Semiconductor structure manufacturing method, semiconductor structure and semiconductor device

By forming a quantum well structure of gallium nitride and indium gallium nitride on the groove surface of the semiconductor structure, the pressure-electrode polarization stress is alleviated and the light absorption rate of gallium nitride materials is improved, and the light of gallium nitride materials in the prior art is solved. The problem of low absorption rate improves the efficiency of photohydrolysis applications.

CN118398731BActive Publication Date: 2024-11-19SHANDONG YUNHAI GUOCHUANG CLOUD COMPUTING EQUIP IND INNOVATION CENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410832660.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-19
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

In the prior art, the light absorption rate of gallium nitride materials is low, resulting in limited efficiency in photohydrolysis applications.

Method used

By forming a quantum well structure on the groove surface of the substrate structure, the alternately arranged gallium nitride and indium nitride material layers can alleviate the piezoelectric polarization stress on the gallium nitride film and increase the concentration and light of the indium nitride material. Absorption rate.

Benefits of technology

It effectively improves the light absorption rate of gallium nitride materials, enhances the efficiency in photohydrolysis applications, and solves the problem of low light absorption rate of gallium nitride materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118398731B_ABST
    Figure CN118398731B_ABST
Patent Text Reader

Abstract

The embodiment of the present application provides a method for manufacturing a semiconductor structure, a semiconductor structure and a semiconductor device, the method comprising: providing a substrate structure, the substrate structure having a plurality of grooves, the material of the substrate structure comprising at least gallium nitride; forming a quantum well structure on the surface of the grooves of the substrate structure, the quantum well structure comprising at least a stacking structure, the stacking structure comprising a first material layer and a second material layer arranged alternately, a first material layer in direct contact with the surface of the grooves, the material of the first material layer comprising at least gallium nitride, and the material of the second material layer comprising at least indium gallium nitride. Through the present application, the problem of low light absorption rate of indium nitride material in the related art is solved, thereby achieving the effect of improving the light absorption rate of gallium nitride material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the semiconductor field, and in particular, to a method for manufacturing a semiconductor structure, a semiconductor structure, and a semiconductor device. Background Art

[0002] By adding In components to GaN materials to form InGaN materials, the band gap can be adjusted from 3.4 to 0.7 eV at room temperature. Semiconductors with lower band gaps can absorb a wider spectrum, which is beneficial to improving the photocurrent density of GaN materials in photo-splitting water applications. However, during the growth of GaN, InGaN is prone to In precipitation problems due to its low melting point, resulting in a decrease in In concentration and affecting the light absorption rate of indium nitride materials. Summary of the invention

[0003] The embodiments of the present application provide a method for manufacturing a semiconductor structure, a semiconductor structure, and a semiconductor device, so as to at least solve the problem of low light absorption rate of indium nitride materials in the related art.

[0004] According to one embodiment of the present application, a method for manufacturing a semiconductor structure is provided, comprising: providing a substrate structure, wherein the substrate structure has a plurality of grooves, and the material of the substrate structure includes at least gallium nitride; forming a quantum well structure on the surface of the grooves of the substrate structure, wherein the quantum well structure includes at least a stacking structure, and the stacking structure includes alternating first material layers and second material layers, wherein one of the first material layers is in direct contact with the surface of the grooves, the material of the first material layer includes at least gallium nitride, and the material of the second material layer includes at least indium gallium nitride.

[0005] In an exemplary embodiment, a base structure is provided, including: providing a substrate, wherein the material of the substrate includes at least gallium nitride; forming an oxide layer on the surface of the substrate; forming a mask layer on the surface of the oxide layer away from the substrate; removing part of the mask layer, part of the oxide layer and part of the substrate to expose part of the surface of the substrate to form the base structure.

[0006] In another exemplary embodiment, a substrate is provided, comprising: providing a base layer, wherein the material of the base layer includes at least sapphire; forming a nucleation layer on the surface of the base layer, wherein the material of the nucleation layer includes at least gallium nitride; and forming a first epitaxial layer on a surface of the nucleation layer away from the base layer, wherein the material of the first epitaxial layer includes at least gallium nitride.

[0007] In another exemplary embodiment, after providing the base layer and before forming the nucleation layer on the surface of the base layer, the method further comprises: cleaning the base layer with a first predetermined gas under a first predetermined temperature condition for a predetermined period of time.

[0008] In another exemplary embodiment, the first predetermined temperature ranges from 1000° C. to 1200° C., the first predetermined gas includes at least hydrogen, and the predetermined time period ranges from 8 to 15 minutes.

[0009] In another exemplary embodiment, forming the nucleation layer on the surface of the base layer includes: introducing a second predetermined gas into the chamber where the base layer is located under a second predetermined temperature condition to obtain the nucleation layer.

[0010] In another exemplary embodiment, the second predetermined temperature is in the range of 500° C. to 550° C., the second predetermined gas includes at least trimethylgallium and ammonia, and the thickness of the nucleation layer is in the range of 25 to 35 nm.

[0011] In another exemplary embodiment, a first epitaxial layer is formed on the surface of the nucleation layer away from the base layer, comprising: under a third predetermined temperature condition, a first sub-epitaxial layer is formed on the surface of the nucleation layer away from the base layer, wherein the material of the first sub-epitaxial layer includes at least gallium nitride and the first sub-epitaxial layer is a non-doped material layer; under a fourth predetermined temperature condition, a second sub-epitaxial layer is formed on the surface of the first sub-epitaxial layer away from the nucleation layer, wherein the fourth predetermined temperature is lower than the third predetermined temperature, the material of the second sub-epitaxial layer includes at least gallium nitride and a doped material, the thickness of the second sub-epitaxial layer is greater than the thickness of the first sub-epitaxial layer, and the first sub-epitaxial layer and the second sub-epitaxial layer form the first epitaxial layer.

[0012] In another exemplary embodiment, the third predetermined temperature ranges from 1000 to 1100° C., the thickness of the first sub-epitaxial layer ranges from 0.5 to 1.5 μm, the fourth predetermined temperature ranges from 1000 to 1100° C., the thickness of the second sub-epitaxial layer ranges from 1.5 to 2.5 μm, and the doping concentration of the second sub-epitaxial layer ranges from 2.5 to 3.5×10 18 cm −3 .

[0013] In another exemplary embodiment, forming an oxide layer on the surface of the substrate includes: introducing a third predetermined gas into a chamber where the substrate is located under conditions of a fifth predetermined temperature and a predetermined pressure to form the oxide layer, wherein the material of the oxide layer includes at least silicon dioxide.

[0014] In another exemplary embodiment, the fifth predetermined temperature ranges from 150 to 250° C., the predetermined pressure ranges from 900 to 1100 Pa, the third predetermined gas includes at least silicon source gas and oxidation gas, and the thickness of the oxide layer ranges from 150 to 250 nm.

[0015] In another exemplary embodiment, the removing of part of the mask layer, part of the oxide layer and part of the substrate includes: removing part of the mask layer to expose part of the surface of the oxide layer to form a preliminary substrate, wherein the remaining mask layer forms a mask portion, and the material of the mask layer includes at least anodized aluminum oxide; introducing a fourth predetermined gas into the chamber where the preliminary substrate is located, and etching the oxide layer and the substrate using the mask portion as a mask to remove part of the oxide layer and part of the substrate and expose part of the substrate.

[0016] In yet another exemplary embodiment, the fourth predetermined gas includes at least chlorine gas and boron trichloride.

[0017] In another exemplary embodiment, a quantum well structure is formed on the surface of the groove of the substrate structure, including: forming a second epitaxial layer on the surface of the groove of the substrate structure, wherein the material of the second epitaxial layer includes at least gallium nitride; forming the stacking structure on the surface of the second epitaxial layer away from the substrate structure; forming a third epitaxial layer on the surface of the stacking structure away from the second epitaxial layer, wherein the material of the third epitaxial layer includes at least gallium nitride, and the second epitaxial layer, the stacking structure and the third epitaxial layer form the quantum well structure.

[0018] In another exemplary embodiment, forming the second epitaxial layer on the surface of the groove of the substrate structure includes: introducing a fifth predetermined gas into a chamber where the substrate structure is located under a sixth predetermined temperature condition to form the second epitaxial layer.

[0019] In another exemplary embodiment, the sixth predetermined temperature ranges from 1000 to 1100° C., the fifth predetermined gas includes at least trimethylgallium, ammonia and nitrogen, and the thickness of the second epitaxial layer ranges from 1.5 to 2.5 μm.

[0020] In another exemplary embodiment, the stacking structure is formed on the surface of the second epitaxial layer away from the substrate structure, comprising: a first forming step, introducing a sixth predetermined gas into the chamber where the second epitaxial layer is located to form the first material layer; a second forming step, introducing the sixth predetermined gas into the chamber where the first material layer is located to form the second material layer, wherein the gas flow rate of the sixth predetermined gas in the second forming step is different from the gas flow rate of the sixth predetermined gas in the first forming step, and the thickness of the second material layer is greater than the thickness of the first material layer; and repeating the first forming step and the second forming step in sequence at least once until a predetermined number of times is reached to form the stacking structure.

[0021] In another exemplary embodiment, the sixth predetermined gas includes at least trimethylindium, the thickness of the first material layer is in the range of 4 to 6 nm, and the thickness of the second material layer is in the range of 6 to 8 nm.

[0022] In yet another exemplary embodiment, forming a third epitaxial layer on a surface of the stack structure away from the second epitaxial layer includes: introducing a seventh predetermined gas into a chamber where the stack structure is located to form the third epitaxial layer.

[0023] In another exemplary embodiment, the seventh predetermined gas includes at least bismuthocene magnesium, trimethylgallium, ammonia and nitrogen, and the thickness of the third epitaxial layer is in the range of 30 to 60 nm.

[0024] According to another embodiment of the present application, a semiconductor structure is provided, including: a substrate structure, wherein the substrate structure has a plurality of grooves; a quantum well structure, located in the grooves, the quantum well structure at least including a stacked structure, the stacked structure including alternating first material layers and second material layers, wherein one of the first material layers is in direct contact with a surface of the groove, the material of the first material layer includes at least gallium nitride, and the material of the second material layer includes at least indium gallium nitride.

[0025] In another exemplary embodiment, the base structure includes: a substrate, wherein the material of the substrate includes at least gallium nitride; an oxide layer located on a surface of one side of the substrate; and a mask portion located on a surface of the oxide layer away from the substrate, wherein two adjacent mask portions form the groove.

[0026] In another exemplary embodiment, the substrate includes: a base layer, wherein the material of the base layer includes at least sapphire; a nucleation layer, located on a surface of one side of the base layer, wherein the material of the nucleation layer includes at least gallium nitride; and a first epitaxial layer, located on a surface of the nucleation layer away from the base layer, wherein the material of the first epitaxial layer includes at least gallium nitride.

[0027] In another exemplary embodiment, the quantum well structure includes: a second epitaxial layer, located on the surface of the groove of the base structure, wherein the material of the second epitaxial layer includes at least gallium nitride; a stacked structure, located on the surface of the second epitaxial layer away from the base structure; and a third epitaxial layer, located on the surface of the stacked structure away from the second epitaxial layer, wherein the material of the third epitaxial layer includes at least gallium nitride.

[0028] According to another embodiment of the present application, a semiconductor device is provided, including: a semiconductor structure manufactured by any one of the methods for manufacturing a semiconductor structure or any one of the semiconductor structures described.

[0029] Through the present application, since the non-polar surface or semi-polar surface can effectively relieve the piezoelectric polarization stress of epitaxial indium gallium nitride on the gallium nitride film, and compared with the non-groove structure, the gallium nitride in the groove structure is more likely to preferentially grow the non-polar surface or semi-polar surface, so the indium gallium nitride material grown in the groove has a small stress, and the indium in the indium gallium nitride is not easy to precipitate, thereby increasing the concentration of indium in the indium gallium nitride, and achieving the improvement of the light absorption rate of the gallium nitride material. Therefore, the problem of low light absorption rate of gallium nitride materials in the prior art can be solved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a flow chart of a method for manufacturing a semiconductor structure according to an embodiment of the present application;

[0031] Figure 2 is a schematic structural diagram of a substrate structure according to an embodiment of the present application;

[0032] Figure 3 is Figure 2 A schematic diagram of a quantum well structure formed on the basis of;

[0033] Figure 4 is a partial schematic diagram of a stacking structure according to an embodiment of the present application;

[0034] Figure 5 is a structural schematic diagram of another substrate structure according to an embodiment of the present application;

[0035] Figure 6 is a schematic structural diagram of a substrate structure according to an embodiment of the present application;

[0036] Figure 7 is a SEM image of a quantum well structure according to an embodiment of the present application;

[0037] Figure 8 is a schematic diagram of crystal growth of a semi-polar surface of gallium nitride according to an embodiment of the present application;

[0038] Fig. 9 is a TEM image of a quantum well structure according to an embodiment of the present application;

[0039] Fig.10 CL images of semiconductor structures according to embodiments of the present application, wherein (a) is a SEM image of an observed area under microscopic conditions, (b) is a schematic diagram of the light emission of an observed plane of the semiconductor structure under cathode ray irradiation, (c) is a CL image of a pyramid structure, and (d) is a microscopic schematic diagram of light emission under cathode ray irradiation;

[0040] Fig.11 is a light emission spectrum diagram of a semiconductor structure according to an embodiment of the present application;

[0041] Fig.12 is a PL diagram of a semiconductor structure according to an embodiment of the present application;

[0042] Fig.13 : The IV test curves of the photocatalytic performance of the semiconductor structure according to the embodiment of the present application, wherein (a) is the IV test curve of the photocatalytic performance of the GaN / InGaN quantum well nanopyramid and the 170nm nanocolumn sample under the full spectrum, (b) is the photocatalytic IV test curve of the two samples with the addition of a 420nm filter, and (c) is the photocatalytic water splitting current-voltage response curve of the GaN / InGaN quantum well nanopyramid under the full spectrum and the filter respectively;

[0043] Fig.14 It is a specific flow chart of a method for manufacturing a semiconductor structure according to an embodiment of the present application.

[0044] The above drawings include the following reference numerals:

[0045] 200, base structure; 201, groove; 203, quantum well structure; 204, stacking structure; 205, first material layer; 206, second material layer; 207, substrate; 208, oxide layer; 209, mask layer; 210, base layer; 211, nucleation layer; 212, first epitaxial layer; 213, mask portion; 214, second epitaxial layer; 215, third epitaxial layer. DETAILED DESCRIPTION

[0046] The embodiments of the present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0047] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0048] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0049] It should be understood that when an element (such as a layer, film, region, or substrate) is described as being "on" another element, the element may be directly on the other element, or there may be intermediate elements. Moreover, in the specification and claims, when it is described that an element is "connected" to another element, the element may be "directly connected" to the other element, or "connected" to the other element through a third element.

[0050] It should be clear that the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0052] It should be noted that the terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0053] In this embodiment, a method for manufacturing a semiconductor structure is provided. Figure 1 is a flow chart of a method for manufacturing a semiconductor structure according to an embodiment of the present application, such as Figure 1 As shown, the process includes the following steps:

[0054] Step S102, providing a substrate structure, wherein the substrate structure has a plurality of grooves, and the material of the substrate structure at least includes gallium nitride;

[0055] Specifically, the base structure is Figure 2As shown, the substrate structure 200 has a plurality of grooves 201. Two different regions can be formed inside and outside the above-mentioned groove 201 structure, wherein the region inside the groove 201 structure is prone to grow a structure that mainly exposes the GaN (10-11) crystal plane, and the region outside the groove 201 structure is not prone to grow a GaN structure. At the same time, in the process of growing the GaN pyramid structure, the specific surface area of ​​the planar GaN can be effectively increased, and the increase in its specific surface area can be used to increase the surface state density of GaN, thereby increasing the separation efficiency of photogenerated electron-hole pairs at the semiconductor electrolyte interface. At the same time, the rough surface of the GaN pyramid structure can scatter and reabsorb the incident light, thereby increasing the light absorption rate of the GaN material.

[0056] Step S104, forming a quantum well structure 203 on the surface of the groove of the substrate structure 200, and obtaining Figure 3 The structure shown in FIG. 1 , wherein the quantum well structure 203 at least includes a stacked structure, and a partial diagram of the stacked structure is shown in FIG. Figure 4 As shown, the stacked structure 204 includes alternately arranged first material layers 205 and second material layers 206, wherein one of the first material layers 205 is in direct contact with the surface of the groove, the material of the first material layer 205 includes at least gallium nitride, and the material of the second material layer 206 includes at least indium gallium nitride.

[0057] Specifically, the shape of the quantum well structure can be a pyramid structure or other pyramid structures, and this application does not impose specific restrictions. The manufacturing method of the semiconductor structure can be extended to the preparation process of device arrays such as light emitting diodes (Light Emitting Diode, referred to as LED), lasers, detectors, high electron mobility transistors (High Electron Mobility Transistor, referred to as HEMT) and insulated gate bipolar transistors (Insulated Gate Bipolar Transistor, referred to as IGBT).

[0058] Through the above steps, since the non-polar surface or semi-polar surface can effectively relieve the piezoelectric polarization stress of epitaxial indium gallium nitride on the gallium nitride film, and compared with the non-groove structure, the gallium nitride in the groove structure is more likely to preferentially grow the non-polar surface or semi-polar surface, so the indium gallium nitride material grown in the groove has a small stress, and the indium in the indium gallium nitride is not easy to precipitate, thereby increasing the concentration of indium in the indium gallium nitride, and achieving the improvement of the light absorption rate of the gallium nitride material. Therefore, the problem of low light absorption rate of gallium nitride materials in the prior art can be solved.

[0059] In one embodiment, the step S102 can be implemented by the following steps: step S1021, providing a substrate 207, wherein the material of the substrate 207 includes at least gallium nitride; step S1022, forming an oxide layer 208 on the surface of the substrate 207; step S1023, forming a mask layer 209 on the surface of the oxide layer 208 away from the substrate 207; step S1024, removing part of the mask layer 209, part of the oxide layer 208 and part of the substrate 207, so that part of the surface of the substrate 207 is exposed, and the remaining mask layer 209 forms a plurality of mask portions 213, forming a film such as Figure 5 The manufacturing process of the substrate structure is further simplified by the manufacturing method of the substrate structure including the substrate, the oxide layer and the mask layer.

[0060] Specifically, in addition to the above-mentioned steps of forming the base structure, a mask layer may be prepared first, and then the mask layer may be transferred onto the surface of the sample oxide layer.

[0061] In one embodiment, the step S1021 can be implemented as follows: step S10211, providing a base layer 210, wherein the material of the base layer 210 at least includes sapphire; step S10213, forming a nucleation layer 211 on the surface of the base layer 210, wherein the material of the nucleation layer 211 at least includes gallium nitride; step S10215, forming a first epitaxial layer 212 on the surface of the nucleation layer 211 away from the base layer 210, to obtain Figure 6 The substrate structure shown in the figure, wherein the material of the first epitaxial layer 212 at least includes gallium nitride. The manufacturing process of the substrate is further simplified by the above-mentioned method for forming a substrate including a base layer, a nucleation layer and a first epitaxial layer.

[0062] Specifically, sapphire is an aluminum oxide crystal, which, as a substrate material, has high chemical stability, high thermal stability, excellent optical properties, good electrical properties, high mechanical properties and good biocompatibility. The nucleation layer formed on the surface of the above-mentioned base layer is obtained by taking the sapphire c-plane as the substrate and growing along its

[0001] crystal direction. The above-mentioned nucleation layer refers to a thin atomic or molecular layer formed on the solid surface for crystal growth. Forming an epitaxial layer on the nucleation layer can further significantly improve the crystallinity and defect density of the crystal, while realizing a heterogeneous structure, thereby improving the performance of the device.

[0063] In another embodiment, after the above step S10211 and before the above step S10213, the above method further includes: step S10212, under the first predetermined temperature condition, using the first predetermined gas to clean the above base layer for a predetermined period of time. This method can further ensure the effectiveness of subsequent processes.

[0064] Specifically, the above-mentioned method of achieving surface cleaning by using the first predetermined gas can further remove impurities remaining on the surface of the substrate layer after the above-mentioned etching operation, improve the interface quality of the substrate layer, and facilitate the effectiveness of subsequent processes.

[0065] In order to further improve the cleaning effect of the base layer, the above-mentioned step S10212 can also be implemented in the following way: the above-mentioned first predetermined temperature ranges from 1000°C to 1200°C, the above-mentioned first predetermined gas includes at least hydrogen, and the above-mentioned predetermined time period is 8 to 15 minutes.

[0066] Specifically, in practical applications, using H2 as a carrier gas to clean sapphire at 1100°C for 10 minutes can produce better cleaning effects.

[0067] In another embodiment, the above step S10213 can be implemented by the following steps: Step S102131, introducing a second predetermined gas into the chamber where the above substrate layer is located under a second predetermined temperature condition to obtain the above nucleation layer. The method can further form the above nucleation layer on the surface of the substrate layer.

[0068] Specifically, the above-mentioned methods of forming the nucleation layer can be the following: uniform nucleation, non-uniform nucleation, contact nucleation, induced nucleation, and seed nucleation, etc. These methods of forming the nucleation layer can be used alone or in combination with each other, depending on the properties of the desired crystal and the application requirements. By controlling the formation of the nucleation layer, precise control of the crystal growth process can be achieved, thereby further improving its specific performance and application value.

[0069] In another embodiment, step S102131 further includes: the second predetermined temperature is in the range of 500° C. to 550° C., the second predetermined gas includes at least trimethylgallium and ammonia, and the thickness of the nucleation layer is in the range of 25 to 35 nm. This method can further improve the quality of the nucleation layer.

[0070] In practical applications, TMGa and NH3 can be introduced at a temperature of 525°C to deposit a GaN nucleation layer about 30nm thick on the sapphire surface, which can further improve the quality of the GaN nucleation layer.

[0071] In order to further improve the material selectivity of the epitaxial layer, step S10215 can be implemented in the following manner: step S102151, under a third predetermined temperature condition, forming a first sub-epitaxial layer on the surface of the nucleation layer away from the base layer, wherein the material of the first sub-epitaxial layer at least includes gallium nitride and the first sub-epitaxial layer is a non-doped material layer; step S102152, under a fourth predetermined temperature condition, forming a second sub-epitaxial layer on the surface of the first sub-epitaxial layer away from the nucleation layer, wherein the fourth predetermined temperature is lower than the third predetermined temperature, the material of the second sub-epitaxial layer at least includes gallium nitride and doped material, the thickness of the second sub-epitaxial layer is greater than the thickness of the first sub-epitaxial layer, and the first sub-epitaxial layer and the second sub-epitaxial layer form the first epitaxial layer.

[0072] Specifically, since the first sub-epitaxial layer is a non-doped material and the second sub-epitaxial layer is a non-doped material, through multiple epitaxial layers of different materials, the combination of different materials can be accurately controlled, and defects and discontinuities at the interface can be reduced, thereby further optimizing device performance.

[0073] In order to further improve the quality of the first sub-epitaxial layer and the second sub-epitaxial layer, step S10215 further includes: the third predetermined temperature ranges from 1000 to 1100° C., the thickness range of the first sub-epitaxial layer is 0.5 to 1.5 μm, the fourth predetermined temperature ranges from 1000 to 1100° C., the thickness range of the second sub-epitaxial layer is 1.5 to 2.5 μm, and the doping concentration range of the second sub-epitaxial layer is 2.5 to 3.5×10 18 cm −3 .

[0074] In a specific example, the temperature was then raised to 1060°C, and a non-doped GaN layer of approximately 1 µm thick was grown on the surface of the nucleation layer. Finally, the temperature was set to 1045°C, and the growth doping concentration was 3×10 18 cm −3 The approximately 2µm n-type doped GaN epitaxial layer.

[0075] In another embodiment, step S1022 can be implemented in the following manner: step S10221, under the conditions of a fifth predetermined temperature and a predetermined pressure, a third predetermined gas is introduced into the chamber where the substrate is located to form the oxide layer, wherein the material of the oxide layer at least includes silicon dioxide. The method can further quickly form the oxide layer on the surface of the substrate.

[0076] Specifically, the oxide layer can be deposited by any deposition method in the prior art, and this application does not limit it. In another specific embodiment, the oxide layer is formed by plasma enhanced chemical vapor deposition (PECVD). Compared with traditional chemical vapor deposition (CVD), PECVD technology has the advantages of high rate, low deposition temperature, good film uniformity, and few defects.

[0077] In another embodiment, step S10221 further includes: the fifth predetermined temperature is in the range of 150-250° C., the predetermined pressure is in the range of 900-1100 Pa, the third predetermined gas includes at least silicon source gas and oxidizing gas, and the thickness of the oxide layer is in the range of 150-250 nm. This method can further improve the film quality of the oxide layer.

[0078] In practical applications, 200nm polycrystalline SiO2 is grown on a planar GaN substrate by PECVD, with silane or tetraethoxysilane as the silicon source gas and oxygen as the oxidizing gas. The reaction pressure during the PECVD process is 1000 Pa. The RF frequency used in the PECVD process is 13.56MHz, the RF power is 100W, and the chamber temperature is 200℃.

[0079] In another specific embodiment, step S1024 can be implemented by the following steps: step S10241, removing part of the mask layer to expose part of the surface of the oxide layer to form a preliminary substrate, wherein the remaining mask layer forms a mask portion, and the material of the mask layer at least includes anodized aluminum; step S10242, introducing a fourth predetermined gas into the chamber where the preliminary substrate is located, and etching the oxide layer and the substrate using the mask portion as a mask to remove part of the oxide layer and part of the substrate and expose part of the substrate. This method can further quickly form the substrate structure.

[0080] Specifically, the mask adopts anodized aluminum with high porosity, good chemical stability, highly ordered pore structure, adjustable pore size and good mechanical properties. After the etching step, the impurities remaining on the substrate surface after the etching operation can be further removed by surface cleaning, thereby improving the interface quality of the substrate and facilitating the effectiveness of subsequent processes.

[0081] The above step S1024 further includes: the above fourth predetermined gas includes at least chlorine and boron trichloride. This method can further improve the etching rate in the above etching process.

[0082] In practical applications, the gases used for etching are Cl2 and BCl3, which generate high-density plasma at 300W. The RF power source controls the plasma power of Cl2 and BCl3 by applying a power of 13.56MHz and 40W, and makes it contact the GaN surface vertically from the generation area, physically bombarding and chemically reacting with the material. Since chlorine and boron trichloride can provide high selectivity, it means that they can etch on specific materials without affecting other materials. In addition, since chlorine and boron trichloride produce fewer by-products during the etching process, it helps to maintain the cleanliness of the etching environment, thereby improving product quality. The etching process using chlorine and boron trichloride can be precisely controlled by changing parameters such as gas concentration, pressure and temperature, thereby achieving precise control of etching depth and shape.

[0083] The above step S104 can be implemented by the following steps: step S1041, forming a second epitaxial layer 214 on the surface of the above groove of the above base structure 200, wherein the material of the above second epitaxial layer 214 at least includes gallium nitride; step S1042, forming the above stacked structure 204 on the surface of the above second epitaxial layer 214 away from the above base structure 200; step S1043, forming a third epitaxial layer 215 on the surface of the above stacked structure 204 away from the above second epitaxial layer 214, wherein the material of the above third epitaxial layer 215 at least includes gallium nitride, and the above second epitaxial layer 214, the above stacked structure 204 and the above third epitaxial layer 215 are formed as follows Figure 4 The method can further form the quantum well structure mentioned above quickly.

[0084] Specifically, the second epitaxial layer may be formed by a deposition method in the prior art, and this application does not impose any specific limitation thereto. Figure 7 FIG. 4 shows a top view of a quantum well structure obtained under a scanning electron microscope (SEM). Figure 7 As shown in the figure, the radius of the prepared GaN nano-pyramid is about 400nm and the period is about 450nm. The shape of the grown pyramid is relatively uniform, with a regular hexagonal structure and a growth density of about 4.94×10 12 m -2 . Figure 8The growth diagram of the GaN semipolar plane (10-11) crystal plane is shown. Since there is a difference in the electronegativity of Ga atoms and N atoms in the GaN polar plane (0001), their positive and negative charge centers do not overlap, so there is a strong polarization effect. In the (10-11) plane, Ga atoms and N atoms grow alternately, which can offset the stress accumulation caused by only Ga atom planes or N atom planes. In other words, in the (10-11) plane, the GaN crystal growth process grows at a lower binding energy than the polar plane. Since crystals tend to exist in a state of lower energy, during the selective area epitaxy (SAG) growth process, GaN is more likely to preferentially grow the (10-11) crystal plane, so that it self-assembles into the shape of a nano-pyramid. Fig. 9 FIG. 4 shows a transmission electron microscope (TEM) cross-sectional view of a quantum well nano-pyramid structure. Fig. 9 As shown in the figure, after the growth of GaN / InGaN quantum well heterojunction nano-pyramid structure is completed, the main exposed crystal planes are (0001) and (10-11) crystal planes. There are five pairs of light and dark stripes alternating with each other in the GaN quantum well pyramid structure, which is the quantum well structure of epitaxy during the growth of GaN material. The quantum well structure is mainly composed of an InGaN well with a thickness of about 5nm and a GaN quantum barrier with a thickness of about 8nm.

[0085] In another example, step S1041 can be implemented in the following manner: Step S10411, under a sixth predetermined temperature condition, a fifth predetermined gas is introduced into the chamber where the substrate structure is located to form the second epitaxial layer. This method can further quickly form a second epitaxial layer on the surface of the substrate structure.

[0086] Specifically, before forming the stacked structure, pre-forming a second epitaxial layer can reduce crystal defects and improve crystal quality, which is conducive to the formation of the quantum well structure. In addition, the second epitaxial layer can also serve as a buffer layer to help alleviate the stress caused by the lattice mismatch between materials, which helps to maintain the stability of the quantum well structure. The above-mentioned second epitaxial layer can be formed by metal-organic chemical vapor deposition (MOCVD). MOCVD technology can be carried out at a lower temperature, which is conducive to achieving precise control of the crystal growth process, thereby obtaining high-quality thin films.

[0087] In order to further improve the quality of the second epitaxial layer, step S10411 includes: the sixth predetermined temperature ranges from 1000 to 1100° C., the fifth predetermined gas includes at least trimethylgallium, ammonia and nitrogen, and the thickness range of the second epitaxial layer is 1.5 to 2.5 μm.

[0088] In practical applications, TMGa, NH3 and N2 gases can be introduced into the MOCVD chamber respectively, with a growth temperature of 1060°C to continue growing an n-GaN epitaxial layer of about 2µm.

[0089] In another embodiment, step S1042 can be implemented by the following steps: step S10421, a first forming step, introducing a sixth predetermined gas into the chamber where the second epitaxial layer is located to form the first material layer; step S10422, a second forming step, introducing the sixth predetermined gas into the chamber where the first material layer is located to form the second material layer, wherein the gas flow rate of the sixth predetermined gas in the second forming step is different from the gas flow rate of the sixth predetermined gas in the first forming step, and the thickness of the second material layer is greater than the thickness of the first material layer; step S10423, repeating the first forming step and the second forming step at least once in sequence until a predetermined number of times is reached to form the stacked structure. This method can further quickly form the stacked structure on the surface of the second epitaxial layer.

[0090] Specifically, the stacked structure can be formed by MOCVD technology. Since MOCVD has high repeatability, it can ensure that films produced in different batches have similar properties, which is conducive to the formation of the stacked structure.

[0091] Step S1042 further includes: the sixth predetermined gas includes at least trimethyl indium, the thickness of the first material layer is in the range of 4-6 nm, and the thickness of the second material layer is in the range of 6-8 nm. This method can further improve the generation quality of the stacked structure.

[0092] In practical applications, the staggered growth of GaN and InGaN layers is controlled by adding TMIn gas and controlling the gas flow rate, and seven pairs of quantum wells are grown, with the GaN and InGaN layers being 5nm and 7nm respectively.

[0093] Step S1043 includes: Step S10431, introducing a seventh predetermined gas into the chamber where the stack structure is located to form the third epitaxial layer. This method can further quickly form a third epitaxial layer on the surface of the stack structure.

[0094] Specifically, similar to the second epitaxial layer, forming a third epitaxial layer on the surface of the quantum well structure can protect the quantum well structure from the influence of the external environment, such as air, moisture, dust, etc., thereby ensuring the stability and performance of the quantum well structure. In addition, in some electronic devices, such as lasers, photodetectors, etc., it is necessary to form a pn junction to achieve the recombination of electron-hole pairs and the generation of photons. The epitaxial layer can be used to achieve this purpose by forming a p-type or n-type region through doping. In a multi-layer quantum well structure, the epitaxial layer can be used as an isolation layer between quantum wells to prevent the coupling of electrons between different quantum wells, thereby improving the performance and stability of the device.

[0095] Step S10431 further includes: the seventh predetermined gas at least includes bis(cyclopentadienyl)magnesium, trimethylgallium, ammonia and nitrogen, and the thickness of the third epitaxial layer is in the range of 30-60 nm. This method can further improve the quality of the third epitaxial layer.

[0096] In practical applications, bismuth magnesium, TMGa, NH3 and N2 gases are introduced to grow 50nm p-GaN to obtain the third epitaxial layer, and finally form the above-mentioned quantum well structure.

[0097] Fig.10 The cathode fluorescence cathode ray spectrum (Cathodeluminescence, abbreviated as CL) of a semiconductor structure manufactured by the above-mentioned semiconductor structure manufacturing method is shown, wherein (a) is a SEM image of the observed area under microscopic conditions, (b) shows the luminescence of the observed plane of the semiconductor structure under cathode ray irradiation, (c) is a pyramid structure used as a research object to observe its CL luminescence spectrum, and (d) is a microscopic image of luminescence under cathode ray irradiation. The non-polar side r-plane and the top c-plane of a single GaN quantum well nanopyramid begin to emit light under cathode ray irradiation. Fig.11The spectrum of pyramid luminescence is shown, and the CL peak at 365nm in the figure corresponds to the band edge peak of GaN (band gap is 3.4eV). Since the In component of the GaN / InGaN quantum well nano-pyramid c-face quantum well is 20%, its luminescence peak is about 420nm for blue light, which is consistent with the second peak in the figure. In the CL luminescence spectrum of the pyramid GaN, a new luminescence peak appears at a peak position of about 570nm, which is the yellow light peak presented by the r-face quantum well with a GaN crystal plane of (10-11). In other words, the r-face of the GaN pyramid has In enrichment during the preparation of the InGaN quantum well. When the GaN pyramid structure epitaxies the InGaN material, the radius of the In atom is larger than that of the Ga atom, which makes the In atom more inclined to grow at the bottom of the side of the GaN nano-column when it is adsorbed on the GaN nano-column. Then, it diffuses from the bottom to form the InGaN quantum well growth layer on the side. At the same time, due to the lattice mismatch between GaN and sapphire, the c-face of the GaN pyramid structure is subjected to a large lattice mismatch stress during the growth process. The side of the GaN pyramid can effectively relieve the stress caused by lattice mismatch. The material tends to be in the most stable and lowest energy state during the growth process. Therefore, in order to relieve the stress generated during the growth process, In atoms will also be enriched on the side of the pyramid structure. The above two effects cause In to be enriched on the side of the pyramid. It can be estimated from the CL spectrum that the band gap of the c-plane of the GaN / InGaN quantum well nanopyramid is about 2.88eV, and the band gap of InGaN on the (10-11) plane is about 2.18eV. According to Vegard's law: ,in, for The band gap of the material, x is the In component content, for The band gap of the material, for Band gap of the material. Calculations show that the In component content on the c-plane is about 19%, and the In component content on the (10-11) crystal plane is about 45%. It can be seen that the content of the In component on the side of the GaN pyramid structure is about 2.37 times that of the (0001) plane. This wider band gap can expand the absorption spectrum of GaN materials from ultraviolet and blue light to the yellow light spectrum during the photolysis of water. The broadening of the absorption spectrum will increase the absorption of light by GaN materials during the photolysis of water, thereby improving the efficiency of photolysis of water.

[0098] Fig.12The photoluminescence spectrum (PL) of the semiconductor structure obtained by the manufacturing method of the above semiconductor structure under 325nm laser irradiation is shown. Its peak distribution is basically consistent with the CL spectrum. The photoluminescence peak at 365nm is the band edge peak of GaN, the peak around 420nm is the InGaN quantum well luminescence peak on the (0001) crystal plane, and the luminescence peak near 541nm is the InGaN quantum well luminescence peak on the (10-11) crystal plane. Therefore, the above PL spectrum further illustrates that the GaN / InGaN quantum well nanopyramid can increase the In component of the side (10-11) crystal plane.

[0099] Fig.13 The photocatalytic performance IV test curve of the semiconductor structure obtained by the above-mentioned semiconductor structure manufacturing method is shown, wherein (a) is the photocatalytic performance IV test curve of GaN / InGaN quantum well nanopyramid and 170nm nanocolumn samples under full spectrum, (b) is the photocatalytic IV test curve of the two samples with the addition of 420nm filter, and (c) is the photocatalytic water splitting current voltage response curve of GaN / InGaN quantum well nanopyramid under full spectrum and filter respectively. Fig.13 As shown in (a), under full spectrum conditions, GaN nanorods and pyramid structures have significantly improved photocatalytic performance compared to planar GaN. The saturation photocurrents of the nanorod sample and pyramid structure reached 0.34 and 0.45 mA / cm, respectively. 2 The GaN pyramid structure has been improved by 32% compared to the nanocolumn sample. This is mainly because the InGaN layer in the GaN pyramid structure broadens the range of absorption of the xenon lamp spectrum. The InGaN layer on the (0001) crystal plane can absorb blue light around 420nm, and the (10-11) crystal plane can even absorb yellow light with a wavelength of around 541nm. Due to the addition of the InGaN layer, the absorption range of the GaN pyramid for light is increased, thereby improving the photocatalytic performance of the GaN pyramid in the full spectrum range. Fig.13 As can be seen in (b), after adding the 420nm filter, the GaN nanocolumns have no photocatalytic performance under light, and their IV curve is exactly the same as the IV curve without light. However, the GaN / InGaN quantum well nanopyramid structure still has certain photocatalytic performance after adding the filter, and the saturated photocurrent under light is about 0.13mA / cm 2 For the GaN pyramid structure, the turn-on voltages are -0.66 and -0.31 V under the full spectrum and 420 nm filter, respectively. This is because the photogenerated electron-hole pairs excited by ultraviolet light under full spectrum conditions have higher energy and are more easily driven to the semiconductor interface for photocatalytic reactions. Fig.13As can be seen from (c) in the figure, the GaN pyramid structure has a good light-dark current response under different lighting conditions.

[0100] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the implementation process of the method for manufacturing the semiconductor structure of the present application will be described in detail below in conjunction with specific embodiments.

[0101] This embodiment relates to a specific method for manufacturing a semiconductor structure, such as Fig.14 As shown, the following steps are included:

[0102] Step S1: providing a GaN substrate;

[0103] Step S2: forming SiO2 on the surface of the GaN substrate;

[0104] Step S3: transferring the prepared AAO film to the surface of SiO2;

[0105] Step S4: using AAO as a mask to etch SiO2 using ICP to form nanopores;

[0106] Step S5: forming InGaN nano-pyramids by SAG epitaxy.

[0107] In this embodiment, a semiconductor structure is also provided. Figure 3 A semiconductor structure provided according to an embodiment of the present application is as follows: Figure 3 As shown, the semiconductor structure includes:

[0108] A base structure 200, wherein the base structure 200 has a plurality of grooves;

[0109] Specifically, two different regions can be formed inside and outside the above groove structure, wherein the region inside the groove structure is prone to grow a structure that mainly exposes the GaN (10-11) crystal plane, and the region outside the groove structure is not easy to grow a GaN structure. At the same time, in the process of growing the GaN pyramid structure, the specific surface area of ​​the planar GaN can be effectively increased, and the increase in its specific surface area can be used to increase the surface state density of GaN, thereby increasing the separation efficiency of photogenerated electron-hole pairs at the semiconductor electrolyte interface. At the same time, the rough surface of the GaN pyramid structure can scatter and reabsorb the incident light, thereby increasing the light absorption rate of the GaN material.

[0110] The quantum well structure 203 is located in the above-mentioned groove. The above-mentioned quantum well structure 203 at least includes a stacked structure. The above-mentioned stacked structure includes a first material layer and a second material layer that are alternately arranged, wherein one of the above-mentioned first material layers is in direct contact with the surface of the above-mentioned groove, the material of the above-mentioned first material layer at least includes gallium nitride, and the material of the above-mentioned second material layer at least includes indium gallium nitride.

[0111] Specifically, the local diagram of the stacking structure is as follows: Figure 4 As shown, the stacked structure 204 includes alternately arranged first material layers 205 and second material layers 206, wherein one of the first material layers 205 is in direct contact with the surface of the groove, the material of the first material layer 205 includes at least gallium nitride, and the material of the second material layer 206 includes at least indium gallium nitride. The shape of the quantum well structure can be a pyramid structure or other pyramid structures, and the present application does not impose specific restrictions. The manufacturing method of the semiconductor structure can be extended to the preparation process of device arrays such as light emitting diodes (Light Emitting Diode, referred to as LED), lasers, detectors, high electron mobility transistors (High Electron Mobility Transistor, referred to as HEMT) and insulated gate bipolar transistors (Insulated Gate Bipolar Transistor, referred to as IGBT).

[0112] In the above semiconductor structure, since the non-polar surface or semi-polar surface can effectively relieve the piezoelectric polarization stress of epitaxial indium gallium nitride on the gallium nitride film, and compared with the non-groove structure, the gallium nitride in the groove structure is more likely to preferentially grow the non-polar surface or semi-polar surface, so the indium gallium nitride material grown in the groove has a small stress, and the indium in the indium gallium nitride is not easy to precipitate, thereby increasing the concentration of indium in the indium gallium nitride, and achieving the improvement of the light absorption rate of the gallium nitride material. Therefore, the problem of low light absorption rate of gallium nitride materials in the prior art can be solved.

[0113] In one embodiment, if Figure 5 As shown, the substrate structure includes: a substrate 207, wherein the material of the substrate 207 includes at least gallium nitride; an oxide layer 208, located on a surface of one side of the substrate 207; and a mask portion 213, located on a surface of the oxide layer 208 away from the substrate 207, and two adjacent mask portions 213 form the groove. The substrate structure includes a substrate, an oxide layer and a mask portion, which can further simplify the manufacturing process of the substrate structure.

[0114] Specifically, the base structure can be formed by sequentially forming a substrate, an oxide layer and a mask layer, and then etching; or the mask layer can be prepared first, and then the mask layer is transferred to the surface of the oxide layer to obtain the base structure.

[0115] In another specific embodiment, Figure 6As shown, the substrate includes: a base layer 210, wherein the material of the base layer 210 includes at least sapphire; a nucleation layer 211, located on a surface of one side of the base layer 210, wherein the material of the nucleation layer 211 includes at least gallium nitride; and a first epitaxial layer 212, located on a surface of the nucleation layer 211 away from the base layer 210, wherein the material of the first epitaxial layer 212 includes at least gallium nitride. The substrate includes the base layer, the nucleation layer and the first epitaxial layer, which can further simplify the manufacturing process of the substrate.

[0116] Specifically, sapphire is an aluminum oxide crystal, which, as a substrate material, has high chemical stability, high thermal stability, excellent optical properties, good electrical properties, high mechanical properties and good biocompatibility. The nucleation layer formed on the surface of the above-mentioned base layer is obtained by taking the sapphire c-plane as the substrate and growing along its

[0001] crystal direction. The above-mentioned nucleation layer refers to a thin atomic or molecular layer formed on the solid surface for crystal growth. Forming an epitaxial layer on the nucleation layer can further significantly improve the crystallinity and defect density of the crystal, while realizing a heterogeneous structure, thereby improving the performance of the device.

[0117] In order to further simplify the process of the above quantum well structure, Figure 4 As shown, the quantum well structure includes: a second epitaxial layer 214, located on the surface of the groove of the substrate structure 200, wherein the material of the second epitaxial layer 214 includes at least gallium nitride; a stacking structure 204, located on the surface of the second epitaxial layer 214 away from the substrate structure 200; and a third epitaxial layer 215, located on the surface of the stacking structure 204 away from the second epitaxial layer 214, wherein the material of the third epitaxial layer 215 includes at least gallium nitride.

[0118] Specifically, the formation method of the second epitaxial layer, the stacked structure and the third epitaxial layer can adopt the deposition method in the prior art, and the present application does not make specific restrictions. Before forming the stacked structure, pre-forming a second epitaxial layer can reduce crystal defects and improve crystal quality, thereby facilitating the formation of a quantum well structure. In addition, the second epitaxial layer can also be used as a buffer layer to help alleviate the stress caused by the lattice mismatch between materials, which helps to maintain the stability of the quantum well structure. Similar to the second epitaxial layer, forming a third epitaxial layer on the surface of the quantum well structure can protect the quantum well structure from the influence of the external environment, such as air, moisture, dust, etc., thereby ensuring the stability and performance of the quantum well structure. In addition, in some electronic devices, such as lasers, photodetectors, etc., it is necessary to form a pn junction to achieve the recombination of electron-hole pairs and the generation of photons. The epitaxial layer can be used to achieve this purpose by forming a p-type or n-type region by doping. In a multi-layer quantum well structure, the epitaxial layer can be used as an isolation layer between quantum wells to prevent the coupling of electrons between different quantum wells, thereby improving the performance and stability of the device.

[0119] An embodiment of the present invention provides a semiconductor device, including a semiconductor structure manufactured by any one of the above-mentioned semiconductor structure manufacturing methods or any one of the above-mentioned semiconductor structures.

[0120] Specifically, the semiconductor devices may be light emitting diodes (LEDs), lasers, detectors, high electron mobility transistors (HEMTs), insulated gate bipolar transistors (IGBTs), and other devices.

[0121] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the principles of the present application shall be included in the protection scope of the present application.

Claims

1. A method for manufacturing a semiconductor structure, characterized in that: include: Providing a substrate structure, wherein the substrate structure has a plurality of grooves, and the material of the substrate structure includes at least gallium nitride; A quantum well structure is formed on the surface of the groove of the base structure, wherein the quantum well structure at least includes a stacked structure, and the stacked structure includes first material layers and second material layers that are alternately arranged, wherein one of the first material layers is in direct contact with the surface of the groove, the material of the first material layer at least includes gallium nitride, and the material of the second material layer at least includes indium gallium nitride, Provide a base structure, including: Providing a substrate, wherein the material of the substrate includes at least gallium nitride; forming an oxide layer on the surface of the substrate; forming a mask layer on a surface of the oxide layer away from the substrate, wherein the mask layer is an AAO film; removing part of the mask layer, part of the oxide layer and part of the substrate to expose part of the surface of the substrate to form the base structure, A substrate is provided, comprising: Providing a base layer, wherein the material of the base layer at least includes sapphire; forming a nucleation layer on the surface of the base layer, wherein the material of the nucleation layer at least includes gallium nitride; A first epitaxial layer is formed on a surface of the nucleation layer away from the base layer, wherein a material of the first epitaxial layer at least includes gallium nitride.

2. The method according to claim 1, characterized in that After providing the base layer and before forming the nucleation layer on the surface of the base layer, the method further includes: Under a first predetermined temperature condition, the base layer is cleaned with a first predetermined gas for a predetermined period of time.

3. The method according to claim 2, characterized in that The first predetermined temperature ranges from 1000° C. to 1200° C., the first predetermined gas includes at least hydrogen, and the predetermined time period ranges from 8 to 15 minutes.

4. The method according to claim 1, characterized in that: The forming of a nucleation layer on the surface of the base layer comprises: A second predetermined gas is introduced into the chamber where the substrate layer is located under a second predetermined temperature condition to obtain the nucleation layer.

5. The method according to claim 4, characterized in that The second predetermined temperature ranges from 500° C. to 550° C., the second predetermined gas includes at least trimethylgallium and ammonia, and the thickness of the nucleation layer ranges from 25 to 35 nm.

6. The method according to claim 1, characterized in that Forming a first epitaxial layer on a surface of the nucleation layer away from the base layer comprises: Under a third predetermined temperature condition, forming a first sub-epitaxial layer on a surface of the nucleation layer away from the base layer, wherein the material of the first sub-epitaxial layer at least includes gallium nitride and the first sub-epitaxial layer is a non-doped material layer; Under a fourth predetermined temperature condition, a second sub-epitaxial layer is formed on a surface of the first sub-epitaxial layer away from the nucleation layer, wherein the fourth predetermined temperature is lower than the third predetermined temperature, a material of the second sub-epitaxial layer includes at least gallium nitride and a doping material, a thickness of the second sub-epitaxial layer is greater than a thickness of the first sub-epitaxial layer, and the first sub-epitaxial layer and the second sub-epitaxial layer form the first epitaxial layer.

7. The method according to claim 6, characterized in that The third predetermined temperature ranges from 1000 to 1100° C., the thickness range of the first epitaxial layer is 0.5 to 1.5 μm, the fourth predetermined temperature ranges from 1000 to 1100° C., the thickness range of the second epitaxial layer is 1.5 to 2.5 μm, and the doping concentration range of the second epitaxial layer is 2.5 to 3.5×10 18 cm −3 .

8. The method according to claim 1, characterized in that The step of forming an oxide layer on the surface of the substrate comprises: Under conditions of a fifth predetermined temperature and a predetermined pressure, a third predetermined gas is introduced into the chamber where the substrate is located to form the oxide layer, wherein the material of the oxide layer at least includes silicon dioxide.

9. The method according to claim 8, characterized in that The fifth predetermined temperature ranges from 150 to 250° C., the predetermined pressure ranges from 900 to 1100 Pa, the third predetermined gas includes at least silicon source gas and oxidation gas, and the thickness of the oxide layer ranges from 150 to 250 nm.

10. The method according to claim 1, characterized in that The removing of part of the mask layer, part of the oxide layer and part of the substrate comprises: Removing part of the mask layer to expose part of the surface of the oxide layer to form a preliminary substrate, wherein the remaining mask layer forms a mask portion, and the material of the mask layer includes at least anodized aluminum; A fourth predetermined gas is introduced into the chamber where the prepared substrate is located, and the oxide layer and the substrate are etched using the mask portion as a mask to remove a portion of the oxide layer and a portion of the substrate and expose a portion of the substrate.

11. The method according to claim 10, characterized in that The fourth predetermined gas includes at least chlorine and boron trichloride.

12. The method according to claim 1, characterized in that Forming a quantum well structure on the surface of the groove of the base structure, comprising: forming a second epitaxial layer on the surface of the groove of the base structure, wherein the material of the second epitaxial layer at least includes gallium nitride; forming the stacked structure on a surface of the second epitaxial layer away from the substrate structure; A third epitaxial layer is formed on a surface of the stacked structure away from the second epitaxial layer, the material of the third epitaxial layer at least includes gallium nitride, and the second epitaxial layer, the stacked structure and the third epitaxial layer form the quantum well structure.

13. The method according to claim 12, characterized in that The forming of a second epitaxial layer on the surface of the groove of the substrate structure comprises: Under a sixth predetermined temperature condition, a fifth predetermined gas is introduced into the chamber where the substrate structure is located to form the second epitaxial layer.

14. The method according to claim 13, characterized in that The sixth predetermined temperature ranges from 1000 to 1100° C., the fifth predetermined gas includes at least trimethylgallium, ammonia and nitrogen, and the thickness of the second epitaxial layer ranges from 1.5 to 2.5 μm.

15. The method according to claim 12, characterized in that The forming the stacked structure on a surface of the second epitaxial layer away from the substrate structure comprises: A first forming step, introducing a sixth predetermined gas into the chamber where the second epitaxial layer is located, to form the first material layer; a second forming step of introducing the sixth predetermined gas into the chamber where the first material layer is located to form the second material layer, wherein the gas flow rate of the sixth predetermined gas in the second forming step is different from the gas flow rate of the sixth predetermined gas in the first forming step, and the thickness of the second material layer is greater than the thickness of the first material layer; The first forming step and the second forming step are sequentially repeated at least once until a predetermined number of times is reached to form the stacked structure.

16. The method according to claim 15, characterized in that The sixth predetermined gas includes at least trimethyl indium, the thickness of the first material layer is in the range of 4 to 6 nm, and the thickness of the second material layer is in the range of 6 to 8 nm.

17. The method according to claim 12, characterized in that Forming a third epitaxial layer on a surface of the stacked structure away from the second epitaxial layer, comprising: A seventh predetermined gas is introduced into the chamber where the stack structure is located to form the third epitaxial layer.

18. The method according to claim 17, characterized in that The seventh predetermined gas at least includes bismuthocene magnesium, trimethylgallium, ammonia and nitrogen, and the thickness of the third epitaxial layer ranges from 30 to 60 nm.

19. A semiconductor structure, characterized in that: include: A base structure, wherein the base structure has a plurality of grooves; A quantum well structure is located in the groove, the quantum well structure at least includes a stacked structure, the stacked structure includes a first material layer and a second material layer arranged alternately, wherein one of the first material layers is in direct contact with the surface of the groove, the material of the first material layer at least includes gallium nitride, and the material of the second material layer at least includes indium gallium nitride, The base structure comprises: A substrate, wherein the material of the substrate at least includes gallium nitride; an oxide layer, located on a surface of one side of the substrate; The mask portion is located on the surface of the oxide layer away from the substrate, and two adjacent mask portions form the groove. The substrate comprises: A base layer, wherein the material of the base layer at least includes sapphire; A nucleation layer, located on a surface of one side of the base layer, wherein the material of the nucleation layer at least comprises gallium nitride; The first epitaxial layer is located on a surface of the nucleation layer away from the base layer, wherein the material of the first epitaxial layer at least includes gallium nitride.

20. The semiconductor structure according to claim 19, characterized in that The quantum well structure comprises: A second epitaxial layer is located on the surface of the groove of the base structure, wherein the material of the second epitaxial layer at least includes gallium nitride; A stacked structure, located on a surface of the second epitaxial layer away from the substrate structure; The third epitaxial layer is located on a surface of the stacked structure away from the second epitaxial layer, and the material of the third epitaxial layer at least includes gallium nitride.

21. A semiconductor device, characterized in that: include: A semiconductor structure manufactured by the method for manufacturing a semiconductor structure as described in any one of claims 1 to 18 or a semiconductor structure as described in any one of claims 19 to 20.