A method for preparing glass fiber using construction waste and waste incineration fly ash

By mixing waste incineration fly ash and construction waste with sodium carbonate and performing high-temperature melting and drawing processes, corrosion-resistant and high-temperature-resistant glass fibers are prepared, which solves the problem of waste incineration fly ash and construction waste disposal and reduces the cost of glass fiber production. , and realized resource utilization.

CN118388141BActive Publication Date: 2024-10-22NORTH CHINA UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410687213.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-10-22
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

It is difficult to effectively process and utilize waste incineration fly ash and construction waste with existing technology, and the cost of glass fiber production process is high, making it difficult to meet market demand.

Method used

Waste incineration fly ash and construction waste are mixed with sodium carbonate, and glass fiber is prepared through high-temperature melting and drawing processes. Secondary fly ash is captured during the melting process to reduce energy consumption and improve the performance of the glass fiber.

Benefits of technology

The preparation of corrosion-resistant and high-temperature-resistant glass fiber reduces production costs, realizes the resource utilization of two types of solid waste, achieves the purpose of treating waste with waste, and improves the strength and chemical stability of the glass fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118388141B_ABST
    Figure CN118388141B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing glass fiber using construction waste and waste incineration fly ash. A method for preparing glass fiber using construction waste and waste incineration fly ash, comprising the following steps: mixing waste incineration fly ash, crushed construction waste and sodium carbonate to obtain a mixture, placing the mixture in a muffle furnace for melting and heat preservation, during which the mixture becomes glass liquid; during the heat preservation process, the flue gas is captured to obtain secondary fly ash; after the heat preservation is completed, the glass liquid is poured into a wire drawing machine for wire drawing, and during the wire drawing cooling process, an impregnating agent is quickly sprayed to obtain a glass fiber coated with an impregnating agent; the glass fiber coated with an impregnating agent is preheated and dried to obtain a glass fiber. The glass fiber prepared by the present invention is mainly a medium-alkali glass fiber of the SiO2-Al2O3-CaO-MgO system, which has high strength, good corrosion resistance and chemical stability, and is a green, low-carbon, environmentally friendly glass fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing glass fiber by utilizing construction waste and waste incineration fly ash. Background Art

[0002] At present, the main methods of domestic waste treatment in my country are landfill, incineration and composting. In comparison, incineration has gradually become the main way to treat domestic waste due to its advantages of reducing the amount and volume, high degree and the use of heat generated by combustion.

[0003] Waste incineration fly ash refers to fine particles collected by air pollution equipment, and neutralized reactants collected by cyclone dust collectors, electrostatic precipitators or bag filters. The waste incineration fly ash produced by grate incinerators accounts for 3-5% of the amount of domestic waste incinerated; the waste incineration fly ash produced by fluidized bed incinerators accounts for more than 10% of the amount of domestic waste incinerated. Waste incineration fly ash is defined as hazardous waste because it gathers pollutants generated by waste incineration, mainly heavy metals and dioxins. Therefore, the proper disposal and utilization of incineration fly ash has become an urgent problem to be solved.

[0004] Construction waste refers to construction waste generated in projects due to human or natural reasons, including waste soil, abandoned soil, silt and abandoned materials. With the accelerated development of urbanization in my country, the amount of construction waste is increasing, and it is urgent to improve the processing capacity of construction waste.

[0005] As a multifunctional material, glass fiber plays a vital role in the fields of construction, aerospace, automotive industry, electronic equipment, environmental protection, etc. With the continuous development of technology and market, manufacturers are constantly facing the pressure of improving competitiveness, reducing costs and improving quality. In order to meet these challenges, the optimization of glass fiber production process technology has become an urgent task.

[0006] Therefore, there is an urgent need to provide a technical solution to the above-mentioned deficiencies in the prior art. Summary of the invention

[0007] The purpose of the present invention is to provide a method for preparing glass fiber by using construction waste and fly ash from garbage incineration, wherein the two solid wastes, construction waste and garbage incineration, are processed in a coordinated manner to prepare glass fiber, which is corrosion-resistant and high-temperature-resistant and can be used as fiber concrete, refractory materials, etc. The method can reduce the preparation cost of glass fiber, and at the same time realize the resource utilization of the two solid wastes, thereby achieving the purpose of treating waste with waste.

[0008] In order to achieve the above objectives, this application provides the following technical solutions:

[0009] A method for preparing glass fiber using construction waste and waste incineration fly ash, comprising the following steps:

[0010] (1) mixing fly ash from garbage incineration, crushed construction waste and sodium carbonate to obtain a mixture, placing the mixture in a crucible, and then placing the crucible in a muffle furnace for melting and heat preservation. During the heat preservation process, the mixture becomes a glass liquid;

[0011] (2) During the heat preservation process, the flue gas is captured to obtain secondary fly ash;

[0012] (3) After the insulation is completed, the crucible is taken out and the glass liquid is poured into a wire drawing machine for wire drawing. During the cooling process of the wire drawing, the impregnating agent is quickly sprayed to obtain glass fibers coated with the impregnating agent; the glass fibers coated with the impregnating agent are preheated and dried to obtain glass fibers.

[0013] Preferably, in step (1), the mass percentage of the waste incineration fly ash is 20-50%, the mass percentage of the crushed construction waste is 40-70%, the mass percentage of the sodium carbonate is 0-10%, and the particle size of the crushed construction waste is -200 mesh ≥ 80%.

[0014] Further preferably, in step (1), the mixture is placed in a corundum or graphite crucible, and then the crucible is placed in a muffle furnace, the temperature of the muffle furnace is increased to 1100-1300°C at 3-6°C per minute, and the mixture is melted and kept warm for 50-100 minutes. During the melting and keeping warm process, the mixture becomes molten glass.

[0015] Preferably, in step (2), the flue gas is captured during the melting and heat preservation process to obtain secondary fly ash mainly composed of NaCl and KCl, and the sum of the percentages of NaCl and KCl is ≥ 60%.

[0016] Preferably, in step (3), the wire drawing temperature is 900-1100°C, and the wire drawing diameter is 8-15 μm.

[0017] Further preferably, in step (3), the preheating temperature is 110-120°C, and the preheating time is 1-2.5 hours; the drying temperature is 120-135°C, and the drying time is 6-15 hours.

[0018] Preferably, the construction waste includes waste concrete, slag, and waste bricks; the main components of the construction waste are: CaO 10-40%, SiO 2 25~70%,Al 2 O 3 10~20%, MgO 4~10%, Na 2 O 0.1~5%, SO 2 0.01~1%.

[0019] Preferably, the main components of the waste incineration fly ash are: CaO 30-50%, C 5-12%, SiO 2 0.1~15%,Al 2 O 3 0.1~10%, Cl 5~25%, Na 2 O 0.1~10%, K 2 O 0.1~10%, MgO 0.1~10%, Fe 2 O 3 0.1~10%, SO 3 0.1~5%,TiO 2 0~3%, P 2 O 5 0~5%, ZnO 0~1%, PbO 0~1%, Cr 2 O 3 0~1%, CuO 0~1%, MnO 0~1%, NiO 0~1%, BaO 0~1%, SrO 0~1%, CdO 0~1%.

[0020] Preferably, the sizing agent is at least one of vinyl triethoxysilane, methacryloxy functional silane, and vinyl trimethoxy silane, among which vinyl triethoxy silane (A151), methacryloxy functional silane (kh-570), and vinyl trimethoxy silane (A171).

[0021] Beneficial effects:

[0022] The present invention uses two kinds of solid waste, waste incineration fly ash and construction waste, adds sodium carbonate as an additive, and prepares glass fiber with similar performance to traditional glass fiber through high-temperature melting, wire drawing and other processes. The glass fiber prepared by waste incineration fly ash and construction waste in the present invention is mainly SiO 2 -Al 2 O 3 -CaO-MgO system of medium-alkali glass fiber, this kind of glass fiber has high strength, corrosion resistance and good chemical stability. Waste incineration fly ash also contains a small amount of metals, such as Fe, Cr, Cu, etc. The presence of these substances can improve the performance of glass fiber to a certain extent. The present invention can save natural stone, and has a relatively low melting temperature, reducing energy consumption. It is a green, low-carbon and environmentally friendly glass fiber. The present invention also recovers the chlorides of Na, K and other substances in the fly ash. During the high-temperature melting process, the flue gas is captured by chlorination volatilization to obtain secondary fly ash. The secondary fly ash is mainly composed of NaCl and KCl, and the content of both exceeds 60%, which can be used as a snow melting agent, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The drawings constituting part of the present application are used to provide a further understanding of the present application. The exemplary embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. Among them:

[0024] Figure 1 This is a flow chart of Embodiment 1 of the present invention;

[0025] Figure 2 is the XRD pattern of the glass fiber in Example 1 of the present invention;

[0026] Figure 3 This is a scanning electron microscope image of the glass fiber in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The present application will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments. Each example is provided by way of explanation of the present application and does not limit the present application. In fact, it will be clear to those skilled in the art that modifications and variations may be made in the present application without departing from the scope or spirit of the present application. For example, a feature shown or described as a part of an embodiment may be used in another embodiment to produce yet another embodiment. All other embodiments obtained by those of ordinary skill in the art based on the embodiments in the embodiments of the present invention should belong to the scope of protection of the embodiments of the present invention.

[0028] Example 1

[0029] A method for preparing glass fiber using construction waste and waste incineration fly ash, comprising the following steps:

[0030] First, the construction waste is crushed to a particle size of -200 mesh, accounting for 87%; then 25% of waste incineration fly ash, 65% of construction waste and 10% of sodium carbonate are mixed to obtain a mixture; then, the mixture is placed in a crucible, the crucible is placed in a muffle furnace, and the temperature is raised to a melting temperature of 1100°C at a rate of 3°C per minute for melting and heat preservation for 100 minutes. During the melting and heat preservation process, the mixture becomes a glass liquid. After the insulation is completed, the crucible is quickly taken out, and the glass liquid is poured into the wire drawing machine for wire drawing, wherein the wire drawing temperature is 1100°C and the diameter after wire drawing is 9.26μm. During the wire drawing cooling process, the impregnating agent kh-570 is quickly sprayed to obtain a glass fiber coated with an impregnating agent. The glass fiber coated with the impregnating agent is first preheated at a preheating temperature of 110°C for a preheating time of 2.5h, and then dried at 120°C for 15h to obtain glass fiber, which is chopped after drying and subjected to relevant new energy tests. During the melting and heat preservation process, the flue gas is captured to obtain secondary fly ash, which contains 45.12% NaCl and 37.58% KCl. The flow chart is as follows: Figure 1 The main components of construction waste are: CaO 18.71%, SiO 250.31%,Al 2 O 3 14.58%, MgO 7.54%, Na 2 O 1.23%, SO 2 0.05%.

[0031] The main components of waste incineration fly ash are: CaO 37.23%, C 9.55%, Cl 17.23%, SiO 2 8.81%, MgO3.51%, Al 2 O 3 2.87%,Fe 2 O 3 4.33%, SO 3 2.57%, K 2 O 5.12%, Na 2 O 3.13%, ZnO 0.43%, TiO 2 0.32%,P 2 O 5 0.31%, PbO 0.17%, CuO 0.03%, NiO 0.04%, Cr 2 O 3 0.05%, SrO 0.03%, MnO 0.02%.

[0032] The physical and chemical properties of glass fiber are shown in Table 1.

[0033] Example 2

[0034] A method for preparing glass fiber using construction waste and waste incineration fly ash, comprising the following steps:

[0035] The construction waste is crushed to a particle size of -200 mesh, accounting for 92%; then 50% of the waste incineration fly ash, 47% of the construction waste and 3% of the sodium carbonate are mixed to obtain a mixture; then, the mixture is placed in a crucible, the crucible is placed in a muffle furnace, and the temperature is raised to a melting temperature of 1200°C at a rate of 5°C per minute, and the melting is kept warm for 80 minutes. During the melting and heat preservation process, the mixture becomes a glass liquid. After the insulation is completed, the crucible is quickly taken out, and the glass liquid is poured into the wire drawing machine for wire drawing, wherein the wire drawing temperature is 900°C and the diameter after wire drawing is 11.53μm. During the wire drawing cooling process, the impregnant A151 is quickly sprayed to obtain a glass fiber coated with the impregnant. The glass fiber coated with the impregnant is first preheated at a preheating temperature of 115°C for a preheating time of 2h, and then dried at 130°C for 9h to obtain the glass fiber, which is chopped after drying and subjected to relevant new energy tests. During the melting and heat preservation process, the flue gas is captured to obtain secondary fly ash, which contains 33.89% NaCl and 28.67% KCl. The main components of construction waste are: CaO 12.15%, SiO 2 63.34%,Al 2 O 3 10.22%, MgO 8.29%, Na 2 O 1.63%, SO 2 0.14%.

[0036] The main components of waste incineration fly ash are: CaO 47.26%, C 6.2%, Cl 14.61%, SiO 2 4.53%, MgO2.87%, Al 2 O 3 1.68%,Fe 2 O 3 2.89%, SO 3 4.28%, K 2 O 5.17%, Na 2 O 3.18%, ZnO 0.85%, TiO 2 0.43%, P 2 O 5 0.39%, PbO 0.17%, CuO 0.05%, NiO 0.07%, Cr 2 O 3 0.04%, SrO 0.03%, MnO 0.11%.

[0037] The physical and chemical properties of glass fiber are shown in Table 1.

[0038] Example 3

[0039] A method for preparing glass fiber using construction waste and waste incineration fly ash, comprising the following steps:

[0040] The construction waste is crushed to a particle size of -200 mesh, accounting for 82%, and then 35% of waste incineration fly ash, 59% of construction waste and 6% of sodium carbonate are mixed to obtain a mixture; the mixture is placed in a crucible, and the crucible is placed in a muffle furnace, and the temperature is raised to a melting temperature of 1300°C at a rate of 6°C per minute, and the melting is kept warm for 50 minutes. During the melting and heat preservation process, the mixture becomes a glass liquid. After the insulation is completed, the crucible is quickly taken out, and the glass liquid is poured into the wire drawing machine for wire drawing. The wire drawing temperature is 1000°C, and the diameter after wire drawing is 10.12μm; during the wire drawing cooling process, the impregnant A171 is quickly sprayed to obtain a glass fiber coated with an impregnant. The glass fiber coated with the impregnant is first preheated at a preheating temperature of 120°C and a preheating time of 1h, and then dried at 135°C for 6h to obtain glass fiber, which is chopped after drying and subjected to relevant new energy tests. During the melting and heat preservation process, the flue gas is captured to obtain secondary fly ash, which contains 48.18% NaCl and 42.33% KCl. The main components of construction waste are: CaO24.19%, SiO 2 46.33%,Al 2 O 3 19.35%, MgO 4.13%, Na 2 O 2.71%, SO 2 0.08%.

[0041] The main components of waste incineration fly ash are: CaO 33.59%, C 11.67%, Cl 12.56%, SiO 2 13.12%, MgO1.59%, Al 2 O 3 4.38%,Fe 2 O 3 6.17%, SO 3 1.89%, K 2 O 4.61%, Na 2 O 5.08%, ZnO 0.29%, TiO 2 0.33%,P 2 O 5 0.48%, PbO 0.17%, CuO 0.08%, NiO 0.05%, Cr 2 O 3 0.11%, CdO 0.02%, Sb 2 O 3 0.03%, MnO 0.05%.

[0042] The physical and chemical properties of glass fiber are shown in Table 1.

[0043] Acid and alkali resistance test method: Acid and alkali resistance tests are performed using sulfuric acid (H 2 SO 4 ) as the acid source and sodium hydroxide (NaOH) as the alkali source, prepare 0.5 mol / L sulfuric acid solution and 1 mol / L sodium hydroxide solution in a volumetric flask at 25°C in proportion. Put the glass body, glass fiber and glass fiber filaments into the sulfuric acid solution respectively, weigh their initial mass and mass after immersion for 48 hours, and use the difference in mass before and after acid immersion as the acid erosion loss.

[0044] Table 1 Physical and chemical properties of glass fiber

[0045]

[0046] It can be seen from Table 1 that the glass fiber prepared by this process has higher tensile strength, better elongation, and better acid and alkali resistance.

[0047] Depend on Figure 2 It can be seen that the obtained glass fiber is mainly composed of amorphous diffraction peaks, indicating that it is mainly composed of a non-crystalline glass structure.

[0048] Depend on Figure 3 It can be seen that the surface of glass fiber is smooth and the fineness is about 10μm.

[0049] The present invention utilizes two solid wastes, namely, garbage incineration fly ash and construction waste, adds an additive of sodium carbonate, and prepares glass fibers having similar properties to traditional glass fibers through processes such as high-temperature melting and drawing. The glass fibers prepared by the present invention have high strength, good corrosion resistance and good chemical stability. Garbage incineration fly ash also contains a small amount of metals, such as Fe, Cr, Cu, etc., which can improve the performance of glass fibers to a certain extent.

[0050] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" mean that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0051] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing glass fiber using construction waste and waste incineration fly ash, characterized in that: The following steps are involved: (1) Mix waste incineration fly ash, crushed construction waste and sodium carbonate to obtain a mixture, put the mixture into a corundum or graphite crucible, and then put the crucible into a muffle furnace. The muffle furnace is heated to 1100-1300°C at 3-6°C per minute, and the mixture is melted and kept warm for 50-100 minutes. During the melting and heat preservation process, the mixture becomes glass liquid; (2) During the heat preservation process, the flue gas is captured to obtain secondary fly ash; (3) After the insulation is completed, the crucible is taken out and the glass liquid is poured into a wire drawing machine for wire drawing. During the cooling process of the wire drawing, the impregnating agent is quickly sprayed to obtain glass fibers coated with the impregnating agent; the glass fibers coated with the impregnating agent are preheated and dried to obtain glass fibers.

2. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 1, characterized in that: In step (1), the mass percentage of the waste incineration fly ash is 20-50%, the mass percentage of the crushed construction waste is 40-70%, the mass percentage of the sodium carbonate is 0-10%, and the particle size of the crushed construction waste is -200 mesh ≥ 80%.

3. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 1, characterized in that: In step (2), the flue gas is captured during the melting and heat preservation process to obtain secondary fly ash mainly composed of NaCl and KCl, and the sum of the percentages of NaCl and KCl is ≥ 60%.

4. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 1, characterized in that: In step (3), the wire drawing temperature is 900-1100°C, and the wire drawing diameter is 8-15 μm.

5. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 4, characterized in that: In step (3), the preheating temperature is 110-120°C, and the preheating time is 1-2.5 hours; the drying temperature is 120-135°C, and the drying time is 6-15 hours.

6. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to any one of claims 1 to 5, characterized in that: The construction waste includes waste concrete, slag and waste bricks; the main components of the construction waste are: CaO 10-40%, SiO2 25-70%, Al2O3 10-20%, MgO 4-10%, Na2O 0.1-5%, P2O5 1-5%, SO2 0.01-1%.

7. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 6, characterized in that: The main components of the waste incineration fly ash are: CaO 30-50%, C 5-12%, SiO2 0.1-15%, Al2O3 0.1-10%, Cl 5-25%, Na2O 0.1-10%, K2O 0.1-10%, MgO 0.1-10%, Fe2O3 0.1-10%, SO3 0.1-5%, TiO2 0-3%, P2O5 0-5%, ZnO 0-1%, PbO 0-1%, Cr2O3 0-1%, CuO 0-1%, MnO 0-1%, NiO 0-1%, BaO 0-1%, SrO 0-1%, and CdO 0-1%.

8. The method for preparing glass fiber by using construction waste and waste incineration fly ash according to claim 6, characterized in that: The wetting agent is at least one of vinyl triethoxy silane, methacryloxy functional silane and vinyl trimethoxy silane.