A composite material of polyurethane resin for pultrusion and preparation method thereof

By adding modified aerogel and nano-expanded graphite to the pultrusion polyurethane resin and adopting specific pretreatment technology, the problem of insufficient mechanical properties of existing resin materials is solved, and high strength, toughness and pressure resistance are achieved. Composite material preparation.

CN118388951BActive Publication Date: 2024-12-03NMG ADVANCED MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410641060.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-12-03
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

The existing pultrusion resins, such as unsaturated polyester, epoxy resin and polyurethane resin, each have insufficient performance, poor mechanical properties, and are expensive or prone to aging.

Method used

Using a composite material, including reinforcing fibers and modified polyurethane resins, the latter consisting of isocyanates, polymer polyols, catalysts, antioxidants, anti-UV agents, chain growth agents, modified aerogels and nanoexpanded graphite. And improve the binding performance of fiber and aerogel by specific proportions and process treatments, such as lignin derivative infiltration pretreatment and bacterial cellulose fermentation pretreatment.

Benefits of technology

It achieves rapid molding, improves the mechanical strength and toughness of composite materials, enhances its pressure resistance, flexibility and self-lubricity, fills the internal pore structure, and significantly improves the overall mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118388951B_ABST
    Figure CN118388951B_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of polyurethane resin for pultrusion, and provides a composite material of polyurethane resin for pultrusion and a preparation method thereof. The composite material comprises reinforcing fiber and polyurethane resin, and the polyurethane resin comprises the following raw materials: isocyanate, polymer polyol, catalyst, dewatering agent, antioxidant, anti-ultraviolet agent, chain extender, release agent, modified aerogel, modified polyethylene glycol, and nano-expanded graphite. The invention forms crosslinks between isocyanate and polymer polyol to enhance mechanical strength, and improves the connection performance of the composite material interface by adding modified aerogel. Meanwhile, the modified aerogel can improve the mechanical properties of the composite material, and the modified polyethylene glycol is added to closely combine with the reinforcing fiber to improve the mechanical properties of the composite material, and the nano-expanded graphite is added to expand the volume of the composite material at high temperature during pultrusion molding, effectively fill the internal pore structure of the composite material, and further improve the mechanical properties of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyurethane resin for pultrusion, and in particular relates to a composite material of polyurethane resin for pultrusion and a preparation method thereof. Background Art

[0002] Pultruded composite materials are made of various resins and high-performance fibers through pultrusion. Existing pultrusion resins include unsaturated polyester, epoxy resin, polyurethane, etc. Unsaturated polyester has poor mechanical properties; epoxy resin is a high-performance resin, but it is expensive and has a slow curing speed. In addition, due to its high cross-linking rate, the material is hard and brittle, and has insufficient toughness; polyurethane resin has relatively poor toughness, is weak in the ability to withstand impact, and is more prone to aging. Summary of the invention

[0003] The present invention provides a composite material of polyurethane resin for pultrusion, aiming to solve the above problems.

[0004] The present invention is achieved in this way. A composite material of polyurethane resin for pultrusion comprises reinforcing fibers and polyurethane resin. The polyurethane resin comprises the following raw materials in parts by weight: 150-250 parts of isocyanate, 90-110 parts of polymer polyol, 0.2-1 parts of catalyst, 1-3 parts of dewatering agent, 1-3 parts of antioxidant, 1-3 parts of anti-ultraviolet agent, 1-5 parts of chain extender, 1-5 parts of release agent, 3-7 parts of modified aerogel, 2-6 parts of modified polyethylene glycol and 1-5 parts of nano-expanded graphite.

[0005] Preferably, the polyurethane resin comprises the following raw materials in parts by weight: 180-220 parts of isocyanate, 95-105 parts of polymer polyol, 0.4-0.8 parts of catalyst, 1.5-2.5 parts of dewatering agent, 1.5-2.5 parts of antioxidant, 1.5-2.5 parts of anti-ultraviolet agent, 2-4 parts of chain extender, 2-4 parts of release agent, 4-6 parts of modified aerogel, 3-5 parts of modified polyethylene glycol, and 2-4 parts of nano-expanded graphite.

[0006] Preferably, the polyurethane resin comprises the following raw materials in parts by weight: 200 parts of isocyanate, 100 parts of polymer polyol, 0.6 parts of catalyst, 2 parts of dehydrating agent, 2 parts of antioxidant, 2 parts of anti-ultraviolet agent, 3 parts of chain extender, 3 parts of release agent, 5 parts of modified aerogel, 4 parts of modified polyethylene glycol, and 3 parts of nano-expanded graphite.

[0007] Preferably, the reinforcing fiber accounts for 70-85% of the total weight of the composite material, and the polyurethane resin accounts for 15-30% of the total weight of the composite material.

[0008] Preferably, the reinforcing fibers include one or more combinations of glass fibers, carbon fibers, and aramid fibers. The reinforcing fibers are pretreated by impregnation with an aqueous solution of a lignin derivative having a mass percentage concentration of 40-60% before use. The mechanical properties of the reinforcing fibers are further improved by impregnating the reinforcing fibers with an aqueous solution of a lignin derivative.

[0009] Preferably, the polymer polyol includes one or more combinations of polyether diols, polyether triols, polyester diols, and polyester triols; the catalyst includes one or more combinations of organic metal tin, organic metal mercury, and organic metal bismuth; the dehydrating agent includes a carbodiimide dehydrating agent; the antioxidant includes one or more combinations of hindered phenol antioxidants and phosphite antioxidants; and the release agent includes one or more combinations of stearic acid, paraffin powder, and polyether silicone oil.

[0010] Preferably, the preparation method of the modified aerogel is as follows: 15-20 parts by weight of silica aerogel are taken, vacuumed and calcined first, and then cooled to form nano-scale particles, and 50-60 parts of dopamine hydrochloric acid solution with a concentration of 5-10 mg / ml are added, and the modified aerogel is obtained after drying with a microwave drying device; first, the moisture and volatile impurities in the silica aerogel are removed by vacuuming and calcining, and then dopamine is added, and the functional groups in dopamine are used to enhance the bonding between the fiber and the aerogel and other components, and improve the connection performance of the interface of the composite material. At the same time, the modified aerogel can improve the mechanical properties of the composite material.

[0011] Preferably, the preparation method of the modified polyethylene glycol is as follows: by weight, 12-16 parts of polyethylene glycol are added to 30-40 parts of N,N-dimethylformamide, 2-4 parts of 3-amino-1,2-propylene glycol and 1-3 parts of diethylamine are added, the temperature is raised to 80-90°C and stirred for 30-50 minutes, then 10-20 parts of succinic anhydride are added and stirred for 20-40 minutes, extracted with cyclohexane, the obtained product is mixed with thionyl chloride at a mass ratio of 7-10:1, stirred for 20-30 minutes, and then distilled under reduced pressure to obtain the modified polyethylene glycol; by grafting amino groups on the ends of the polyethylene glycol, the reaction activity of the polyethylene glycol is enhanced, and then succinic anhydride is added for cross-linking modification, so that the modified polyethylene glycol can react with other components to form a macromolecular network structure, improve the interface properties of other components, and closely combine with the reinforcing fibers to improve the mechanical properties of the composite material.

[0012] The present invention also provides a method for preparing the composite material of the polyurethane resin for pultrusion, comprising the following steps:

[0013] Weigh each raw material according to the ratio;

[0014] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0015] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0016] The components in barrel A and barrel B are mixed and injected into a glue injection box at a weight ratio of 1-2:1 through a glue injection machine to impregnate the reinforcing fibers, and then pultruded to obtain a composite material, wherein the process parameters of the pultrusion molding are a temperature of 80-100°C in zone 1, a temperature of 150-170°C in zone 2, a temperature of 110-130°C in zone 3, and a pultrusion speed of 1-3m / min.

[0017] Specifically, by adding nano-expanded graphite to the polyurethane resin raw material, on the one hand, the nano-expanded graphite has good pressure resistance, flexibility, plasticity and self-lubrication, which can improve the mechanical properties of the composite material; on the other hand, during pultrusion, high temperature can cause its volume to expand, effectively filling the internal pore structure of the composite material, further improving the mechanical properties of the composite material.

[0018] Preferably, the modified aerogel and expanded graphite are subjected to fermentation pretreatment before being added to the barrel of the glue injection machine B. The fermentation pretreatment method is: the modified aerogel and expanded graphite are mixed, loaded into a culture vessel and injected with bacterial cellulose fermentation liquid, wrapped, and cultured at 25-30°C for 2-5 days, the culture product is rinsed with deionized water, the residual culture liquid is removed, and it is soaked with deionized water until it is colorless, and finally filtered and dried to obtain a mixed fermentation pretreatment product of modified aerogel and expanded graphite. By fermenting the modified aerogel and expanded graphite, the bacterial cellulose grows into the modified aerogel and expanded graphite during the fermentation process, forming an interlaced interpenetrating network with them, and is fully combined with other components and reinforcing fibers to improve the mechanical properties of the composite material.

[0019] The preparation method of the bacterial cellulose fermentation liquid is as follows: inoculating Gluconacetobacter species into a culture liquid, the temperature is 24-28°C, the stirring speed is 200-240r / min, and the culture time is 24-36 hours to obtain a seed liquid; the seed liquid with a volume of 8-12% of the culture liquid is introduced into the culture liquid, mixed and set aside, to obtain a bacterial cellulose fermentation liquid.

[0020] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0021] The composite material of polyurethane resin for pultrusion provided by the present invention has a fast reaction speed of isocyanate and polymer polyol, can be quickly formed by pultrusion, can form crosslinking, and enhance mechanical strength. By adding modified aerogel, the connection performance of the interface of the composite material is improved. At the same time, the modified aerogel can improve the mechanical properties of the composite material. By adding modified polyethylene glycol, it can react with other components to form a macromolecular network structure, improve the interface properties of other components, and closely combine with reinforcing fibers to improve the mechanical properties of the composite material. By adding nano-expanded graphite, it has good pressure resistance, flexibility, plasticity and self-lubrication, and can improve the mechanical properties of the composite material. During pultrusion molding, high temperature can cause its volume to expand, effectively fill the internal pore structure of the composite material, and further improve the mechanical properties of the composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a flow chart for preparing a composite material of a polyurethane resin for pultrusion provided by Examples 1-5 of the present invention;

[0023] Figure 2 This is a flow chart for preparing a composite material of a polyurethane resin for pultrusion provided in Example 6 of the present invention;

[0024] Figure 3 This is a flow chart for preparing a composite material of polyurethane resin for pultrusion provided in Example 7 of the present invention. DETAILED DESCRIPTION

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned drawings are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, not to describe a specific order.

[0026] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0027] Example 1

[0028] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 1 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0029] The raw materials of the polyurethane resin are weighed according to the ratio, including 150 parts of isocyanate, 90 parts of polymer polyol, 0.2 parts of catalyst, 1 part of dewatering agent, 1 part of antioxidant, 1 part of anti-ultraviolet agent, 1 part of chain extender, 1 part of release agent, 3 parts of modified aerogel, 2 parts of modified polyethylene glycol, and 1 part of nano-expanded graphite;

[0030] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0031] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0032] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0033] The process parameters of the pultrusion molding are: a temperature of 80°C in the first zone, a temperature of 150°C in the second zone, a temperature of 110°C in the third zone, and a pultrusion speed of 1 m / min.

[0034] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0035] In a specific implementation, the preparation method of the modified aerogel is as follows: 15 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 50 parts of dopamine hydrochloric acid solution with a concentration of 5 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0036] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 12 parts of polyethylene glycol are added to 30 parts of N, N-dimethylformamide, 2 parts of 3-amino-1,2-propylene glycol and 1 part of diethylamine are added, the temperature is raised to 80° C. and stirred for 30 minutes, then 10 parts of succinic anhydride are added and stirred for 20 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 7:1, stirred for 20 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0037] Example 2

[0038] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 1 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0039] The raw materials of the polyurethane resin are weighed according to the ratio, including 180 parts of isocyanate, 95 parts of polymer polyol, 0.4 parts of catalyst, 1.5 parts of water remover, 1.5 parts of antioxidant, 1.5 parts of anti-ultraviolet agent, 2 parts of chain extender, 2 parts of release agent, 4 parts of modified aerogel, 3 parts of modified polyethylene glycol, and 2 parts of nano-expanded graphite;

[0040] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0041] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0042] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0043] The process parameters of the pultrusion molding are: a temperature of 80°C in the first zone, a temperature of 150°C in the second zone, a temperature of 110°C in the third zone, and a pultrusion speed of 1 m / min.

[0044] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0045] In a specific implementation, the preparation method of the modified aerogel is as follows: 15 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 50 parts of dopamine hydrochloric acid solution with a concentration of 5 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0046] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 12 parts of polyethylene glycol are added to 30 parts of N, N-dimethylformamide, 2 parts of 3-amino-1,2-propylene glycol and 1 part of diethylamine are added, the temperature is raised to 80° C. and stirred for 30 minutes, then 10 parts of succinic anhydride are added and stirred for 20 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 7:1, stirred for 20 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0047] Example 3

[0048] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 1 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0049] The raw materials of the polyurethane resin are weighed according to the ratio, including 200 parts of isocyanate, 100 parts of polymer polyol, 0.6 parts of catalyst, 2 parts of dewatering agent, 2 parts of antioxidant, 2 parts of anti-ultraviolet agent, 3 parts of chain extender, 3 parts of release agent, 5 parts of modified aerogel, 4 parts of modified polyethylene glycol, and 3 parts of nano-expanded graphite;

[0050] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0051] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0052] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0053] The process parameters of the pultrusion molding are: a temperature of 90° C. in the first zone, 160° C. in the second zone, 120° C. in the third zone, and a pultrusion speed of 2 m / min.

[0054] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0055] In a specific implementation, the preparation method of the modified aerogel is as follows: 18 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 55 parts of dopamine hydrochloric acid solution with a concentration of 5-10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0056] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 14 parts of polyethylene glycol are added to 35 parts of N, N-dimethylformamide, 3 parts of 3-amino-1,2-propylene glycol and 2 parts of diethylamine are added, the temperature is raised to 85° C. and stirred for 30-50 minutes, then 15 parts of succinic anhydride are added and stirred for 30 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 8:1, stirred for 25 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0057] Example 4

[0058] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 1 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0059] The raw materials of the polyurethane resin are weighed according to the ratio, and in parts by weight, 220 parts of isocyanate, 105 parts of polymer polyol, 0.8 parts of catalyst, 2.5 parts of dewatering agent, 2.5 parts of antioxidant, 2.5 parts of anti-ultraviolet agent, 4 parts of chain extender, 4 parts of release agent, 6 parts of modified aerogel, 5 parts of modified polyethylene glycol, and 4 parts of nano-expanded graphite;

[0060] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0061] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0062] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0063] The process parameters of the pultrusion molding are: the temperature of zone 1 is 100°C, the temperature of zone 2 is 170°C, the temperature of zone 3 is 130°C, and the pultrusion speed is 3m / min.

[0064] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0065] In a specific implementation, the preparation method of the modified aerogel is as follows: 20 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 60 parts of dopamine hydrochloric acid solution with a concentration of 10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0066] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 16 parts of polyethylene glycol are added to 40 parts of N, N-dimethylformamide, 4 parts of 3-amino-1,2-propylene glycol and 3 parts of diethylamine are added, the temperature is raised to 90° C. and stirred for 50 minutes, then 20 parts of succinic anhydride are added and stirred for 40 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 10:1, stirred for 30 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0067] Example 5

[0068] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 1 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0069] The raw materials of the polyurethane resin are weighed according to the ratio, including 250 parts of isocyanate, 110 parts of polymer polyol, 0.1 parts of catalyst, 3 parts of dewatering agent, 3 parts of antioxidant, 3 parts of anti-ultraviolet agent, 5 parts of chain extender, 5 parts of release agent, 7 parts of modified aerogel, 6 parts of modified polyethylene glycol, and 5 parts of nano-expanded graphite;

[0070] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0071] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0072] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0073] The process parameters of the pultrusion molding are: the temperature of zone 1 is 100°C, the temperature of zone 2 is 170°C, the temperature of zone 3 is 130°C, and the pultrusion speed is 3m / min.

[0074] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0075] In a specific implementation, the preparation method of the modified aerogel is as follows: 20 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 60 parts of dopamine hydrochloric acid solution with a concentration of 10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0076] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 16 parts of polyethylene glycol are added to 40 parts of N, N-dimethylformamide, 4 parts of 3-amino-1,2-propylene glycol and 3 parts of diethylamine are added, the temperature is raised to 90° C. and stirred for 50 minutes, then 20 parts of succinic anhydride are added and stirred for 40 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 10:1, stirred for 30 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0077] Example 6 (Based on Example 3, the reinforcing fiber is pre-treated by being soaked in an aqueous solution of a lignin derivative having a mass percentage concentration of 40-60% before use)

[0078] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 2 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0079] The raw materials of the polyurethane resin are weighed according to the ratio, including 200 parts of isocyanate, 100 parts of polymer polyol, 0.6 parts of catalyst, 2 parts of dewatering agent, 2 parts of antioxidant, 2 parts of anti-ultraviolet agent, 3 parts of chain extender, 3 parts of release agent, 5 parts of modified aerogel, 4 parts of modified polyethylene glycol, and 3 parts of nano-expanded graphite;

[0080] The reinforcing fiber is pretreated by being impregnated with a lignin derivative aqueous solution having a mass percentage concentration of 40-60%;

[0081] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0082] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0083] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0084] The process parameters of the pultrusion molding are: a temperature of 90°C in the first zone, a temperature of 160°C in the second zone, a temperature of 120°C in the third zone, and a pultrusion speed of 3m / min.

[0085] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0086] In a specific implementation, the preparation method of the modified aerogel is as follows: 18 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 55 parts of dopamine hydrochloric acid solution with a concentration of 5-10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0087] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 14 parts of polyethylene glycol are added to 35 parts of N, N-dimethylformamide, 3 parts of 3-amino-1,2-propylene glycol and 2 parts of diethylamine are added, the temperature is raised to 85° C. and stirred for 30-50 minutes, then 15 parts of succinic anhydride are added and stirred for 30 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 8:1, stirred for 25 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0088] Example 7 (Based on Example 3, the modified aerogel and expanded graphite were pretreated by fermentation before being added to the barrel of the glue injection machine B)

[0089] The embodiment of the present invention provides a composite material of polyurethane resin for pultrusion, comprising reinforcing fibers and polyurethane resin, wherein the reinforcing fibers include glass fibers, carbon fibers, and aramid fibers mixed in a medium ratio, and the reinforcing fibers account for 78% of the total weight of the composite material. Figure 3 As shown, the preparation method of the composite material of the polyurethane resin for pultrusion comprises the following steps:

[0090] The raw materials of the polyurethane resin are weighed according to the ratio, including 200 parts of isocyanate, 100 parts of polymer polyol, 0.6 parts of catalyst, 2 parts of dewatering agent, 2 parts of antioxidant, 2 parts of anti-ultraviolet agent, 3 parts of chain extender, 3 parts of release agent, 5 parts of modified aerogel, 4 parts of modified polyethylene glycol, and 3 parts of nano-expanded graphite;

[0091] performing fermentation pretreatment on the modified aerogel and expanded graphite;

[0092] Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine;

[0093] Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly;

[0094] The components in barrel A and barrel B are mixed at a weight ratio of 1.5:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

[0095] The process parameters of the pultrusion molding are: a temperature of 90° C. in the first zone, 160° C. in the second zone, 120° C. in the third zone, and a pultrusion speed of 2 m / min.

[0096] Specifically, the polymer polyol includes a combination of polyether diol, polyether triol, polyester diol, and polyester triol in equal proportions, the catalyst includes a combination of organic metal tin, organic metal mercury, and organic metal bismuth in equal proportions, the dewatering agent includes a carbodiimide dewatering agent, the antioxidant includes a combination of hindered phenol antioxidants and phosphite antioxidants in equal proportions, and the release agent includes a combination of stearic acid, paraffin powder, and polyether silicone oil in equal proportions.

[0097] In a specific implementation, the preparation method of the modified aerogel is as follows: 18 parts of silica aerogel are taken by weight, and first vacuumized and calcined, and then cooled to form nano-scale particles, 55 parts of dopamine hydrochloric acid solution with a concentration of 5-10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device.

[0098] In this embodiment, the preparation method of the modified polyethylene glycol is as follows: by weight, 14 parts of polyethylene glycol are added to 35 parts of N, N-dimethylformamide, 3 parts of 3-amino-1,2-propylene glycol and 2 parts of diethylamine are added, the temperature is raised to 85° C. and stirred for 30-50 minutes, then 15 parts of succinic anhydride are added and stirred for 30 minutes, and then extracted with cyclohexane, and the obtained product is mixed with dichlorothionyl at a mass ratio of 8:1, stirred for 25 minutes, and then distilled under reduced pressure to obtain modified polyethylene glycol.

[0099] Preferably, the fermentation pretreatment method is: mixing the modified aerogel and expanded graphite, placing them in a culture vessel and injecting bacterial cellulose fermentation liquid, wrapping them, and culturing them at 25-30° C. for 2-5 days, rinsing the culture product with deionized water, removing the residual culture liquid, soaking them with deionized water until they are colorless, and finally filtering and drying them to obtain a mixed fermentation pretreatment product of modified aerogel and expanded graphite.

[0100] Comparative Example 1: Compared with Example 3, the modified aerogel is replaced by ordinary aerogel.

[0101] Comparative Example 2: Compared with Example 3, the modified polyethylene glycol was replaced by ordinary polyethylene glycol.

[0102] Comparative Example 3: Compared with Example 3, the comparative example 3 does not contain nano-expanded graphite.

[0103] Comparative Example 4: Compared with Example 3, the modified aerogel is replaced by ordinary aerogel and the modified polyethylene glycol is replaced by ordinary polyethylene glycol, and no expanded graphite is contained.

[0104] Comparative Example 5: A composite material of a commercially available polyurethane resin for pultrusion.

[0105] experiment

[0106] The composite materials of Examples 1-7 and Comparative Examples 1-5 were subjected to mechanical tests according to the standards (GB / T1499, GB / T1447), and the test results are shown in the following table:

[0107]

[0108]

[0109] It can be seen from the above results that the composite material prepared by the present invention has excellent mechanical properties, especially by adding modified aerogel, modified polyethylene glycol and expanded graphite, the three have a synergistic effect and can further improve the mechanical properties of the composite material.

[0110] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A composite material of polyurethane resin for pultrusion, characterized in that: The invention comprises reinforcing fibers and polyurethane resin, wherein the polyurethane resin comprises the following raw materials in parts by weight: 150-250 parts of isocyanate, 90-110 parts of polymer polyol, 0.2-1 parts of catalyst, 1-3 parts of dewatering agent, 1-3 parts of antioxidant, 1-3 parts of anti-ultraviolet agent, 1-5 parts of chain extender, 1-5 parts of release agent, 3-7 parts of modified aerogel, 2-6 parts of modified polyethylene glycol, and 1-5 parts of nano-expanded graphite; The preparation method of the modified aerogel is as follows: 15-20 parts by weight of silica aerogel are first vacuumized and calcined, and then cooled to form nano-sized particles, and 50-60 parts of a dopamine hydrochloric acid solution with a concentration of 5-10 mg / ml are added, and the modified aerogel is obtained after drying using a microwave drying device; The preparation method of the modified polyethylene glycol is as follows: by weight, 12-16 parts of polyethylene glycol are added to 30-40 parts of N,N-dimethylformamide, 2-4 parts of 3-amino-1,2-propylene glycol and 1-3 parts of diethylamine are added, the temperature is raised to 80-90° C. and stirred for 30-50 minutes, then 10-20 parts of succinic anhydride are added and stirred for 20-40 minutes, and then extracted with cyclohexane, the obtained product is mixed with dichlorothionyl at a mass ratio of 7-10:1, stirred for 20-30 minutes, and then distilled under reduced pressure to obtain the modified polyethylene glycol.

2. The composite material of polyurethane resin for pultrusion according to claim 1, characterized in that: The polyurethane resin comprises the following raw materials in parts by weight: 180-220 parts of isocyanate, 95-105 parts of polymer polyol, 0.4-0.8 parts of catalyst, 1.5-2.5 parts of dewatering agent, 1.5-2.5 parts of antioxidant, 1.5-2.5 parts of anti-ultraviolet agent, 2-4 parts of chain extender, 2-4 parts of release agent, 4-6 parts of modified aerogel, 3-5 parts of modified polyethylene glycol and 2-4 parts of nano-expanded graphite.

3. The composite material of polyurethane resin for pultrusion according to claim 2, characterized in that: The polyurethane resin comprises the following raw materials in parts by weight: 200 parts of isocyanate, 100 parts of polymer polyol, 0.6 parts of catalyst, 2 parts of dewatering agent, 2 parts of antioxidant, 2 parts of anti-ultraviolet agent, 3 parts of chain extender, 3 parts of release agent, 5 parts of modified aerogel, 4 parts of modified polyethylene glycol and 3 parts of nano-expanded graphite.

4. The composite material of polyurethane resin for pultrusion according to claim 1, characterized in that: The reinforcing fiber accounts for 70-85% of the total weight of the composite material, and the polyurethane resin accounts for 15-30% of the total weight of the composite material.

5. The composite material of polyurethane resin for pultrusion according to claim 1, characterized in that: The reinforcing fibers include one or more combinations of glass fibers, carbon fibers, and aramid fibers. The reinforcing fibers are pre-treated by being soaked in an aqueous solution of a lignin derivative with a mass percentage concentration of 40-60% before use.

6. The composite material of polyurethane resin for pultrusion according to claim 1, characterized in that: The polymer polyol includes one or more combinations of polyether diols, polyether triols, polyester diols, and polyester triols; the catalyst includes one or more combinations of organic metal tin, organic metal mercury, and organic metal bismuth; the dewatering agent includes a carbodiimide dewatering agent; the antioxidant includes one or more combinations of hindered phenol antioxidants and phosphite antioxidants; and the release agent includes one or more combinations of stearic acid, paraffin powder, and polyether silicone oil.

7. The method for preparing a composite material of a polyurethane resin for pultrusion according to any one of claims 1 to 6, characterized in that: The steps include: Weigh each raw material according to the ratio; Put isocyanate, the raw material of polyurethane resin, into the barrel A of the glue injection machine; Put the other raw materials of polyurethane resin into the barrel B of the glue injection machine and mix them evenly; The components in barrel A and barrel B are mixed in a weight ratio of 1-2:1 and injected into a glue injection box through a glue injection machine to wet the reinforcing fibers, and then pultruded to obtain a composite material.

8. The method for preparing a composite material of polyurethane resin for pultrusion according to claim 7, characterized in that: The modified aerogel and expanded graphite are subjected to fermentation pretreatment before being added to the B barrel of the glue injection machine. The fermentation pretreatment method is as follows: the modified aerogel and expanded graphite are mixed, loaded into a culture vessel, and bacterial cellulose fermentation liquid is injected, wrapped, and cultured at 25-30° C. for 2-5 days, the culture product is rinsed with deionized water, the residual culture liquid is removed, and the culture product is soaked with deionized water until it is colorless, and finally filtered and dried to obtain a mixed fermentation pretreatment product of the modified aerogel and expanded graphite.

Citation Information

Patent Citations

  • A Method For Composite Geopolymer Grouting Material Used For Asphalt Surface Layer Reinforcement And Anti-flow Deformation

    AU2021105693A4

  • Hyperbranched non-ionic waterborne polyurethane and application thereof in fibreglass sizing agent

    CN103360564A