A high-strength ureteral metal stent with antibacterial and anti-crusting functions

By using high-strength antibacterial stainless steel wire containing copper and nitrogen elements in the ureteral stent, the problem of urinary tract infection and encrustation is solved, the mechanical properties and biocompatibility of the stent are improved, and efficient prevention and treatment of urinary tract infection is achieved. scale inhibition.

CN118403226BActive Publication Date: 2024-10-15SUZHOU SILVAN MEDICAL DEVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410880757.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-15
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

Existing ureteral stents are prone to urinary tract infection and encrustation problems during use, and are difficult to meet mechanical properties, biocompatibility and economic requirements.

Method used

The ureteral metal stent is made of densely wound high-strength antibacterial stainless steel wire containing copper and nitrogen. Its mechanical properties and corrosion resistance are improved through specific processing, and it inhibits the adhesion and growth of Staphylococcus aureus and urease-positive bacteria. .

Benefits of technology

The ureteral metal stent that achieves high strength, antibacterial and encrustation-inhibiting functions significantly reduces the risk of urinary tract infection and scaling while improving the biocompatibility and corrosion resistance of the stent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118403226B_ABST
    Figure CN118403226B_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a high-strength ureteral metal stent with antibacterial and anti-crusting functions, which is made of medical high-strength antibacterial stainless steel wire, and the chemical composition of the material is (weight percentage): Mo: 2~3%, Ni: 12~14%, Cr: 16~18%, Cu: 3~5%, N: 0.10~0.20%, C≤0.03%, Si≤1.00%, Mn≤1.50%, S≤0.01%, P≤0.01%, and the balance is Fe. By adding appropriate amounts of copper and nitrogen elements and combining the ureteral metal stent made by special technology, on the basis of ensuring its excellent tissue compatibility, its mechanical properties and corrosion resistance are further improved, and the adhesion of bacteria and the formation of biofilm are reduced from the source, especially Staphylococcus aureus and urease-positive bacteria are inhibited or killed, thereby overcoming the scaling and related urinary tract infection problems on the ureteral metal stent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to application of a novel medical metal material in a ureteral metal stent, in particular to a high-strength ureteral metal stent with antibacterial and crust-inhibiting functions. Background Art

[0002] Urinary tract stones are a common disease in urology. Currently, minimally invasive surgeries such as ureteral rigid / flexible endoscopic lithotripsy and percutaneous nephrolithotomy are commonly used methods for treating urinary tract stones. After surgery, it is recommended to routinely place a ureteral stent to support the ureter to promote the excretion of urine and stones, and prevent the occurrence of problems such as ureteral obstruction.

[0003] Ureteral stents have become an indispensable medical consumable in clinical practice, and most of the stents currently used are made of metal or polymer. An ideal ureteral stent should have the following characteristics: good mechanical properties to provide the necessary support; good biocompatibility, no immune rejection reaction in the human body; less biofilm formed, reducing the adhesion of bacteria and proteins on the surface; simple insertion and easy removal; opaque under B-ultrasound or X-ray; economical price, reducing the overall economic burden, etc.

[0004] The coated ureteral stents currently under development have advantages such as good mechanical support and the ability to prevent polyps from growing inward, but they are extremely expensive and have disadvantages such as difficulty in removal at a later stage. Drug-eluting stents can deliver drugs to specific locations, avoiding the problem of systemic administration, but the drug release rate of current drug-eluting stents is too fast to achieve the effect of sustained-release therapy. Tissue engineering scaffolds have also been a research hotspot in recent years, but are still in the research process and have not yet been applied clinically. There are also problems such as difficulty in obtaining seed cells, proliferation capacity that does not meet clinical needs, and overly complicated process processes. There is currently no ureteral stent that can fully meet all the requirements of the above ideal stents.

[0005] At present, the most common pathogens of ureteral stent-associated urinary tract infection are mainly Gram-negative bacteria (Escherichia coli, Klebsiella pneumoniae, Pseudomonas aeruginosa and Proteus mirabilis) and Gram-positive bacteria (Enterococcus faecalis and Staphylococcus aureus). Studies have found that these pathogens can float and aggregate in the urinary tract to induce infection, and some pathogens can also adhere to the surface of the double J tube. Under the influence of urine, blood and surrounding tissues in the human body, ions and glycoproteins are deposited on the surface of the double J tube, and a conditional membrane can be formed within a few minutes. The conditional membrane is conducive to the continuous adhesion of bacteria, the formation of microcolonies, and gradually forming a mature structure with the extracellular matrix secreted by it. At the same time, other microorganisms are constantly added through quorum sensing, and finally form a complex biofilm system with multi-microorganisms and multi-forms coexisting. Biofilm not only reduces the sensitivity of pathogens to antibiotics, but also greatly enhances the resistance of pathogens due to the transfer of resistance genes.

[0006] Therefore, it is particularly important to curb the formation of biofilms. It is urgent to develop ureteral stents made of new materials, hoping to inhibit urinary tract planktonic bacteria and prevent biofilm formation, thereby reducing the incidence of ureteral stent-related urinary tract infections.

[0007] On the other hand, although the application of ureteral stents has improved the prognosis of stone treatment surgery, it has also faced a series of challenges. Among them, the easy crusting of the stent surface is a common problem of existing ureteral stents on the market. The currently known pathological mechanism of ureteral stent crusting is that urease-positive microorganisms decompose urea, causing the pH value of urine to increase, which in turn promotes the aggregation and growth of crystals formed in the urine on the stent wall. Severe stent crusting will affect the drainage of urine after surgery, and even cause urinary tract mucosal damage, hematuria, urinary tract obstruction and difficulty in stent removal.

[0008] Therefore, for the two major problems of ureteral stent-related urinary tract infection and ureteral stent surface crusting, the fundamental way to solve the problem is to reduce bacterial adhesion and biofilm formation from the source, especially to inhibit or kill Staphylococcus aureus and urease-positive bacteria, so as to overcome the problems of scaling on ureteral stents and related urinary tract infections. Summary of the invention

[0009] The purpose of the present invention is to provide a high-strength ureteral metal stent with antibacterial and anti-crusting functions. Through a unique material composition design, appropriate addition of copper and nitrogen elements, and combined with a special process to make a ureteral metal stent, while ensuring its excellent tissue compatibility, its mechanical properties and corrosion resistance are further improved. The tensile strength of the ureteral metal stent can reach 2300~2800MPa, and the pitting potential is ≥500 mV, so that it can provide excellent support and corrosion resistance during use. On the other hand, the ureteral metal stent reduces bacterial adhesion and biofilm formation from the source, especially inhibits or kills Staphylococcus aureus and urease-positive bacteria, thereby overcoming the scaling on the ureteral metal stent and the related urinary tract infection problems.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] A high-strength ureteral metal stent with antibacterial and anti-crusting functions is made of medical high-strength antibacterial stainless steel wire, and the chemical composition of the ureteral metal stent is as follows (wt.%): Mo: 2-3%, Ni: 12-14%, Cr: 16-18%, Cu: 3-5%, N: 0.10-0.20%, C≤0.03%, Si≤1.00%, Mn≤1.50%, S≤0.01%, P≤0.01%, and the balance is Fe;

[0012] Made by a method comprising the following steps:

[0013] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0014] Step 2, forging the stainless steel ingot in step 1 into a rod;

[0015] Step 3, hot rolling the stainless steel bar in step 2 into wire rod;

[0016] Step 4, cold drawing the stainless steel wire rod in step 3 to gradually draw it into stainless steel wire;

[0017] Step 5: performing intermediate annealing and pickling on the stainless steel wire in step 4, and then cold drawing again;

[0018] Step 6: Performing medium-temperature microstructure control heat treatment on the stainless steel wire in step 5;

[0019] Step 7, performing a deformation strengthening treatment on the stainless steel wire after the organization adjustment in step 6;

[0020] Step 8, performing low temperature structure control heat treatment on the stainless steel wire in step 7;

[0021] Step nine, performing secondary deformation strengthening treatment on the stainless steel wire in step eight;

[0022] Step 10, pickling the stainless steel wire in step 9 to obtain high-strength antibacterial stainless steel wire;

[0023] Step 11, performing vacuum vertical heat straightening on the stainless steel wire in step 10;

[0024] According to the needs, the heat-straightened stainless steel wire is densely wound and finely processed into a high-strength ureteral metal stent with antibacterial and anti-crusting functions.

[0025] In some embodiments, in step 2, the forging temperature is 1150-1250°C.

[0026] In some embodiments, in step three, the hot rolling temperature is 1100-1200°C.

[0027] In some embodiments, in step 4, the cold drawing is performed step by step in five times, and the deformation amount of each cold drawing is 20-25%.

[0028] In some embodiments, in step five, the intermediate annealing temperature is 850-1050° C., pickling is performed after annealing, and then cold drawing is performed again with a deformation amount of 50-70%.

[0029] In some embodiments, in step six, the medium temperature organization heat treatment temperature is regulated to be 600-700°C.

[0030] In some embodiments, in step seven, the deformation amount of the primary deformation strengthening is 40-70%.

[0031] In some embodiments, in step eight, the low temperature tissue heat treatment temperature is regulated to be 300-500°C.

[0032] In some embodiments, in step nine, the deformation amount of the secondary deformation strengthening is 80-95%.

[0033] In some embodiments, in step ten, the diameter of the obtained high-strength antibacterial stainless steel wire is 0.05~1mm.

[0034] In some embodiments, in step eleven, the heating temperature is 640-770°C.

[0035] The tensile strength of the obtained ureteral metal stent can reach 2300~2800MPa.

[0036] The obtained ureteral metal stent had a cytotoxicity rating of ≤1 and a pitting potential of ≥500 mV.

[0037] The obtained ureteral metal stent can provide a relative antibacterial rate of more than 90% by comparing the co-culture results of the current ureteral metal stents on the market with Staphylococcus aureus and urease-positive bacteria.

[0038] The beneficial effects of the present invention are:

[0039] (1) The present invention aims to solve the pain points in the application of ureteral metal stents. Through unique materials and preparation processes, the present invention ensures that the ureteral metal stent has better tissue compatibility and further improves its mechanical properties and corrosion resistance, so that it can provide excellent support and corrosion resistance during use. At the same time, it reduces bacterial adhesion and biofilm formation from the source, especially inhibits or kills Staphylococcus aureus and urease-positive bacteria, thereby overcoming the scaling on the ureteral metal stent and the related urinary tract infection problems.

[0040] (2) In the production of the above-mentioned ureteral metal stent, the required equipment and processing technology are mature and stable and can meet the requirements of mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the ureteral metal stent of the present invention. DETAILED DESCRIPTION

[0042] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0043] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0044] Example 1

[0045] In this embodiment, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 4.5%, N: 0.15%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe. The preparation method is as follows:

[0046] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0047] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0048] Step 3, hot rolling the stainless steel bar in step 2 into wire rod, with the hot rolling temperature being 1150° C.;

[0049] Step 4: cold-draw the stainless steel wire rod in step 3 in five steps, with each step drawing a deformation of 20%;

[0050] Step 5: The stainless steel wire in step 4 is subjected to intermediate annealing at a temperature of 900°C, pickled after annealing, and then cold drawn again with a deformation of 60%;

[0051] Step 6: Perform medium-temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium-temperature microstructure control heat treatment is performed at 650° C.

[0052] Step 7: Perform a deformation strengthening on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 60%;

[0053] Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 400° C.;

[0054] Step 9, performing secondary deformation strengthening on the stainless steel wire in step 8, wherein the deformation amount of the secondary deformation strengthening is 90%;

[0055] Step 10, pickling the stainless steel wire in step 9 to obtain high-strength antibacterial stainless steel wire;

[0056] Step 11: The high-strength antibacterial stainless steel wire in step 10 is subjected to vacuum vertical heat straightening at a heating temperature of 700° C. After straightening, the stainless steel wire is tightly wound and finely processed into a high-strength ureteral metal stent with antibacterial and anti-crusting functions according to final needs.

[0057] Example 2

[0058] In this embodiment, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 3%, N: 0.15%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe. The preparation method is as follows:

[0059] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0060] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0061] Step 3, hot rolling the stainless steel bar in step 2 into wire rod, with the hot rolling temperature being 1150° C.;

[0062] Step 4: cold-draw the stainless steel wire rod in step 3 in five steps, with each step drawing a deformation of 20%;

[0063] Step 5: The stainless steel wire in step 4 is subjected to intermediate annealing at a temperature of 850°C, pickled after annealing, and then cold drawn again with a deformation of 50%;

[0064] Step 6: Perform medium temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium temperature microstructure control heat treatment is 600° C.;

[0065] Step 7: Perform a deformation strengthening on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 40%;

[0066] Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 300° C.;

[0067] Step 9: Perform secondary deformation strengthening on the stainless steel wire in step 8, and the deformation amount of the secondary deformation strengthening is 80%;

[0068] Step 10, pickling the stainless steel wire in step 9 to obtain high-strength antibacterial stainless steel wire;

[0069] Step 11: The high-strength antibacterial stainless steel wire in step 10 is subjected to vacuum vertical heat straightening at a heating temperature of 700° C. After straightening, the stainless steel wire is tightly wound and finely processed into a high-strength ureteral metal stent with antibacterial and anti-crusting functions according to final needs.

[0070] Example 3

[0071] In this embodiment, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 5%, N: 0.15%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe. The preparation method is as follows:

[0072] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0073] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0074] Step 3, hot rolling the stainless steel bar in step 2 into wire rod, with the hot rolling temperature being 1150° C.;

[0075] Step 4: cold-draw the stainless steel wire rod in step 3 in five steps, with each step drawing a deformation of 20%;

[0076] Step 5: The stainless steel wire in step 4 is subjected to intermediate annealing at a temperature of 1050°C, pickled after annealing, and then cold drawn again with a deformation of 70%;

[0077] Step 6: Perform medium temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium temperature microstructure control heat treatment is 700° C.;

[0078] Step 7: Perform a deformation strengthening on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 70%;

[0079] Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 500° C.;

[0080] Step 9: Perform secondary deformation strengthening on the stainless steel wire in step 8, and the deformation amount of the secondary deformation strengthening is 95%;

[0081] Step 10, pickling the stainless steel wire in step 9 to obtain high-strength antibacterial stainless steel wire;

[0082] Step 11: The high-strength antibacterial stainless steel wire in step 10 is subjected to vacuum vertical heat straightening at a heating temperature of 700° C. After straightening, the stainless steel wire is tightly wound and finely processed into a high-strength ureteral metal stent with antibacterial and anti-crusting functions according to final needs.

[0083] Comparative Example 1

[0084] In this comparative example, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe, that is, no copper and nitrogen elements are added. The preparation method is as follows:

[0085] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0086] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0087] Step 3, hot rolling the stainless steel in step 2 into wire rods at a hot rolling temperature of 1150° C.

[0088] Step 4: cold-draw the stainless steel wire rod in step 3 in five steps, with each step drawing a deformation of 20%;

[0089] Step 5: The stainless steel wire in step 4 is subjected to intermediate annealing at a temperature of 900°C, pickled after annealing, and then cold drawn again with a deformation of 60%;

[0090] Step 6: Perform medium-temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium-temperature microstructure control heat treatment is performed at 650° C.

[0091] Step 7: Perform a deformation strengthening on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 60%;

[0092] Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 400° C.;

[0093] Step 9, performing secondary deformation strengthening on the stainless steel wire in step 8, wherein the deformation amount of the secondary deformation strengthening is 90%;

[0094] Step 10, pickling the stainless steel wire in step 9 to obtain stainless steel wire;

[0095] Step 11: vacuum vertical heat straightening is performed on the stainless steel wire in step 10 at a heating temperature of 700° C. After straightening, the stainless steel wire is densely wound and finely processed into a ureteral metal stent according to final needs. Comparative Example 2

[0096] In this comparative example, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 4.5%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe, that is, no nitrogen element is added.

[0097] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0098] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0099] Step 3, hot rolling the stainless steel bar in step 2 into wire rod, with the hot rolling temperature being 1150° C.;

[0100] Step 4: cold-draw the stainless steel wire rod in step 3 in five steps, with each step drawing a deformation of 20%;

[0101] Step 5: The stainless steel wire in step 4 is subjected to intermediate annealing at a temperature of 900°C, pickled after annealing, and then cold drawn again with a deformation of 60%;

[0102] Step 6: Perform medium-temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium-temperature microstructure control heat treatment is performed at 650° C.

[0103] Step 7: Perform a deformation strengthening on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 60%;

[0104] Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 400° C.;

[0105] Step 9, performing secondary deformation strengthening on the stainless steel wire in step 8, wherein the deformation amount of the secondary deformation strengthening is 90%;

[0106] Step 10, pickling the stainless steel wire in step 9 to obtain stainless steel wire;

[0107] Step 11: vacuum vertical heat straightening is performed on the stainless steel wire in step 10 at a heating temperature of 700° C. After straightening, the stainless steel wire is densely wound and finely processed into a ureteral metal stent according to final needs. Comparative Example 3

[0108] In this comparative example, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 4.5%, N: 0.15%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe. The preparation method is as follows:

[0109] Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition;

[0110] Step 2: Forging the stainless steel ingot in step 1 into a rod at a forging temperature of 1200° C.

[0111] Step 3, hot rolling the stainless steel bar in step 2 into wire rod, with the hot rolling temperature being 1150° C.;

[0112] Step 4: Performing conventional process treatment (annealing temperature 1000° C., pickling after annealing, and then cold drawing) on ​​the stainless steel wire rod in step 3 to obtain stainless steel wire;

[0113] Step 5: After straightening at 700°C, the stainless steel wire is densely wound and finely processed into a ureteral metal stent according to final needs. Comparative Example 4

[0114] In this comparative example, the chemical composition is as follows (wt.%): Mo: 2.5%, Ni: 13%, Cr: 17%, Cu: 4.5%, N: 0.15%, C: 0.01%, Si: 0.5%, Mn: 1.0%, S: 0.006%, P: 0.005%, and the balance is Fe. The preparation method is the same as Example 1 except that the process parameters are different from those in Example 1 (see Table 1 for details).

[0115] The key information of the above embodiments and comparative examples is summarized in Table 1 for easy comprehensive comparison.

[0116] Table 1 Main chemical components (wt.%) and preparation process differences between the examples and comparative examples

[0117]

[0118] Performance Testing

[0119] According to the national standard GB / T 228.1, the room temperature tensile mechanical properties of the materials in the examples and comparative examples were tested using an Instron 8872 tensile testing machine at a tensile rate of 0.5 mm / min. Three parallel samples were taken from each group of samples to measure the tensile strength of the corresponding materials.

[0120] According to the national standard GB / T 16886.5 biological evaluation method for medical devices, the cell survival rate was determined by MTT colorimetry to evaluate the biological safety of the materials in the examples and comparative examples. The results of each group were evaluated according to the 5-level cytotoxicity evaluation standard (level 0 and 1 meet the requirements of biomedical materials).

[0121] The pitting potential of the alloy was tested by electrochemical corrosion experiment. The corrosion resistance of the materials in the examples and comparative examples was tested, and the anodic polarization curve was obtained according to the method in the national standard GB / T 17899 to measure the corrosion resistance.

[0122] The performance test results of the materials in the embodiments and comparative examples are summarized in Table 2.

[0123] Table 2 Performance test results of the examples and comparative examples

[0124]

[0125] In vitro bacterial co-culture assay

[0126] Inoculate Staphylococcus aureus and urease-positive bacterial strains on a slant of nutrient agar medium in a 1:1 ratio, culture at 37±1°C for 24 hours, and then store at 0-5°C (not more than 1 month) as slant-preserved bacteria.

[0127] Transfer the slant-preserved bacteria to a plate of nutrient agar medium and culture at 37±1℃ for 24 hours, once a day for no more than 2 weeks. The test should use fresh bacterial cultures after two consecutive transfers (transferred within 24 hours).

[0128] Use an inoculation loop to take a small amount (scrape 1-2 loops) of fresh bacteria from the culture medium, add it to the culture medium, and make 10-fold incremental dilutions in sequence. Count the cells using a cell counting plate and select a bacterial solution concentration of 5.0-10.0×10 5 The dilution with cfu / ml was used as the bacterial solution for experimental detection.

[0129] Prepare 15 φ90mm sterile dishes, place 5-6 φ90mm sterile filter papers on the bottom of the dishes, and pour in an appropriate amount of sterile purified water to allow the filter paper to fully absorb water. It is best if no large amount of water precipitates when pressing the filter paper with sterile tweezers.

[0130] Take 15 sterile filter membranes with a size of φ0.24μm×50mm, cover them on the sterile filter paper of each plate, and spread them flat. Take 0.2ml of the experimental bacterial solution and drop it on the sterile filter membrane with a size of φ0.24μm×50mm.

[0131] Use sterile tweezers to pick up the negative control TC titanium alloy sample (A), the blank control medical high-density polyethylene sample (B), and the test sample (C). Prepare 5 parallel samples for each sample, cover them on a φ0.24μm×50mm sterile filter membrane to allow the bacterial solution to evenly contact the sample, and culture them at 37±1℃ for 24h.

[0132] Take out the samples that have been cultured for 24 hours, add 20 ml of eluent respectively, wash sample A, sample B, sample C and the covering film repeatedly, and shake well. Use a sterile pipette tip to absorb 1 ml of the original eluent solution and transfer it to a sterile culture dish. Inject about 15 ml of nutrient agar medium into the culture dish and rotate the culture dish to mix evenly. Repeat the plate-laying operation twice to obtain 2 culture dishes with the original elution solution. Take another 1 ml of the original eluent solution and slowly inject it into a test tube containing 9 ml of sterile saline along the wall of the tube. The tip of the pipette tip does not touch the diluent in the tube. Shake the test tube to mix evenly to make a 1:10 elution dilution solution.

[0133] Take 1 ml of 1:10 elution diluent and transfer it to a sterile culture dish. Inject about 15 ml of nutrient agar medium into the culture dish and rotate the culture dish to mix evenly. Repeat the plate-laying operation twice to obtain two 1:10 elution diluent culture dishes. Take 1 ml of 1:10 elution diluent and slowly inject it into a test tube containing 9 ml of sterile physiological saline along the tube wall. The tip of the gun does not touch the diluent in the tube. Shake the test tube to mix evenly to make a 1:100 elution diluent.

[0134] Take 1 ml of 1:100 elution diluent and transfer it to a sterile culture dish. Inject about 15 ml of nutrient agar medium into the culture dish and rotate the culture dish to mix evenly. Repeat the plate-laying operation twice to obtain two 1:100 elution diluent culture dishes. Take 1 ml of 1:100 elution diluent and slowly inject it into a test tube containing 9 ml of sterile physiological saline along the tube wall. The tip of the gun does not touch the diluent in the tube. Shake the test tube to mix evenly to make a 1:1000 elution diluent.

[0135] Take 1 ml of 1:1000 elution dilution and transfer it to a sterile culture dish. Pour about 15 ml of nutrient agar medium into the culture dish and rotate the culture dish to mix evenly. Repeat the plating operation twice to obtain 2 1:1000 elution dilution culture dishes.

[0136] When counting the colonies on the plates, you can observe with your naked eyes, and use a magnifying glass if necessary to prevent omissions. After recording the number of colonies on each plate, calculate the average total number of colonies on each plate with the same dilution. Select plates with a colony count between 30 and 300 as the standard for determining the total number of colonies.

[0137] If two plates are used for one dilution, the average of the two plates should be used. If one of the plates has large flake colonies growing, it should not be used. Instead, the plate without flake colonies should be used as the colony count for that dilution. If the flake colonies are less than half of the plate, and the colonies in the remaining half are evenly distributed, half of the plate can be counted and multiplied by 2 to represent the colony count of the whole plate. If there are chain colonies growing in the plate, if there is only one chain, it can be regarded as one colony; if there are several chains from different sources, each chain should be counted as a colony. A dilution with an average colony count between 30 and 300 should be selected and reported by multiplying it by the dilution multiple. If there are two dilutions, and the number of colonies grown is between 30 and 300, the decision will be made based on the ratio between the two. If the ratio is less than or equal to 2, the average should be reported; if it is greater than 2, the smaller number should be reported. If the average colony count of all dilutions is greater than 300, the average colony count of the highest dilution multiplied by the dilution multiple should be reported. If the average colony count of all dilutions is less than 30, the average colony count of the lowest dilution multiplied by the dilution factor should be reported. If no colonies grow at all dilutions, report as less than 1 multiplied by the lowest dilution factor. If the average colony count of all dilutions is not between 30 and 300, and some of them are greater than 300 or less than 30, report as the average colony count closest to 30 or 300 multiplied by the dilution factor.

[0138] When the colony count is less than 100, it is reported as the actual number. When it is greater than 100, two significant figures are used, and the value after the two significant figures is rounded off. In order to shorten the number of zeros after the number, it can also be expressed as an exponent of 10.

[0139] The measured viable bacterial count result is multiplied by 100 to obtain the actual recovered viable bacterial counts of sample A, sample B, and sample C after culturing for 24 hours, which are A, B, and C respectively.

[0140] Ensure that the experimental results meet the following requirements, otherwise the test is invalid:

[0141] The five parallel viable bacteria values ​​of the same blank control sample B must meet the requirement of (highest logarithm value - lowest logarithm value) / average viable bacteria value logarithm value not greater than 0.3;

[0142] The actual recovered viable bacteria value A of sample A should not be less than 1.0×10 5 cfu / piece, and the actual recovered viable bacteria value B of sample B should not be less than 1.0×10 4 cfu / piece.

[0143] The antibacterial rate is calculated according to the following formula:

[0144] R (%) = (BC) / B × 100

[0145] Where:

[0146] R——antibacterial rate, %;

[0147] B——Average number of recovered bacteria in blank control samples, cfu / piece;

[0148] C——Average number of recovered bacteria in antibacterial samples, cfu / tablet.

[0149] The antibacterial rate experimental results of the embodiments and comparative examples are summarized in Table 3.

[0150] Table 3 Antibacterial rate of examples and comparative examples

[0151]

[0152] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high-strength ureteral metal stent with antibacterial and anti-crusting functions, made of medical high-strength antibacterial stainless steel wire, characterized in that: The chemical composition of the ureteral metal stent includes, by weight percentage: Mo: 2~3%, Ni: 12~14%, Cr: 16~18%, Cu: 3~5%, N: 0.10~0.20%, C≤0.03%, Si≤1.00%, Mn≤1.50%, S≤0.01%, P≤0.01%, and the balance is Fe; The ureteral metal stent is made by a method comprising the following steps: Step 1: Use a vacuum induction furnace to melt stainless steel ingots according to the set chemical composition; Step 2, forging the stainless steel ingot in step 1 into a rod; Step 3, hot rolling the stainless steel bar in step 2 into wire rod; Step 4, cold drawing the stainless steel wire rod in step 3 to gradually draw it into stainless steel wire; Step 5: perform intermediate annealing and pickling on the cold-drawn stainless steel wire in step 4, and then perform cold drawing again, the intermediate annealing temperature is 850-1050°C, pickling is performed after annealing, and then the deformation amount of cold drawing is 50-70%; Step 6: Performing medium-temperature microstructure control heat treatment on the stainless steel wire in step 5, wherein the medium-temperature microstructure control heat treatment temperature is 600-700°C; Step 7: Perform a deformation strengthening treatment on the stainless steel wire after the organization adjustment in step 6, and the deformation amount of the deformation strengthening is 40-70%; Step 8: performing low temperature structure control heat treatment on the stainless steel wire in step 7, wherein the low temperature structure control heat treatment temperature is 300-500° C.; Step 9: Perform secondary deformation strengthening treatment on the stainless steel wire in step 8, and the deformation amount of the secondary deformation strengthening is 80-95%; Step 10, pickling the stainless steel wire in step 9 to obtain high-strength antibacterial stainless steel wire; Step 11, performing vacuum vertical heat straightening on the stainless steel wire in step 10; According to the needs, the heat-straightened stainless steel wire is densely wound and finely processed into a high-strength ureteral metal stent with antibacterial and anti-crusting functions.

2. The high-strength ureteral metal stent with antibacterial and anti-crusting functions according to claim 1, characterized in that: Step 2: Forging temperature is 1150~1250℃; Step three, the hot rolling temperature is 1100~1200℃.

3. The high-strength ureteral metal stent with antibacterial and anti-crusting functions according to claim 1, characterized in that: Step 4: cold drawing is carried out in five steps, and the deformation amount of each cold drawing is 20-25%.

4. The high-strength ureteral metal stent with antibacterial and anti-crusting functions according to claim 1, characterized in that: Step 10, the diameter of the obtained high-strength stainless steel wire is 0.05~1mm; Step eleven, the heating temperature is 640~770℃.

5. The high-strength ureteral metal stent with antibacterial and anti-crusting functions according to claim 1, characterized in that: Step 11, the obtained ureteral metal stent has a tensile strength of 2300-2800 MPa, a cytotoxicity rating of ≤1, and a pitting potential of ≥500 mV; The obtained ureteral metal stent has a relative antibacterial rate of more than 90% in co-culture with Staphylococcus aureus and urease-positive bacteria.