A bridge expansion joint filling material and its preparation method and application

By using carbon black and polydopamine-modified graphene in the bridge expansion joint sealing material, which absorbs ultraviolet light and conducts heat, combined with lignin modification treatment, the aging problem of the sealing material is solved, and the aging resistance and waterproofing effect are improved. Extended service life and reduced maintenance frequency.

CN118388952BActive Publication Date: 2024-10-22TIANJIN BINHAI NEW AREA BRANCH OF CCCC FOURTH HIGHWAY ENG CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410846695.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Bridge expansion joint sealing materials are prone to aging, yellowing, brittleness and cracking when exposed to ultraviolet rays and harsh climatic conditions for a long time, resulting in shortened service life, and regular cleaning is time-consuming and labor-intensive, affecting traffic efficiency.

Method used

Use polyurethane prepolymer as the matrix, add carbon black and polydopamine modified graphene, carbon black absorbs ultraviolet light through reflection and scattering, graphene conducts heat to reduce heat accumulation, polydopamine captures free radicals, and combined with lignin modified carbon black improves Dispersion and compatibility, extending material life.

Benefits of technology

The aging resistance and waterproof effect of the sealing material are significantly improved, the service life is extended, and the maintenance frequency and traffic closure time are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The present application relates to the technical field of bridge construction, in particular to a bridge expansion joint filling material and its preparation method and application. A bridge expansion joint filling material, including component A and component B; the component A includes the following raw materials in parts by weight: 60-70 parts of polyurethane prepolymer, 5-10 parts of plasticizer, 5-15 parts of carbon black, 3-10 parts of polydopamine modified graphene, 0.1-1 parts of catalyst, and 1-3 parts of defoaming agent; the component B includes the following raw materials in parts by weight: 10-15 parts of curing agent and 1-3 parts of silane coupling agent. The sealing material of the present application has strong aging resistance, is applied to bridge expansion joints, has excellent waterproof performance and has a long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of bridge construction, and in particular to a bridge expansion joint filling material and a preparation method and application thereof. Background Art

[0002] Bridge expansion joints are set up between the two beam ends, between the beam ends and the abutments, or at the hinges of the bridge to meet the needs of bridge deck deformation and waterproofing. They can freely expand and contract in parallel and vertical directions along the bridge axis, and can adjust the displacement and connection between the superstructures caused by vehicle loads and bridge construction materials. They play an important role in adjusting the displacement and connection caused by vehicle loads and bridge construction materials.

[0003] Bridge expansion joints are usually composed of steel structures and elastic waterproof strips, which can ensure sealing, durability and resistance to damage. However, during long-term service, rainwater and wheels will bring a lot of mud and gravel into the expansion joints, which will form hard fillers over time, greatly reducing the deformation capacity of the expansion joints. For this reason, the road maintenance department needs to clean the expansion joints regularly, which not only consumes a lot of manpower and material resources, time and energy, but also requires long-term traffic closure, resulting in reduced traffic efficiency.

[0004] For this purpose, some special materials are used to seal and protect the expansion joints, such as polyurethane and silicone sealing materials, which have excellent elasticity and can play a good role in sealing and protection. Their low modulus can ensure their flexibility and deformability, and are widely used in repair and sealing.

[0005] The above-mentioned related technologies have the following defects: when the sealing material is exposed to ultraviolet rays and adverse weather conditions for a long time, it may age, turn yellow, become brittle and crack, which will affect the service life of the sealing material. Summary of the invention

[0006] In order to extend the service life of a bridge expansion joint filling material, the present application provides a bridge expansion joint filling material and a preparation method and application thereof.

[0007] In a first aspect, the present application provides a bridge expansion joint filling material, which adopts the following technical solution:

[0008] A bridge expansion joint filling material, comprising component A and component B;

[0009] The component A comprises the following raw materials in parts by weight: 60-70 parts of polyurethane prepolymer, 5-10 parts of plasticizer, 5-15 parts of carbon black, 3-10 parts of polydopamine-modified graphene, 0.1-1 parts of catalyst, and 1-3 parts of defoaming agent;

[0010] The B component includes the following raw materials in parts by weight: 10-15 parts of a curing agent and 1-3 parts of a silane coupling agent.

[0011] By adopting the above technical scheme, polyurethane prepolymer is cured as the matrix, and carbon black and polydopamine are added to modify graphene. Carbon black is a black particle formed by the polymerization of carbon atoms, with a polynuclear aromatic hydrocarbon structure and an o-hydroxy aromatic ketone structure around it. When ultraviolet rays irradiate the surface of carbon black, an interaction occurs between photons and carbon black particles. The special structure of carbon black particles causes photons to be reflected and scattered multiple times on the surface of the particles, and continuously interact with carbon atoms in the particles. These reflections, scatterings and interactions lead to the absorption of ultraviolet light energy, thereby converting most of the ultraviolet radiation into heat energy. In addition to its light absorption ability, carbon black can also effectively block the transmission of ultraviolet rays, thereby reducing the possibility of ultraviolet rays transmitting into the interior of the substrate.

[0012] Ultraviolet rays and heat are both factors that accelerate the aging of polyurethane sealing materials. Although the addition of carbon black greatly reduces the aging effect of ultraviolet rays on polyurethane sealing materials, carbon black will convert most of the ultraviolet radiation into heat energy when absorbing ultraviolet light energy. If the heat energy is stored in the polyurethane sealing material, it will also accelerate the aging of the polyurethane sealing material to a certain extent. Graphene is a two-dimensional material composed of a single layer of carbon atoms and has excellent thermal conductivity. The addition of graphene can conduct the heat inside the polyurethane sealing material in a timely manner and reduce the accumulation of heat inside the polyurethane sealing material. In addition, polydopamine is a macromolecule with polyphenolic hydroxyl groups formed by the polymerization of dopamine. It can be used as a free radical scavenger to slow down the aging of polyurethane sealing materials. Modifying graphene with polydopamine can improve the dispersion performance of graphene on the one hand, and on the other hand, it can cooperate with carbon black to improve the effect of resisting ultraviolet aging.

[0013] Furthermore, the preparation method of the polyurethane prepolymer is:

[0014] The polytetrahydrofuran polyol and the terminal hydroxyl polydimethylsiloxane are mixed and heated for dehydration, and then toluene diisocyanate is added for reaction, and then a chain extender is added for further reaction to obtain a polyurethane prepolymer.

[0015] By adopting the above technical solution, hydroxy-terminated polydimethylsiloxane is introduced into the polyurethane prepolymer to obtain an organosilicon-modified polyurethane material. The intermolecular force of hydroxy-terminated polydimethylsiloxane is weak and the microphase separation degree of the polyurethane material is reduced, and the fracture growth rate of the polyurethane material is increased, thereby improving the adaptability of the polyurethane sealing material to the deformation of the expansion joint. In addition, the hydrophobicity of hydroxy-terminated polydimethylsiloxane reduces the water absorption rate of the polyurethane material and significantly increases the water contact angle, thereby improving the waterproof effect of the polyurethane sealing material.

[0016] Furthermore, the chain extender is one or more of 1,4-butanediol and 1,6-hexanediol.

[0017] By adopting the above technical solution, the chain extender can regulate the group and structure of the hard segment in the polyurethane. The group generated by the reaction of the chain extender of the present application with isocyanate has a high thermal decomposition temperature, which can effectively improve the heat-oxidative aging resistance of the polyurethane material.

[0018] In some embodiments, the chain extender is 1,4-butanediol; in some embodiments, the chain extender is 1,6-hexanediol; in some embodiments, the chain extender is a mixture of 1,4-butanediol and 1,6-hexanediol.

[0019] Furthermore, the preparation method of the polydopamine-modified graphene is:

[0020] Graphene oxide is dispersed in water to obtain a graphene dispersion, and then the graphene dispersion is mixed with a dopamine hydrochloride solution, and the pH value of the mixed solution is adjusted to 8-9, and the mixed solution is reacted at a temperature of 55-65°C for 24 hours, and then filtered, centrifuged, washed, and dried to obtain polydopamine-modified graphene.

[0021] Furthermore, the carbon black is lignin-modified carbon black, and the preparation method is:

[0022] 1) Preparation of lignin quaternary ammonium salt

[0023] The alkaline lignin solution is mixed with the 3-chloro-2-hydroxypropyltrimethylammonium chloride solution, and then a sodium hydroxide aqueous solution is added to react at 85-90° C. After the reaction is completed, the reaction solution is purified by dialysis, and freeze-dried to obtain lignin quaternary ammonium salt powder;

[0024] 2) Preparation of lignin modified carbon black

[0025] Disperse carbon black in water, then add the quaternary ammonium salt of lignin obtained in 1) above, then heat the mixed solution to 120-125°C for reaction for 4-6 hours, cool after the reaction is completed, then collect the solid precipitate, dry and grind to obtain lignin modified carbon black.

[0026] By adopting the above technical scheme, carbon black is modified with lignin, and lignin is grafted on carbon black under the action of electrostatic interaction, van der Waals force, and π-π interaction. On the one hand, the steric hindrance between particles can be increased, thereby improving the dispersion stability of the composite particles; on the other hand, it can promote the increase of the specific surface area of ​​the composite particles, provide more active sites to interact with the polyurethane matrix, thereby improving the compatibility of carbon black and polyurethane. In addition, lignin modification can introduce hydroxyl functional groups on carbon black, which interact with the amino functional groups in polyurethane through hydrogen bonds, so that the disordered "soft segments" in the polyurethane molecules are transformed into ordered "hard segments", thereby improving the mechanical properties and heat resistance of polyurethane materials. Finally, the light absorption intensity of lignin-modified carbon black in the ultraviolet light region increases, further slowing down the light aging of polyurethane materials.

[0027] Furthermore, the weight ratio of alkali lignin to 3-chloro-2-hydroxypropyltrimethylammonium chloride in the lignin quaternary ammonium salt is 1:(0.8-1.2), and the weight ratio of lignin quaternary ammonium salt to carbon black in the lignin-modified carbon black is 1:(1.5-2).

[0028] Furthermore, the particle size of the carbon black is 10-20 nm.

[0029] In a second aspect, the present application provides a method for preparing a bridge expansion joint filling material, using the following technical solution:

[0030] A method for preparing a bridge expansion joint filling material comprises the following steps:

[0031] S1. The polyurethane prepolymer, plasticizer, carbon black, polydopamine-modified graphene, catalyst, and defoamer are mixed and sealed to obtain component A;

[0032] S2. Mixing the curing agent and the silane coupling agent and sealing to obtain component B;

[0033] S3. Mix component A and component B, and react them at a temperature of 10-60° C. to obtain a bridge expansion joint filling material.

[0034] In a third aspect, the present application provides an application of a bridge expansion joint filling material, using the following technical solution:

[0035] The invention discloses an application of a bridge expansion joint filling material, which is used for filling the expansion joint of a road bridge. When in use, component B is first applied to the wall surface of the expansion joint, and then component A is poured into the expansion joint for a curing reaction.

[0036] In summary, this application has the following beneficial effects:

[0037] Carbon black and polydopamine-modified graphene are used as fillers. Carbon black causes photons to reflect and scatter multiple times on the surface of the particles through reflection and scattering, and constantly interacts with the carbon atoms in the particles. These reflections, scattering and interactions lead to the absorption of ultraviolet light energy, thereby converting most of the ultraviolet radiation into heat energy. In addition to its light-absorbing ability, carbon black can also effectively block the transmission of ultraviolet light, thereby reducing the possibility of ultraviolet light transmitting into the interior of the substrate. Carbon black absorbs ultraviolet light, but it generates heat inside the material. Graphene conducts the heat inside the material away, reducing the chance of material aging. At the same time, polydopamine itself acts as a free radical scavenger to slow down the aging of polyurethane sealing materials. DETAILED DESCRIPTION

[0038] The present application is further described in detail below with reference to the embodiments.

[0039] Raw materials and intermediate preparation examples

[0040] raw material

[0041] The raw materials in the examples of this application can be obtained from commercial sources:

[0042] Plasticizer, ethyl acetate;

[0043] Catalyst, stannous octoate;

[0044] Defoamer, BYK024 defoamer;

[0045] Curing agent, which is Incozol 4 curing agent;

[0046] Silane coupling agent, KH550;

[0047] Polytetramethylene glycol, technical grade, M n is 1000;

[0048] Hydroxyl-terminated polydimethylsiloxane, industrial grade, M n is 1000;

[0049] Toluene diisocyanate, technical grade;

[0050] Alkali lignin, solid content is about 45 wt%, lignin purity is about 90%, and the rest is impurities such as organic acid, sugar, low molecular carbohydrates, etc.; after acid precipitation purification, the purified alkali lignin solid is dissolved in water with a pH of 12 to prepare a solution with a mass percentage concentration of about 25 wt% for standby use;

[0051] 3-Chloro-2-hydroxypropyltrimethylammonium chloride, analytical grade.

[0052] Preparation Example

[0053] Preparation Example I-1

[0054] A polyurethane prepolymer, the preparation method of which is:

[0055] 60kg of polytetrahydrofuran polyol and 15kg of terminal hydroxyl polydimethylsiloxane were mixed, then heated to 125°C, dehydrated for 2h under a vacuum degree of 0.01MPa, nitrogen protective gas was introduced, 10kg of 120# solvent oil was added, and the temperature was lowered to 55°C; then 25kg of toluene diisocyanate was added, the temperature was raised to 80°C, and the reaction was kept warm for 2h, and then 3kg of 1,4-butanediol chain extender was added and the temperature was raised to 100°C for aging for 10h to obtain a polyurethane prepolymer.

[0056] Preparation Example I-2

[0057] Different from Preparation Example I-1, the chain extender in Preparation Example I-2 is 1,4-butanediol and 1,6-hexanediol in a weight ratio of 2:1.

[0058] Preparation Example I-3

[0059] Different from Preparation Example I-1, in Preparation Example I-3, an equal amount of polytetrahydrofuran polyol is used to replace the terminal hydroxyl polydimethylsiloxane.

[0060] Preparation Example II-1

[0061] A polydopamine-modified graphene, the preparation method of which is as follows:

[0062] 2 kg of graphene oxide was dispersed in 2 L of water to obtain a graphene dispersion; 4 kg of dopamine hydrochloride was mixed with 0.3 kg of Tris-HCl solution to obtain a dopamine hydrochloride solution; the graphene dispersion was then mixed with the dopamine hydrochloride solution, and ammonia water was added dropwise to adjust the pH value of the mixture to 8.5, and the mixture was reacted at 60 ° C for 24 h, and then filtered and centrifuged. The precipitate was repeatedly rinsed with anhydrous ethanol and deionized water until the supernatant was clear, and dried in a vacuum drying oven at 60 ° C for 24 h to obtain polydopamine-modified graphene.

[0063] Preparation Example III-1

[0064] A lignin modified carbon black, the preparation method of which is:

[0065] 1) Preparation of lignin quaternary ammonium salt

[0066] The alkali lignin solution was mixed with a 3-chloro-2-hydroxypropyltrimethylammonium chloride solution (mass percentage concentration of 60%), wherein the content of alkali lignin in the alkali lignin solution was 4 kg, and the content of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the 3-chloro-2-hydroxypropyltrimethylammonium chloride solution was 4 kg, and then 0.3 kg of a 20% sodium hydroxide aqueous solution was added and reacted at 90° C. for 4 hours. After the reaction was completed, the reaction solution was purified by dialysis, and freeze-dried to obtain a lignin quaternary ammonium salt powder;

[0067] 2) Preparation of lignin modified carbon black

[0068] 10 kg of carbon black was dispersed in water, and then 6 kg of the lignin quaternary ammonium salt obtained in 1) was added, and then the mixed solution was heated to 120°C for reaction for 5 h. After the reaction was completed, it was placed in a 25°C environment for 24 h for natural cooling, and then the solid precipitate was collected, rinsed with deionized water for 3 times, dried at 50°C, and then ground to obtain lignin-modified carbon black;

[0069] The particle size of carbon black is 10-20nm.

[0070] Preparation Example III-2

[0071] The difference from Preparation Example III-1 is that the content of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the 3-chloro-2-hydroxypropyltrimethylammonium chloride solution in Preparation Example III-1 is 3.2 kg.

[0072] Preparation Example III-3

[0073] Different from Preparation Example III-1, the content of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the 3-chloro-2-hydroxypropyltrimethylammonium chloride solution in Preparation Example III-3 is 4.8 kg.

[0074] Preparation Example III-4

[0075] Different from Preparation Example III-1, the amount of carbon black in Preparation Example III-4 is 9 kg.

[0076] Preparation Example III-5

[0077] Different from Preparation Example III-1, the amount of carbon black in Preparation Example III-4 is 12 kg.

[0078] Preparation Example III-6

[0079] Different from Preparation Example III-1, the amount of carbon black in Preparation Example III-6 is 6 kg.

[0080] Preparation Example III-7

[0081] Different from Preparation Example III-1, the particle size of carbon black in Preparation Example III-7 is 30-40 nm.

[0082] Example

[0083] Examples 1-3

[0084] A bridge expansion joint filling material, and a preparation method thereof is as follows:

[0085] S1. According to the raw material ratio in Table 1, the polyurethane prepolymer, plasticizer, carbon black, polydopamine-modified graphene, catalyst, and defoamer are mixed and sealed to obtain component A;

[0086] S2. Mixing the curing agent and the silane coupling agent and sealing to obtain component B;

[0087] S3. Component A and component B are mixed, and reacted and cured at a temperature of 25° C. to obtain a bridge expansion joint filling material.

[0088] Table 1 Raw material ratios in Examples 1-3 (kg)

[0089]

[0090] Wherein, the carbon black particle size is 10-20 nm, the polyurethane prepolymer comes from Preparation Example I-1, and the polydopamine-modified graphene comes from Preparation Example II-1.

[0091] Embodiment 4-5

[0092] Different from Example 2, the polyurethane prepolymers in Examples 4-5 are respectively from Preparation Examples I-2~I-3.

[0093] Example 6

[0094] Different from Example 2, the carbon black particle size in Example 6 is 30-40nm.

[0095] Embodiment 7-13

[0096] Different from Example 4, in Examples 7-13, the carbon black was replaced by an equal amount of lignin-modified carbon black.

[0097] Comparative Example

[0098] Comparative Example 1

[0099] Different from Example 1, in Comparative Example 1, an equal amount of carbon black is used to replace the polydopamine-modified graphene.

[0100] Comparative Example 2

[0101] Different from Example 1, in Comparative Example 2, an equal amount of polydopamine-modified graphene is used to replace carbon black.

[0102] Comparative Example 3

[0103] Different from Example 1, in Comparative Example 3, an equal amount of graphene is used to replace the polydopamine-modified graphene.

[0104] Performance Testing

[0105] Performance testing methods

[0106] The sealing materials in the embodiments and comparative examples were subjected to the following performance tests, and the test results are shown in Table 2.

[0107] The test of the tensile adhesion after immersion in water was carried out in accordance with "Test Methods for Building Sealing Materials Part 11: Determination of Tensile Adhesion after Immersion in Water" GB / T13477.11-2017, and the immersion time was 360h.

[0108] The sample was exposed to ultraviolet light with a wavelength of 340 nm and a radiation intensity of 45 w / m 2 After aging for 360 hours in an environment with an internal temperature of 80°C and a relative humidity of 45%, the tensile strength of the material was tested.

[0109] Table 2 Performance test results

[0110]

[0111] Combining Examples 1-13 with Comparative Examples 1-3 and Table 2, it can be seen that the tensile strength of the sealing materials in Examples 1-13 after UV aging is higher than that of Comparative Examples 1-3, which indicates that the sealing materials of the present application have better aging resistance.

[0112] Combining Example 1 with Comparative Examples 1-3, and combining Table 2, it can be seen that compared with the use of carbon black and polydopamine modified graphene compounded as filler in Example 1, carbon black is used as filler in Comparative Example 1, polydopamine modified graphene is used as filler in Comparative Example 2, and carbon black and graphene are compounded as filler in Comparative Example 3. The anti-aging properties of the sealing materials in Comparative Examples 1-3 are all reduced, wherein the anti-aging properties of the sealing material in Comparative Example 3 are relatively high, which shows that the compounding of carbon black and graphene as filler can improve the anti-aging properties of the sealing material, wherein the modification of graphene with polydopamine can further improve the anti-aging properties of the sealing material. This may be because carbon black can cause photons to be reflected and scattered multiple times on the surface of the particles through reflection and scattering, and constantly interact with the carbon atoms in the particles. These reflections, scattering and interactions lead to the absorption of ultraviolet light energy, thereby converting most of the ultraviolet radiation into heat energy. In addition to the light absorption ability, carbon black can also effectively block the transmission of ultraviolet rays, thereby reducing the possibility of ultraviolet rays transmitting into the interior of the substrate. Carbon black absorbs ultraviolet rays, but generates heat inside the material. Graphene conducts the heat inside the material away, reducing the chance of material aging. At the same time, polydopamine itself acts as a free radical scavenger to slow down the aging of the polyurethane sealing material. Among them, the fixed stretch adhesion of the sealing material in Comparative Example 3 is reduced, which may be caused by the uneven dispersion of graphene inside the material.

[0113] Combining Example 2, Example 6, Example 7 and Example 13, and combining Table 2, it can be seen that the carbon black particle size in Example 2 and Example 7 is 10-20nm, and the carbon black particle size in Example 6 and Example 13 is 30-40nm. The aging resistance of the sealing material in Example 6 is better than that in Example 2, and the aging resistance of the sealing material in Example 13 is lower than that in Example 7. This may be because the carbon black with a smaller particle size has a better reflection effect on ultraviolet rays, but the carbon black with a particle size of 10-20nm is poorly dispersed in the material relative to the carbon black with a particle size of 30-40nm, and the carbon black agglomerates to reduce its reflection of ultraviolet rays. After the carbon black is modified with lignin, the steric hindrance between the particles can be increased, thereby improving the dispersion stability of the composite particles.

[0114] Combining Example 2 with Example 5 and Table 2, it can be seen that the fixed elongation adhesion and aging resistance of the sealing material in Example 5 are both reduced. This may be because grafting terminal hydroxyl polydimethylsiloxane into the polyurethane material can not only improve the aging resistance of the material, but also improve the hydrophobicity of the material, thereby improving the waterproof ability of the material, so that the material can still maintain good adhesion after being soaked in water.

[0115] Application Examples

[0116] An application of a bridge expansion joint filling material, and an application method thereof is as follows:

[0117] Apply component B evenly on the wall surface of the bridge expansion joint, then pour component A into the expansion joint to carry out the curing reaction, and the cured sealing material is filled in the bridge expansion joint.

[0118] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A bridge expansion joint filling material, characterized in that: It includes component A and component B; The component A comprises the following raw materials in parts by weight: 60-70 parts of polyurethane prepolymer, 5-10 parts of plasticizer, 5-15 parts of carbon black, 3-10 parts of polydopamine-modified graphene, 0.1-1 parts of catalyst, and 1-3 parts of defoaming agent; The B component includes the following raw materials in parts by weight: 10-15 parts of a curing agent and 1-3 parts of a silane coupling agent; The preparation method of the polyurethane prepolymer is: The polytetrahydrofuran polyol and the terminal hydroxyl polydimethylsiloxane are mixed and heated for dehydration, and then toluene diisocyanate is added for reaction, and then a chain extender is added for further reaction to obtain a polyurethane prepolymer.

2. A bridge expansion joint filling material according to claim 1, characterized in that: The chain extender is one or more of 1,4-butanediol and 1,6-hexanediol.

3. A bridge expansion joint filling material according to claim 1, characterized in that: The preparation method of the polydopamine modified graphene is: Graphene oxide is dispersed in water to obtain a graphene dispersion, and then the graphene dispersion is mixed with a dopamine hydrochloride solution, and the pH value of the mixed solution is adjusted to 8-9, and the mixed solution is reacted at a temperature of 55-65°C for 24 hours, and then filtered, centrifuged, washed, and dried to obtain polydopamine-modified graphene.

4. The bridge expansion joint filling material according to claim 1, characterized in that: The carbon black is lignin modified carbon black, and its preparation method is as follows: 1) Preparation of lignin quaternary ammonium salt The alkaline lignin solution is mixed with the 3-chloro-2-hydroxypropyltrimethylammonium chloride solution, and then a sodium hydroxide aqueous solution is added to react at 85-90° C. After the reaction is completed, the reaction solution is purified by dialysis, and freeze-dried to obtain lignin quaternary ammonium salt powder; 2) Preparation of lignin modified carbon black Disperse carbon black in water, then add the lignin quaternary ammonium salt obtained in 1) above, then heat the mixed solution to 120-125°C for reaction for 4-6 hours, cool after the reaction is completed, then collect the solid precipitate, wash, dry and grind to obtain lignin modified carbon black.

5. A bridge expansion joint filling material according to claim 4, characterized in that: The weight ratio of alkali lignin to 3-chloro-2-hydroxypropyltrimethylammonium chloride in the lignin quaternary ammonium salt is 1:(0.8-1.2), and the weight ratio of lignin quaternary ammonium salt to carbon black in the lignin-modified carbon black is 1:(1.5-2).

6. The bridge expansion joint filling material according to claim 1, characterized in that: The particle size of the carbon black is 10-20 nm.

7. A method for preparing the bridge expansion joint filling material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. The polyurethane prepolymer, plasticizer, carbon black, polydopamine-modified graphene, catalyst, and defoamer are mixed and sealed to obtain component A; S2. Mixing the curing agent and the silane coupling agent and sealing to obtain component B; S3. Mix component A and component B, and react them at a temperature of 10-60° C. to obtain a bridge expansion joint filling material.

8. An application of the bridge expansion joint filling material according to any one of claims 1 to 6, characterized in that: Used for filling expansion joints of roads and bridges. When using, first apply component B to the wall of the expansion joint, and then pour component A into the expansion joint to carry out the curing reaction.