A photothermal aerogel enhanced by EOG and liquid metal Ga and preparation method thereof
By using ultrasonic method to prepare edge graphene oxide in a multi-layer arrangement structure prepared in solar seawater desalinator, the problem of easy oxidation and poor dispersion of liquid metal gallium is solved. , realizes efficient photothermal conversion and seawater evaporation, and improves seawater desalination efficiency and stability.
Patent Information
- Application Number
- CN202411248014.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Liquid metal gallium is easy to oxidize and has poor dispersion in photothermal conversion applications, and cannot form a continuous thermal conductivity network, which limits its application in solar seawater desalinators, and the water and heat transfer mechanisms in the pore structure are unclear.
Ultrasonic method is used to prepare edge graphene oxide (EOG) with multi-layer arrangement of "nut cake-like" structures coated with liquid metal gallium nanoparticles, and combined with polyvinyl alcohol (PVA) to form Ga@EOG with a vertical pore structure. /PVA aerogel is isolated from oxidation through the EOG cladding layer, forming a continuous thermal conductivity network to improve photothermal performance.
It significantly improves the thermal conductivity and photothermal performance of liquid metal gallium, enhances the evaporation rate and efficiency of seawater, reduces the energy required for evaporation, improves the stability and salt resistance of the aerogel, and achieves efficient photothermal conversion and Moisture transfer.
Smart Images

Figure CN118751167B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of aerogel preparation, and in particular to an EOG and liquid metal Ga-enhanced photothermal aerogel and a preparation method thereof. The photothermal aerogel is composed of liquid metal gallium (Ga)@edge oxidized graphene (EOG) (Ga@EOG) nanoparticles with a special multi-layered "nut cake-like" structure as photothermal filler and polyvinyl alcohol (PVA) as a matrix, and is a Ga@EOG / PVA aerogel with a vertical pore structure. Background Art
[0002] Due to the development of human society, the industrial, agricultural and domestic water use is increasing, the development of water resources is increasing, the natural runoff of rivers is decreasing, and the shortage of clean fresh water resources has become a serious challenge. The rising level of water pollution has made this problem more serious, and it is urgent to find a more reliable source of clean water to alleviate the water crisis. Traditional fresh water preparation methods, such as distillation, ion exchange, reverse osmosis and freezing, are limited by various factors such as high energy consumption, secondary pollution and complex operation process. Solar desalination technology provides a sustainable solution to these shortcomings, making it an ideal way to solve the problem of fresh water shortage. Solar steam generator (SSG) is a key component of solar desalination, which is environmentally friendly and energy-saving. These characteristics make it possible to solve the problem of water shortage without harming the environment. SSG is mainly composed of photothermal materials (such as conjugated polymers, metal nanoparticles, carbon materials and semiconductors) integrated with a hydrophilic polymer matrix. According to research, the evaporation rate of SSG water can be increased by optimizing light absorption, inhibiting heat loss, enhancing water supply, reducing evaporation enthalpy and constructing a cold evaporation surface. However, due to the low photothermal conversion efficiency and structural design defects, it is difficult to increase the evaporation rate of SSG.
[0003] Liquid metal (LM) refers to metal that is liquid at room temperature or higher. Liquid gallium (Ga) can exhibit reversible deformation and reconstruction capabilities that solid metals cannot achieve at room temperature due to its good fluidity and high electrical and thermal conductivity, while maintaining metal properties such as electrical and thermal conductivity, making it have broad application potential in fields such as heat dissipation media and flexible devices. Liquid gallium (Ga) nanoparticles use surface plasmon resonance (SPR) and interface effects to generate high temperature gradients through non-uniform heating, which can improve the photothermal conversion efficiency by promoting heat conduction and improving photothermal efficiency. This makes liquid gallium (Ga) nanoparticles have excellent photothermal conversion capabilities. However, liquid gallium (Ga) is easily oxidized, which affects its fluidity and chemical stability, and because of its high surface tension, it has poor dispersion in the matrix and cannot form a continuous thermal conductive network, which limits their application in SSG.
[0004] Inspired by the anisotropic tubular structure of natural wood in nature, many researchers have prepared aerogel-based seawater evaporators with vertical channels through directional freezing technology. This aerogel-based seawater evaporator mainly imitates the water transport process in plant cells. Since aerogels with vertical pores can act as tree-like conduits, they can enhance heat conduction and shorten the transmission path, reduce the evaporation enthalpy of water, and thus enhance the evaporation rate of seawater. However, the mechanism of water and heat transfer in aerogels with pore structures is still unclear.
[0005] In response to the above-mentioned thorny problems, a Chinese patent with publication number CN114597371A discloses a method for preparing liquid metal@rGO nanodroplets at room temperature liquid metal, wherein the steps for preparing liquid metal@rGO nanodroplets with core-shell structure are as follows: dispersing liquid metal in alcohol, ultrasonically treating at room temperature for 1 to 2 hours to obtain a liquid metal suspension, centrifuging the liquid metal suspension, taking the upper suspension, and drying to obtain liquid metal nanodroplets; dispersing liquid metal nanodroplets in alcohol, ultrasonically treating at room temperature for 30 to 40 minutes to obtain a liquid metal nanosuspension; adding graphene oxide to alcohol for ultrasonic pre-dispersion for 1 to 2 hours, then adding it to the obtained liquid metal nanosuspension, ultrasonically treating at room temperature for 1 to 2 hours, centrifuging, taking the upper suspension, and drying to obtain liquid metal@rGO nanodroplets with core-shell structure. The liquid metal surface of the above-mentioned patent contains an oxide layer because the patent does not treat the oxide layer of the liquid metal in the process of preparing liquid metal@rGO nanodroplets with core-shell structure.
[0006] The Chinese patent with publication number CN 116426028 A discloses a biomass aerogel-based seawater evaporator with controllable pore size and a preparation method thereof. The prepared biomass aerogel-based seawater evaporator has a highly ordered vertically arranged pore structure, which can quickly transport water and dissolve salt in seawater in time, thereby improving the stability of seawater evaporation. The Chinese patent with publication number CN 117069997 A discloses a nanofiber aerogel composite material for seawater desalination and a preparation method thereof. When the nanofiber aerogel composite material is used for seawater desalination, the aerogel matrix with a vertical pore structure contacts the seawater surface, and the magnetic microneedles of the photothermal conversion layer absorb sunlight energy and convert it into heat, so that water is transported along the vertical pores and converted into steam to escape, thereby achieving seawater desalination.
[0007] Although the above-mentioned technology can effectively promote the dispersion of liquid metal in the matrix and aerogels with vertical pore structures can effectively enhance the evaporation rate of seawater, the prepared liquid metal still has an oxide layer, which affects its dispersion, and the mechanism of water and heat transfer in aerogels with pore structures is still unclear. Summary of the invention
[0008] In view of the above-mentioned deficiencies in the prior art, the present invention aims to provide an EOG and liquid metal Ga enhanced photothermal aerogel and a preparation method, so as to solve the defects of the prior art that liquid metal is easy to oxidize, difficult to disperse, and cannot form a continuous thermal conductive network when used as a photothermal filler, heat dissipation medium, and flexible device. At the same time, the mechanism of aerogel with vertical pore structure in the water and heat transfer process is explored through COMSOL simulation.
[0009] To solve the above problems, the technical solution of the present invention is as follows:
[0010] The present invention uses non-toxic and biocompatible liquid metal gallium (Ga) and graphene (Gr) with many excellent properties as basic building units, obtains Ga nanoparticles by ultrasound, and uses electrochemical oxidation of Gr to prepare edge oxide graphene (EOG) as a coating layer to prepare Ga@EOG with a special multi-layered "nut cake-like" structure as a photothermal filler; then, polyvinyl alcohol (PVA) is used as a matrix to prepare Ga@EOG / PVA aerogel-based SSG with a vertical pore structure. Since the prepared photothermal filler Ga@EOG has a multi-layered "nut cake-like" structure, the multi-layered arrangement structure promotes strong multiple light scattering, and improves the light absorption efficiency by extending the absorption path inside the material. At the same time, the continuous heat conduction network constructed by EOG encapsulating Ga nanoparticles provides it with an efficient heat conduction path, which significantly enhances the heat transfer within the structure, thereby improving the thermal conductivity and photothermal performance of Ga@EOG. In addition, the surface plasmon resonance effect caused by Ga nanoparticles as core materials further optimizes the photothermal conversion efficiency by enhancing the surrounding electromagnetic field. Therefore, the prepared photothermal filler with a multi-layered "nut cake-like" structure achieves a photothermal synergistic enhancement effect. The Ga@EOG / PVA aerogel with a vertical pore structure shortens the path length of water to the evaporation surface due to its special vertical pore structure, enhances heat transfer, thereby reducing the energy required for evaporation and reducing the evaporation enthalpy. Therefore, the prepared Ga@EOG / PVA aerogel-based SSG has broad application prospects in seawater desalination.
[0011] The method for preparing the EOG and liquid metal Ga enhanced photothermal aerogel of the present invention specifically comprises the following steps:
[0012] S1. Blending polyvinylidene fluoride (PVDF), graphene (Gr) and N-methylpyrrolidone, and then drying in an oven to obtain a graphene electrode sheet; placing the graphene electrode in an electrolytic cell containing an ammonium sulfate ((NH4)2SO4) solution, and then applying a constant current to disperse edge oxide graphene (EOG), and obtaining EOG powder after washing, centrifugation and freeze drying;
[0013] S2, mixing EOG and deionized water by ultrasonication to obtain an EOG suspension;
[0014] S3, mixing EOG suspension, hydrochloric acid (HCl), liquid metal gallium (Ga) and ethanol by ultrasonication to obtain Ga@EOG suspension, and obtaining Ga@EOG powder after washing, centrifugation and drying;
[0015] S4. The product prepared in step S3 is mixed with polyvinyl alcohol (PVA) and dimethyl sulfoxide (DMSO) solution and stirred to obtain a suspension; the suspension is repeatedly frozen and thawed to obtain Ga@EOG / PVA hydrogel; then, the Ga@EOG / PVA hydrogel is freeze-dried to obtain Ga@EOG / PVA aerogel-based SSG.
[0016] As a further improvement of the present invention, in step S1, the mass ratio of PVDF to Gr is 1:10, the volume of N-methylpyrrolidone is 5 ml; the concentration of (NH4)2SO4 solution is 0.1 mol·mL -1 , applying a constant current of 40 mA·cm -2 and 0.017 Hz, time for 60 s; oven drying, condition temperature at 60℃, time for 24 h; freeze drying, condition temperature at -55℃, time for 24~48 h.
[0017] As a further improvement of the present invention, the power of the ultrasound in step S2 is 300 W, and the time is 30 min; the concentration of the EOG solution is 1 mg / mL.
[0018] As a further improvement of the present invention, the concentration of HCl in step S3 is 0.25 mol / L; the volume ratio of HCl to ethanol is 1:11, and the mass ratio of EOG to liquid metal gallium is 1:200; the ultrasonic conditions are consistent with S2; the concentration of Ga@EOG suspension is 40 mg / mL; the number of washing times is 2-5 times, and the solvent is anhydrous ethanol; the drying environment is a vacuum condition, the pressure is -0.1 MPa, the temperature is 60°C, and the time is 24 h; the mass ratio of liquid metal gallium to EOG is one of 200:1, 100:1, 50:1 or 10:1.
[0019] As a further improvement of the present invention, the mass ratio of Ga@EOG and PVA described in step S4 is 1:1; the temperature of the blending stirring is 90°C, and the time is 2 h; the number of repeated freezing and thawing is 3 times, the freezing temperature is -20°C, and the melting condition is room temperature; the freezing is carried out in a directional freezing device mold, the freezing source is liquid nitrogen, and the freezing time is 30 minutes; the freeze-drying is carried out in a freeze dryer, and the conditions are: vacuum environment, temperature is -50°C, and freezing time is 48~72h.
[0020] As a further improvement of the present invention, the EOG and liquid metal Ga enhanced photothermal aerogel comprises a polyvinyl alcohol (PVA) substrate and a photothermal filler; the photothermal aerogel has a vertical pore structure.
[0021] As a further improvement of the present invention, the EOG and liquid metal Ga enhanced photothermal aerogel, the photothermal filler is composed of graphene-modified liquid metal, the size of which is 10~20 μm; the graphene (Gr) is edge oxidized graphene (EOG), the size of which is 10~15 μm; the liquid metal is metal gallium (Ga), the particle size of which is 200~300 nm; the photothermal filler has a multi-layered "nut cake-like" structure.
[0022] As a further improvement of the present invention, the EOG and liquid metal Ga enhanced photothermal aerogel has a specific surface area of 56.3 cm 2 / g, density is 23.3 mg / cm 3 , pore size of 30-50 μm and porosity of 95.7%; the photothermal aerogel can absorb 97% of light at 250-2500 nm
[0023] As a further improvement of the present invention, the transmission speed of the aerogel with random pore structure in the photothermal aerogel is 2.6 μm / s, and the transmission speed of the aerogel with vertical pore structure is 5.7 μm / s. The photothermal aerogel can absorb 97% of the light at 250-2500 nm.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention adopts an electrochemical oxidation method to prepare edge oxide graphene (EOG). Since EOG has a certain antioxidant ability, the use of EOG to wrap Ga can effectively isolate oxygen and water in the air and prevent its oxidation. Therefore, the liquid metal suspension obtained by the present invention has good colloidal stability. At the same time, since the Ga@EOG powder obtained by modifying Ga with EOG presents a black hue of pure EGO, its light absorption ability is significantly improved.
[0026] (2) The Ga@EOG powder prepared by the present invention has high thermal conductivity and excellent photothermal performance. Ga nanoparticles are wrapped by EOG sheets to form a multi-layered "nut cake-like" structure with a size of 10~20μm. The multi-layered structure promotes strong multiple light scattering and improves the light absorption efficiency by extending the absorption path inside the material. At the same time, the continuous thermal conductive network constructed by EOG wrapping Ga nanoparticles provides them with an efficient heat conduction path, which significantly enhances the heat transfer within the structure, thereby improving the thermal conductivity and photothermal performance of Ga@EOG. In addition, the surface plasmon resonance effect caused by Ga nanoparticles as core materials further optimizes the photothermal conversion efficiency by enhancing the surrounding electromagnetic field.
[0027] (3) The Ga@EOG / PVA aerogel-based SSG prepared in the present invention has a unidirectional highly ordered vertically arranged pore structure and significant water absorption performance. Under the combined effect of this bionic structure and the excellent hydrophilicity of the PVA matrix, it can quickly transport water, reduce the evaporation enthalpy of SSG and the energy required for evaporation, and increase the evaporation rate and efficiency of seawater. At the same time, these characteristics can improve the stability and salt resistance of the aerogel in the seawater desalination process.
[0028] (4) The Ga@EOG / PVA aerogel-based SSG prepared in the present invention has a low density (23.3~46.5mg / cm 3 ), ultra-high specific surface area (56.3 cm 3 / g), high porosity (95.7%), small pore size (30~50μm) and high light absorption (70~97.5%).
[0029] (5) The present invention uses COMSOL simulation to find that the transmission speed of aerogels with random pore structures is 2.6 μm / s, and the transmission speed of aerogels with vertical pore structures is 5.7 μm / s. This indicates that aerogels with vertical pore structures of tree trunk xylem vessels can quickly transfer heat and moisture, and that the bionic structure and hydrogen bonds reduce the evaporation rate, thereby improving the evaporation rate and efficiency of photothermal aerogels. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a preparation flow chart of a method for preparing EOG and liquid metal Ga enhanced photothermal aerogel;
[0031] Figure 2 (a) A physical picture of the EOG, Ga and Ga@EOG suspensions prepared in Example 1 of the present invention;
[0032] Figure 2(b) Physical pictures of Ga / PVA and Ga@EOG / PVA photothermal aerogels prepared in Example 1 and Comparative Example 7;
[0033] Figure 3 (a) and (b) are transmission electron microscopy (TEM) and energy dispersive spectroscopy (EDS) images of the Ga@EOG dispersion prepared in Example 1, respectively;
[0034] Figure 4 (a), (b), (c) and (d) are the corresponding SEM images of the surface and cross-section of the Ga@EOG / PVA aerogel obtained in Example 1 in different directions;
[0035] Figure 5 (a), (b), (c) and (d) are Comsol simulation schematics of the water transport process of Ga@EOG / PVA aerogel-based SSG prepared in Example 1;
[0036] Figure 6 (a) and (b) are Comsol simulation schematic diagrams of the heat transfer process of Ga@EOG / PVA aerogel-based SSG prepared in Example 1; DETAILED DESCRIPTION
[0037] The present invention provides a method for preparing edge graphene oxide and liquid metal gallium enhanced photothermal aerogel. In order to make the purpose, technical scheme and advantages of the present invention clearer and more specific, the present invention is further described in combination with specific embodiments and drawings.
[0038] Example 1
[0039] like Figure 1 As shown, a method for preparing edge-oxidized graphene and liquid metal gallium enhanced photothermal aerogel of the present invention is prepared by the following steps:
[0040] Step 1: 0.3 g PVDF, 3 g Gr and 5 mL N-methylpyrrolidone were mixed and dissolved, and dried at 60 °C for 24 h to prepare a graphene electrode sheet;
[0041] Step 2: Place the graphene electrode in 0.1 mol mL -1 In the electrolytic cell of (NH4)2SO4 solution, 40 mA cm -2 and a constant current of 0.017 Hz for 60 s to obtain an EOG suspension, which was then centrifuged and washed before being placed in a freeze dryer and dried at -55 °C for 24 to 48 h to obtain EOG powder;
[0042] Step 3: 15 mg EOG and 15 ml deionized water were mixed in a beaker and ultrasonically dispersed at an ultrasonic intensity of 300 W for 30 min to obtain an EOG suspension with a concentration of 1 mg / ml;
[0043] Step 4: Add 3 ml EOG solution (1 mg / mL), 1 ml HCl (0.25 M) and 0.1 ml liquid Ga into 11 ml ethanol and ultrasonically treat at 300 W for 30 min to obtain a Ga@EOG suspension with a concentration of 40 mg / mL. Then, centrifuge and wash with anhydrous ethanol for 2 to 5 times. After drying in a vacuum oven at a pressure of -0.1 MPa and a temperature of 60 °C for 24 h, Ga@EOG powder was obtained.
[0044] Step 5: 0.6 g Ga@EOG powder, 1.0 g PVA and 49 g DMSO were blended and mechanically stirred at 400 rpm at 90 °C for 2 h to obtain a mixed suspension;
[0045] Step 6: The mixed suspension obtained in step 4 was repeatedly frozen and thawed at -20°C and room temperature to obtain Ga@EOG / PVA hydrogel. The hydrogel was then placed in a special one-way freezing mold, frozen with liquid nitrogen for 30 minutes, and then placed in a vacuum environment and freeze-dried in a freeze dryer at -50°C for 48 to 72 hours to obtain Ga@EOG / PVA aerogel-based SSG.
[0046] The Ga@EOG suspension prepared in Example 1 and the obtained Ga@EOG / PVA aerogel-based SSG were observed in real life, and the results were as follows: Figure 2 (a) Right and Figure 2 (b) As shown on the right.
[0047] The Ga@EOG dispersion prepared in Example 1 was subjected to transmission electron microscopy and energy spectrum analysis, and the results are as follows: Figure 3 As shown in (a) and (b).
[0048] Figure 3 It revealed the successful preparation of EOG-modified Ga nanoparticles to obtain Ga@EOG powder with a size of 10~20μm, in which Ga nanoparticles were encapsulated inside EOG sheets. EOG effectively connected isolated Ga nanoparticles to form a special "nut pie-like" core-shell structure, effectively forming a continuous thermal conductive network.
[0049] The surface and cross-sectional morphology of the Ga@EOG / PVA aerogel-based SSG prepared in Example 1 were observed by scanning electron microscopy. The aerogel surface showed a unidirectional pore structure, and the aerogels perpendicular to the evaporation surface and vertical pores were arranged in order. The results are as follows: Figure 4 As shown in (a), (b), (c) and (d).
[0050] The Ga@EOG / PVA aerogel-based SSG prepared in Example 1 was subjected to Comsol simulation, and the results were as follows: Figure 5 (a), (b), (c) and (d) and Figure 6 As shown in (a) and (b).
[0051] In the Comsol simulation results, the transmission speed of the aerogel with random pore structure in the photothermal aerogel is 2.6 μm / s, and the transmission speed of the aerogel with vertical pore structure is 5.7 μm / s. Figure 5 (ad) reveals that, unlike random pore structure aerogels, vertical pore structure aerogels have clear and simple water transport paths, thus having a higher transport speed. Figure 6 (ab) reveal that unlike random pore structure aerogels, aerogels with vertical pores are arranged in an orderly manner, and heat is conducted more efficiently in the vertical direction, further forming a more coherent thermal channel.
[0052] The density of the Ga@EOG / PVA aerogel-based SSG prepared in Example 1 was measured by weighing method at room temperature and pressure, and the porosity was measured by mass density method. The density and porosity were 38.2 mg / cm 3 and 95.7%.
[0053] The surface morphology of the Ga@EOG / PVA aerogel-based SSG prepared in Example 1 was observed by scanning electron microscopy. Figure 4 As shown in (a, b), the pore size is 30~50μm.
[0054] Comparative Examples 1 to 4
[0055] Comparative Examples 1 to 4 provide a method for preparing edge graphene oxide and liquid metal gallium enhanced photothermal aerogel. Compared with Example 1, the difference is that in step 5, the mass ratios of Ga@EOG powder and PVA are 0.2, 0.4, 0.8 and 1, respectively, and the rest are the same as Example 1 and will not be repeated here.
[0056] Comparative Example 5
[0057] A method for preparing edge graphene oxide and liquid metal gallium enhanced photothermal aerogel, the specific steps are as follows:
[0058] Step 1: 1.0 g PVA and 49 g DMSO were mixed and mechanically stirred at 400 rpm at 90°C for 2 h to obtain a PVA suspension with a mass fraction of 2 wt%;
[0059] Step 2: The same as step 6 in Example 1, which will not be repeated here, to obtain a single PVA aerogel.
[0060] Comparative Example 6
[0061] Comparative Example 6 provides a method for preparing edge graphene oxide and liquid metal gallium enhanced photothermal aerogel. Compared with Example 1, the difference is that steps 3 and 4 are removed, and in step 5, the added Ga@EOG powder is replaced with EOG powder. The rest is roughly the same as Example 1 and will not be repeated here to obtain EOG / PVA aerogel.
[0062] Comparative Example 7
[0063] Comparative Example 7 provides a method for preparing edge graphene oxide and liquid metal gallium enhanced photothermal aerogel. Compared with Example 1, the difference is that steps 1 to 3 are removed, and in step 4, 3 ml of EOG solution (1 mg / mL) is not added. The rest is roughly the same as Example 1 and will not be repeated here. Ga / PVA aerogel is obtained, and its physical figure is as shown in Figure 2 (b) As shown on the left.
[0064] In summary, the present invention successfully prepared Ga@EOG / PVA aerogel-based SSG with excellent photothermal water purification ability using Ga, EOG and PVA as raw materials. EOG synthesized by electrochemical oxidation effectively encapsulates Ga nanoparticles into a unique multi-layer "nut cake-like" core-shell structure, promoting the formation of a thermal conductive network, thereby achieving synergistic photothermal enhancement. In addition, experimental and COMSOL simulation results show that aerogels with vertical pore structures of tree trunk xylem vessels can quickly transfer heat and moisture. The bionic structure and hydrogen bonds reduce the evaporation rate and increase the evaporation rate and efficiency. Therefore, Ga@EOG / PVA aerogels exhibit a light absorption rate of up to 97.5%. Overall, Ga@EOG / PVA aerogel-based SSG provides a viable solution to water purification challenges, combining high efficiency with wide applicability, and can be used to improve the quality and safety of human drinking water.
Claims
1. A method for preparing EOG and liquid metal Ga enhanced photothermal aerogel, characterized in that: The following steps are involved: S1. Blending polyvinylidene fluoride (PVDF), graphene (Gr) and N-methylpyrrolidone, and then drying in an oven to obtain a graphene electrode sheet; placing the graphene electrode in an electrolytic cell containing an ammonium sulfate ((NH4)2SO4) solution, and then applying a constant current to disperse edge oxide graphene (EOG), and obtaining EOG powder after washing, centrifugation and freeze drying; in step S1, the mass ratio of PVDF to Gr is 1:10, the volume of N-methylpyrrolidone is 5 ml; the concentration of the (NH4)2SO4 solution is 0.1 mol·mL -1 , applying a constant current of 40 mA·cm -2 and 0.017 Hz, time for 60 s; oven drying, condition temperature at 60℃, time for 24 h; freeze drying, condition temperature at -55℃, time for 24~48 h S2, mixing EOG and deionized water by ultrasonication to obtain an EOG suspension; in the step S2, the ultrasonic power is 300W and the time is 30 min; the concentration of the EOG suspension is 1 mg / mL; S3, ultrasonically mixing EOG suspension, hydrochloric acid (HCl), liquid metal gallium (Ga) and ethanol to obtain Ga@EOG suspension, and obtaining Ga@EOG powder after washing, centrifugation and drying; the concentration of HCl in step S3 is 0.25 mol / L; the volume ratio of HCl to ethanol is 1:11, and the mass ratio of EOG to liquid metal gallium is 1:200; the ultrasonic conditions are consistent with S2; the concentration of Ga@EOG suspension is 40 mg / mL; the washing times are 2 to 5 times, and the solvent is anhydrous ethanol; the drying environment is vacuum conditions, the pressure is -0.1 MPa, the temperature is 60°C, and the time is 24 h; S4, the product prepared in step S3 is blended and stirred with polyvinyl alcohol (PVA) and dimethyl sulfoxide (DMSO) solution to obtain a suspension; the suspension is repeatedly frozen and thawed to obtain Ga@EOG / PVA hydrogel; then, the Ga@EOG / PVA hydrogel is freeze-dried to obtain a Ga@EOG / PVA aerogel-based solar steam generator, wherein the mass ratio of Ga@EOG and PVA in step S4 is 0.6:1; the blending temperature is 90°C and the time is 2 h; the number of repeated freeze-thaw cycles is 3 times, the freezing temperature is -20°C, and the melting condition is room temperature; the freezing is carried out in a directional freezing mold, the freezing source is liquid nitrogen, and the freezing time is 30 min; the freeze-drying is carried out in a freeze dryer under the conditions of a vacuum environment, a temperature of -50°C, and a freezing time of 48~72 h.
2. An EOG and liquid metal Ga enhanced photothermal aerogel, characterized in that: The preparation method according to claim 1 is used to obtain the 3. The EOG and liquid metal Ga enhanced photothermal aerogel according to claim 2, characterized in that: The photothermal aerogel comprises a polyvinyl alcohol (PVA) substrate and a photothermal filler; the photothermal aerogel has a vertical pore structure.
4. The EOG and liquid metal Ga enhanced photothermal aerogel according to claim 2, characterized in that: The photothermal filler is composed of graphene-modified liquid metal with a size of 10-20 μm; the graphene (Gr) is edge oxide graphene (EOG) with a size of 10-15 μm; the liquid metal is metal gallium (Ga) with a particle size of 200-300 nm; the photothermal filler has a multi-layered "nut cake-like" structure.
5. The EOG and liquid metal Ga enhanced photothermal aerogel according to claim 2, characterized in that: The specific surface area of the aerogel is 56.3 cm 2 / g, density is 23.3 mg / cm 3 , pore size of 30-50 μm and porosity of 95.7%; the photothermal aerogel can absorb 97% of light at 250-2500 nm.
6. The EOG and liquid metal Ga enhanced photothermal aerogel according to claim 2, characterized in that: The transmission speed of the aerogel with random pore structure in the photothermal aerogel is 2.6 μm / s, and the transmission speed of the aerogel with vertical pore structure is 5.7 μm / s.