[0018] Furthermore, in S21, the contents of the components in the composite epoxy resin are, by weight, 2 to 4 parts of epoxidized lignin stearate and 8 to 12 parts of bisphenol A epoxy resin.
[0019] Furthermore, in S21, the contents of the components in material A are, by weight percentage, 15-20% of polyurethane prepolymer, 1-1.5% of amino graphene, and the remainder is composite epoxy resin.
[0020] Furthermore, in S21, in material B, the amount of curing agent accelerator used accounts for 1.5-2% of the total weight of material B.
[0021] Furthermore, in S21, material A and material B are mixed in a ratio of 1:1 of epoxy equivalent to active hydrogen equivalent.
[0022] Furthermore, in S22, the core material is any one of fir board and paulownia board, with a thickness of 1 to 1.2 cm; the middle board layer is any one of poplar board and eucalyptus board, with a thickness of 2.5 to 3 mm; the balance layer is technological veneer, with a thickness of 1 to 1.2 mm; the graphene layer formed by curing between the layers has a thickness of 0.5 to 0.7 mm.
[0023] Furthermore, in S22, the curing temperature is 80-85°C, and the curing time is 3-5h.
[0024] Furthermore, in S23, the operating temperature of the hot pressing process is 120-130°C and the pressure is 0.8-1 MPa.
[0025] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention synthesizes a green formaldehyde-free adhesive, the main material of the adhesive is a composite epoxy resin, and the composite epoxy resin is composed of an epoxy resin and epoxidized lignin stearate. Among them, the epoxidized lignin stearate is obtained by taking the biomass material lignin as a raw material through a series of modifications. Since lignin contains a large amount of alcohol hydroxyl and phenolic hydroxyl groups, it can react with stearyl chloride, thereby introducing a hydrophobic segment into lignin to obtain lignin stearate; the hydrophobic stearate segment gives the adhesive a good water-resistant effect, thereby improving the performance of the adhesive in a humid environment. With hexadecyl tributyl phosphonium bromide as a catalyst, hydrobromic acid is used to react with lignin stearate, so that the ether bond in the methoxy group in the lignin stearate is broken to generate a phenolic hydroxyl group, and the newly generated phenolic hydroxyl group reacts with epichlorohydrin to introduce an epoxy group to obtain epoxidized lignin stearate.
[0026] The molecule of epoxidized lignin stearate retains the phenolic structure in lignin and contains epoxy groups, which have certain compatibility with bisphenol A epoxy resin; like adding polyurethane prepolymer to composite epoxy resin, epoxy groups in epoxidized lignin stearate and bisphenol A epoxy resin can react chemically with isocyanate groups in polyurethane prepolymer to form bonds, so the compatibility of the three is good, and the prepared adhesive has strong adhesion. The adhesive prepared by the present invention is applied to ecological composite board, and thanks to the good water resistance and adhesion effect of the adhesive, debonding will not occur between the various board layers of the ecological composite board in a humid and high temperature environment.
[0027] Here, it should be noted that in the above-mentioned process of preparing epoxidized lignin stearate, the reaction steps cannot be changed, and the lignin should be hydrophobically modified first for the following reasons: First, if the methoxy groups in the lignin are first reacted to generate phenolic hydroxyl groups, the amount of reactants needs to be controlled during the subsequent reaction with stearyl chloride to avoid the phenolic hydroxyl groups being completely unable to be epoxidized, and the amount of stearyl chloride reactant directly affects the hydrophobic properties of the product, which increases the workload in the actual synthesis process; and reacting stearyl chloride with lignin first can allow an excess of stearyl chloride to improve the efficiency of the reaction; second, the intermediate product lignin stearate generated by the reaction of stearyl chloride with lignin is solid and contains hydrophobic segments, and has better compatibility with N,N-dimethylformamide. When modified in N,N-dimethylformamide later, the solid powder is easier to disperse, which is also conducive to the reaction.
[0028] The present invention also adds a small amount of aminated graphene to the adhesive. When ordinary graphene is mixed with organic matter, it is easy to agglomerate and has problems such as poor compatibility. However, the surface of the aminated graphene used in the present invention is rich in amino groups and can react with some groups in the adhesive, such as isocyanate groups, so it has better dispersibility and compatibility, can be evenly dispersed in the adhesive, and fill some defects during the curing process of the adhesive. The formed graphene layer is denser than the conventional polymer layer, and can effectively prevent the penetration of water, oxygen and other chemicals, thereby enhancing the corrosion resistance and weather resistance. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Materials used in the present invention and their sources: polyurethane prepolymer comes from Zibo Hengjiu Polyurethane Technology Co., Ltd., item number HJ-1880; bisphenol A epoxy resin is bisphenol A epoxy resin E-51; amino graphene comes from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., item number XF315; curing agent is D230 type polyetheramine curing agent, and curing agent accelerator is DMP-30 type curing accelerator; melamine facing paper comes from Shandong Xingmei Decoration Materials Co., Ltd., item number 9334.
[0031] Embodiment 1: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0032] Step 1:
[0033] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 10 with stirring, stirring continuously for 0.5 h, and standing for 2 h; filtering with suction and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 2.5, standing for 10 h, filtering with suction, washing with water, and drying to obtain purified lignin;
[0034] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 90°C, adding stearyl chloride, stirring and mixing, reacting for 2 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0035] S13: 10 g of lignin stearate was dispersed in N, N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 100°C for 6 h, the solvent was distilled off under reduced pressure, N, N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0036] S14: 8 g of phenolic lignin stearate is dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution is added dropwise, 10 g of epichlorohydrin is added, the temperature is raised to 75° C., the reaction is carried out for 2 h, and impurities are removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0037] Step 2:
[0038] S21: 2kg of epoxidized lignin stearate and 8kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 75°C for 2h to obtain material A; the content of each component in material A is 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene by weight percentage; 100g of curing agent and 2g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0039] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 80°C, and the curing time is 3h; wherein the core material is a fir board with a thickness of 1cm; the middle plate layer is a eucalyptus board with a thickness of 3mm; the balancing layer is a technical veneer with a thickness of 1mm; and the thickness of the graphene layer formed by curing between the layers is 0.5mm;
[0040] S23: At 120° C. and 0.8 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0041] Embodiment 2: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0042] Step 1:
[0043] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 1 hour, and standing for 2.5 hours; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 3, standing for 11 hours, filtering with suction, washing with water, and drying to obtain purified lignin;
[0044] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 95°C, adding stearyl chloride and stirring to mix, reacting for 2.5 hours, pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0045] S13: 10 g of lignin stearate was dispersed in N,N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 100°C for 7.5 h, the solvent was distilled off under reduced pressure, N,N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0046] S14: 8 g of phenolic lignin stearate was dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution was added dropwise, 10 g of epichlorohydrin was added, the temperature was raised to 80°C, the reaction was continued for 2.5 h, and impurities were removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0047] Step 2:
[0048] S21: 2kg of epoxidized lignin stearate and 8kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 80°C for 4h to obtain material A; the content of each component in material A is 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene by weight percentage; 100g of curing agent and 2g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0049] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 85°C, and the curing time is 4 hours; wherein the core material is a fir board with a thickness of 1 cm; the middle plate layer is a eucalyptus board with a thickness of 3 mm; the balancing layer is a technical veneer with a thickness of 1 mm; and the thickness of the graphene layer formed by curing between the layers is 0.5 mm;
[0050] S23: At 125° C. and 0.85 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0051] Embodiment 3: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0052] Step 1:
[0053] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 0.5 h, and standing for 3 h; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 3.5, standing for 12 h, filtering, washing with water, and drying to obtain purified lignin;
[0054] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 100°C, adding stearyl chloride and stirring to mix, reacting for 3 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0055] S13: 10 g of lignin stearate was dispersed in N,N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 120° C. for 8 h, the solvent was distilled off under reduced pressure, N,N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0056] S14: 8 g of phenolic lignin stearate is dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution is added dropwise, 10 g of epichlorohydrin is added, the temperature is raised to 85° C., the reaction is carried out for 3 h, and impurities are removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0057] Step 2:
[0058] S21: 2 kg of epoxidized lignin stearate and 8 kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 75° C. for 3.5 hours to obtain material A; the content of each component in material A is 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene by weight percentage; 100 g of curing agent and 2 g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0059] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 85°C, and the curing time is 5 hours; wherein the core material is a fir board with a thickness of 1 cm; the middle plate layer is a eucalyptus board with a thickness of 3 mm; the balancing layer is a technical veneer with a thickness of 1 mm; and the thickness of the graphene layer formed by curing between the layers is 0.5 mm;
[0060] S23: At 130° C. and 1 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0061] Embodiment 4: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0062] Step 1:
[0063] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 1 hour, and standing for 3 hours; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 2.5, standing for 10 hours, filtering, washing with water, and drying to obtain purified lignin;
[0064] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 90°C, adding stearyl chloride, stirring and mixing, reacting for 2 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0065] S13: 10 g of lignin stearate was dispersed in N,N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 105°C for 6.5 h, the solvent was distilled off under reduced pressure, N,N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0066] S14: 8 g of phenolic lignin stearate was dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution was added dropwise, 10 g of epichlorohydrin was added, the temperature was raised to 80°C, the reaction was continued for 2.5 h, and impurities were removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0067] Step 2:
[0068] S21: 3 kg of epoxidized lignin stearate and 8 kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 80° C. for 2 hours to obtain material A; the content of each component in material A is, by weight percentage, 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene; 100 g of curing agent and 2 g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0069] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 80°C, and the curing time is 3h; wherein the core material is a fir board with a thickness of 1cm; the middle plate layer is a eucalyptus board with a thickness of 3mm; the balancing layer is a technical veneer with a thickness of 1mm; and the thickness of the graphene layer formed by curing between the layers is 0.5mm;
[0070] S23: At 125° C. and 1 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0071] Embodiment 5: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0072] Step 1:
[0073] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 1 hour, and standing for 2.5 hours; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 3, standing for 12 hours, filtering, washing with water, and drying to obtain purified lignin;
[0074] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 100°C, adding stearyl chloride and stirring to mix, reacting for 2.5 hours, pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0075] S13: 10 g of lignin stearate was dispersed in N,N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 120° C. for 7.5 h, the solvent was distilled off under reduced pressure, N,N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0076] S14: 8 g of phenolic lignin stearate is dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution is added dropwise, 10 g of epichlorohydrin is added, the temperature is raised to 85° C., the reaction is carried out for 3 h, and impurities are removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0077] Step 2:
[0078] S21: 3.5 kg of epoxidized lignin stearate and 8 kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 80° C. for 3 hours to obtain material A; the content of each component in material A is, by weight percentage, 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene; 100 g of curing agent and 2 g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0079] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer in turn from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 85°C, and the curing time is 4.5h; wherein the core material is a fir board with a thickness of 1cm; the middle plate layer is a eucalyptus board with a thickness of 3mm; the balancing layer is a technical veneer with a thickness of 1mm; and the thickness of the graphene layer formed by curing between the layers is 0.5mm;
[0080] S23: At 125° C. and 0.9 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0081] Embodiment 6: A graphene-based ecological composite board and a preparation method thereof, comprising the following steps:
[0082] Step 1:
[0083] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 1 hour, and standing for 2.5 hours; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 3, standing for 12 hours, filtering, washing with water, and drying to obtain purified lignin;
[0084] S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 95°C, adding stearyl chloride, stirring and mixing, reacting for 3 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0085] S13: 10 g of lignin stearate was dispersed in N,N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 115°C for 7.5 h, the solvent was distilled off under reduced pressure, N,N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin stearate;
[0086] S14: 8 g of phenolic lignin stearate was dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution was added dropwise, 10 g of epichlorohydrin was added, the temperature was raised to 80°C, the reaction was continued for 2.5 h, and impurities were removed by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate;
[0087] Step 2:
[0088] S21: 4 kg of epoxidized lignin stearate and 8 kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 85° C. for 3 hours to obtain material A; the content of each component in material A is, by weight percentage, 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene; 100 g of curing agent and 2 g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0089] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 85°C, and the curing time is 5 hours; wherein the core material is a fir board with a thickness of 1 cm; the middle plate layer is a eucalyptus board with a thickness of 3 mm; the balancing layer is a technical veneer with a thickness of 1 mm; and the thickness of the graphene layer formed by curing between the layers is 0.5 mm;
[0090] S23: At 130° C. and 1 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0091] Comparative Example 1: No epoxidized lignin stearate was added, and other parameters were the same as those in Example 1.
[0092] S1: Add polyurethane prepolymer and amino graphene to bisphenol A epoxy resin by weight percentage, and stir the mixture at 75°C for 2h to obtain material A; in material A, the content of each component by weight percentage is 80% bisphenol A epoxy resin, 19% polyurethane prepolymer, and 1% amino graphene; 100g curing agent and 2g curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0093] S2: From top to bottom, the balance layer, middle plate layer, core material, middle plate layer, and balance layer are assembled in sequence, and the layers are cured and bonded by graphene adhesive to obtain a semi-finished product. The curing temperature is 80°C and the curing time is 3h. Among them, the core material is fir board with a thickness of 1cm; the middle plate layer is eucalyptus board with a thickness of 3mm; the balance layer is technical wood veneer with a thickness of 1mm; the thickness of the graphene layer formed by curing between the layers is 0.5mm;
[0094] S3: At 120°C and 0.8MPa, 1.5mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0095] Comparative Example 2: The reaction order of S12 and S13 in Example 2 was changed.
[0096] Step 1:
[0097] S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution to adjust the pH value of the system to 11 with stirring, stirring for 1 hour, and standing for 2.5 hours; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 3, standing for 11 hours, filtering with suction, washing with water, and drying to obtain purified lignin;
[0098] S12: 10 g of purified lignin stearate was dispersed in N, N-dimethylformamide, 1 g of hydrobromic acid was added, hexadecyl tributyl phosphonium bromide was used as a catalyst, the reaction was carried out at 100°C for 7.5 h, the solvent was distilled off under reduced pressure, N, N-dimethylformamide and hydrobromic acid were removed by pressurized evaporation, anhydrous ether and acetone were used for extraction, the mixture was washed with deionized water until neutral, and the mixture was dried to obtain phenolic lignin;
[0099] S13: adding phenolic lignin to anhydrous pyridine, heating the oil bath to 95°C, adding stearyl chloride and stirring to mix, reacting for 2.5 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the phenolic lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:4;
[0100] S14: 8 g of lignin stearate was dispersed in N,N-dimethylformamide, 30 g of 6% sodium hydroxide solution was added dropwise, 10 g of epichlorohydrin was added, the temperature was raised to 80°C, the reaction was carried out for 2.5 h, and impurities were removed by vacuum distillation and centrifugal washing to obtain modified lignin;
[0101] Step 2:
[0102] S21: 2 kg of modified lignin and 8 kg of bisphenol A epoxy resin are mixed to obtain a composite epoxy resin; polyurethane prepolymer and amino graphene are added to the composite epoxy resin by weight percentage, and the mixture is stirred and reacted at 80° C. for 4 hours to obtain material A; the content of each component in material A is, by weight percentage, 80% of composite epoxy resin, 19% of polyurethane prepolymer, and 1% of amino graphene; 100 g of curing agent and 2 g of curing agent accelerator are mixed to obtain material B, and material A and material B are evenly mixed according to the ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and then vacuum degassing is performed to obtain a graphene adhesive;
[0103] S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer from top to bottom, and curing and bonding the layers together to obtain a semi-finished product, the curing temperature is 85°C, and the curing time is 4 hours; wherein the core material is a fir board with a thickness of 1 cm; the middle plate layer is a eucalyptus board with a thickness of 3 mm; the balancing layer is a technical veneer with a thickness of 1 mm; and the thickness of the graphene layer formed by curing between the layers is 0.5 mm;
[0104] S23: At 125° C. and 0.85 MPa, 1.5 mm thick melamine facing paper is hot-pressed and laminated on both sides of the semi-finished product to obtain a graphene-based ecological composite board.
[0105] Experiment: The adhesives prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were tested, wherein:
[0106] Hydrophilic and hydrophobic performance test: Apply the adhesive on the surface of the fir board, solidify it to form a coating, and test the contact angle between the water surface and the coating;
[0107] Adhesion performance test: refer to GB / T 7124-2008, use 2A12-T4 aluminum alloy as the substrate, use a universal testing machine to measure, each group of parallel samples has 5, and the average value is calculated; the test samples are placed in a dry environment at 25°C (30% air humidity), in deionized water at 25°C, and in boiling deionized water for 12 hours to test their shear strength.
[0108]
[0109] Conclusion: The data of Examples 1 to 6 show that the adhesive prepared by the present invention has good hydrophobic properties, and has excellent moisture resistance and high temperature resistance, and can still maintain good bonding properties in a high temperature water environment. The data of Example 1 and Comparative Example 1 show that the epoxidized lignin stearate prepared by the present invention has good compatibility with bisphenol A epoxy resin and polyurethane prepolymer, so the shear strength of the adhesive is high and the bonding effect is good; the data of Example 2 and Comparative Example 2 show that the modified lignin prepared by changing the order of S12 and S13 has poor compatibility with the main resin of the adhesive, and the performance of the adhesive after adding is therefore poorly modified, and the performance of each data is lower than that of Example 2; and combined with the data of Comparative Examples 1 and 2, it can be seen that the addition of the modified lignin prepared in Comparative Example 2 produces a negative effect.
[0110] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of an ecological composite board based on graphene, characterized in that: The following steps are involved: Step 1: S11: dispersing the alkali lignin in deionized water, adding sodium hydroxide solution while stirring to adjust the pH value of the system to 10-11, stirring continuously for 0.5-1h, and standing for 2-3h; filtering and adding dilute hydrochloric acid to the filtrate to adjust the pH value to 2.5-3.5, standing for 10-12h, filtering, washing with water, and drying to obtain purified lignin; S12: adding purified lignin to anhydrous pyridine, heating the oil bath to 90-100°C, adding stearyl chloride and stirring to mix, reacting for 2-3 hours, and then pouring the reaction mixture into ethanol to terminate the reaction; centrifuging and separating the sediment, dissolving it with tetrahydrofuran, and then precipitating and purifying it with n-hexane, and vacuum drying to obtain lignin stearate; wherein the lignin and stearyl chloride are mixed at a molar ratio of hydroxyl group to acyl chloride group of 1:(3.5-4.5); S13: dispersing lignin stearate in N,N-dimethylformamide, adding hydrobromic acid, using hexadecyl tributyl phosphonium bromide as a catalyst, catalytically reacting at 100-120°C for 6-8h, removing the solvent by vacuum distillation, removing N,N-dimethylformamide and hydrobromic acid by pressurized evaporation, extracting with anhydrous ether and acetone, washing with deionized water until neutral, and drying to obtain phenolic lignin stearate; wherein the lignin stearate and hydrobromic acid react at a mass ratio of (8-10):1; S14: dispersing phenolic lignin stearate in N,N-dimethylformamide, dropping into sodium hydroxide solution, adding epichlorohydrin and heating to 75-85°C, reacting for 2-3 hours, and removing impurities by vacuum distillation and centrifugal washing to obtain epoxidized lignin stearate; Step 2: S21: mixing epoxidized lignin stearate and bisphenol A epoxy resin to obtain a composite epoxy resin; adding a polyurethane prepolymer and amino graphene to the composite epoxy resin, stirring and reacting at 75-85° C. for 2-4 hours to obtain material A; mixing a curing agent and a curing agent accelerator to obtain material B, and mixing material A and material B evenly according to a ratio of epoxy equivalent to active hydrogen equivalent of 1:1, and vacuum degassing to obtain a graphene adhesive; S22: assembling the balancing layer, the middle plate layer, the core material, the middle plate layer, and the balancing layer in sequence from top to bottom, and bonding the layers together by curing the graphene adhesive to obtain a semi-finished product; S23: The melamine facing paper is laminated on both sides of the semi-finished product by a hot pressing process to obtain a graphene-based ecological composite board.
2. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S14, the amount of each component is 5-8 g of phenolic lignin stearate, 30-35 g of sodium hydroxide solution, and 8-10 g of epichlorohydrin; wherein the mass fraction of the sodium hydroxide solution is 5-6%.
3. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S21, the content of each component in the composite epoxy resin is, by weight, 2 to 4 parts of epoxidized lignin stearate and 8 to 12 parts of bisphenol A epoxy resin.
4. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S21, the content of each component in material A, by weight percentage, is 15-20% polyurethane prepolymer, 1-1.5% amino graphene, and the remainder is composite epoxy resin; in material B, the amount of curing agent accelerator accounts for 1.5-2% of the total weight of material B; material A and material B are mixed in a ratio of 1:1 of epoxy equivalent to active hydrogen equivalent.
5. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S22, the core material is any one of fir board and paulownia board, with a thickness of 1~1.2cm; the middle board layer is any one of poplar board and eucalyptus board, with a thickness of 2.5~3mm; the balance layer is technological veneer, with a thickness of 1~1.2mm; the graphene layer formed by curing between the layers has a thickness of 0.5~0.7mm.
6. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S22, the curing temperature is 80-85°C and the curing time is 3-5h.
7. The preparation process of a graphene-based ecological composite board according to claim 1, characterized in that: In S23, the operating temperature of the hot pressing process is 120~130°C and the pressure is 0.8~1MPa.
8. The ecological composite board prepared by the preparation process according to any one of claims 1 to 7.
Citation Information
Patent Citations
Preparation method of environment-friendly ecological board
CN105291540A
Waterproof lignin-based epoxy resin adhesive and preparation method thereof
CN112126391A