A special crack-resistant agent for steel pipe encased in concrete, its preparation method and its application

By adsorbing an aqueous solution of polyvinyl alcohol and carbon nanotubes into the pores of diatomaceous earth and then coating and sealing it, an anti-cracking agent was formed, which solved the problem of easy cracking of concrete encasing steel pipes, improved tensile strength and toughness, and reduced production costs.

CN118405866BActive Publication Date: 2026-11-17GUANGXI ROAD & BRIDGE ENG GRP CO LTD +3
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410235113.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-01
Publication Date
2026-11-17
Estimated Expiration
2044-03-01

AI Technical Summary

Technical Problem

The concrete encasing the steel pipe is prone to cracking. Existing expansion agents have limited hydration reactions in high-strength concrete. Direct addition of diatomaceous earth affects the workability of concrete and makes it difficult to effectively improve tensile strength and toughness.

Method used

A crack-resistant coating agent is formed by using calcium-magnesium composite expansion components, diatomaceous earth with aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and sealing materials. Through physical adsorption and chemical reaction, moisture is stored in the pores of diatomaceous earth, releasing carbon nanotubes and polyvinyl alcohol, thereby regulating humidity and improving tensile strength.

Benefits of technology

It significantly increases the tensile strength and toughness of concrete, improves internal humidity control, reduces the risk of cracking, and does not affect the workability of concrete, thus reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004722382100000111
    Figure BDA0004722382100000111
  • Figure BDA0004722382100000112
    Figure BDA0004722382100000112
  • Figure BDA0004722382100000121
    Figure BDA0004722382100000121
Patent Text Reader

Abstract

This application relates to the field of building materials technology, specifically disclosing a special crack-resistant agent for steel pipe-clad concrete, its preparation method, and its application. The crack-resistant agent of this application is made from raw materials including a calcium-magnesium composite expansion component, diatomaceous earth with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and a sealing material. The diatomaceous earth particles with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed within their pores are coated with a film formed by the sealing material; the calcium-magnesium composite expansion component particles are also coated with a film formed by the sealing material; the mass ratio of the calcium-magnesium composite expansion component, the diatomaceous earth with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and the sealing material is (20-55):(40-70):(5-10). This crack-resistant agent achieves a synergistic effect of toughening and shrinkage compensation, thereby improving the crack resistance of concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of building materials technology, specifically to a special anti-cracking agent for steel pipe-encased concrete, its preparation method, and its application. Background Technology

[0002] In recent years, the construction of high-speed transportation networks in my country and around the world has accelerated, with highways and high-speed railways extending into mountainous areas. The mountainous regions of China, which account for more than two-thirds of the country's area, have an extremely urgent need for long-span arch bridges. The valleys and terrain of these mountains are characterized by high mountains, steep slopes, and favorable geological conditions, making them suitable for constructing arch bridges that are harmonious with the environment but often generate enormous horizontal thrust at the arch abutments. Compared to other bridge types, steel-concrete composite arch bridges have advantages such as lightweight materials, high strength, large load-bearing capacity, and convenient construction and installation, and are therefore widely used.

[0003] The key challenge in reinforced steel-concrete composite arch bridges lies in the crack resistance of the outer concrete casing. This structure, resembling a "sandwich," consists of a steel tube filled with concrete, encased in another layer of concrete. This type of structure offers advantages such as high load-bearing capacity, good seismic performance, and material savings, making it widely used in mountainous bridges. However, mountain bridge construction often faces harsh environments including dryness, large diurnal temperature variations, and monsoons, placing high demands on the volume stability and durability of the concrete. Due to the thinness of the steel tube encased in concrete, the coupling of shrinkage deformation (such as thermal shrinkage, autogenous shrinkage, and drying shrinkage) and hygrothermal deformation creates a high driving force for internal microcracks, making it prone to cracking. Furthermore, the internal and external constraints can easily generate tensile stress on the steel tube wall and surface, further increasing the risk of cracking. In addition, bridges in mountain valleys are generally located in environments with strong monsoons, dry air, and uneven sunlight. During the later stages of service, the steel tube encased in concrete is highly susceptible to microcracks due to long-term drying shrinkage. Once the outer concrete cracks, rainwater and harmful ions from nature will seep into the concrete along the cracks, causing the internal steel bars and pipes to corrode, reducing the structure's load-bearing capacity, durability, and service life. Deep cracks may even damage the integrity of the arch bridge, change the stress mechanism of the steel-concrete composite bridge, and even cause concrete to fall off, affecting structural safety.

[0004] How to effectively reduce or even eliminate various shrinkages, improve the tensile strength and toughness of concrete, and prevent cracking of steel-pipe-encased concrete from the source has always been a problem that engineers have been striving to explore. Currently, the commonly used method is to add concrete expansion agents, polypropylene fibers, or steel fibers to compensate for shrinkage and increase concrete toughness. In ordinary C30 and C40 concrete systems, expansion agents can effectively compensate for shrinkage. However, the strength of steel-pipe-encased concrete is generally above C50, with a low water-cement ratio. The hydration of expansion agents requires a reaction with water; if the water content in the concrete is low, the expansion performance of the expansion material will be affected. As mountain bridges continue to extend into mountainous areas, and structural forms become increasingly tall and long-span, higher demands are placed on the pumping performance of concrete. Especially for high-altitude pumped concrete, both high cohesiveness and high fluidity are required; otherwise, engineering problems such as pipe blockage or even pipe bursting are likely to occur. Polypropylene fibers, due to their low elastic modulus, can only inhibit cracking in the plastic stage of concrete, and have little effect on shrinkage cracking in the hardening stage, and can easily affect the mixing performance of concrete. Steel fibers can improve the tensile strength and toughness of concrete, but their high density makes them difficult to disperse, which can easily lead to difficulties in pumping concrete.

[0005] Furthermore, high-strength concrete has a dense structure, and techniques such as covering with a film and watering can only cure the surface layer, failing to address the insufficient internal water supply during the hydration process. The most suitable approach is to use internal curing materials as a carrier to provide water from within the concrete for self-curing. Internal curing agents are materials that absorb moisture through chemical or physical processes and possess certain water storage and retention functions. Because their mechanism of action lies in water storage and retention, they differ from other common concrete additives, such as water-reducing agents and concrete expansion agents. Existing internal curing agents mainly fall into two categories: porous inorganic materials and polymer-based superabsorbent polymers. Among these, the most common porous inorganic materials are artificial lightweight aggregates (LWA), such as ceramsite, natural zeolite, fly ash, bentonite, and rice husk ash. Inorganic porous materials can significantly improve the relative humidity inside high-strength concrete and alleviate early shrinkage deformation. However, if inorganic materials do not pre-absorb water, it will affect the workability of the concrete; if they do pre-absorb water, it will increase the risk of bleeding, and the concrete strength and modulus of elasticity will decrease with increasing lightweight aggregate content. Superabsorbent polymer (SAP) relies on hydrophilic groups on the polymer chain to adsorb water. However, SAP particles are difficult to disperse and tend to clump together. After releasing water, they leave large voids, which affect the workability, mechanical properties, volume deformation, and durability of concrete.

[0006] Diatomaceous earth is a porous biogenic siliceous rock. It is formed from the deposition of minerals from the cell walls of dead diatoms in water, followed by diagenesis. The main component of diatomaceous earth is amorphous silica, with a mass fraction as high as 90%. Compared to synthetic silica, diatomaceous earth exhibits superior thermal stability and chemical properties, possessing advantages such as a high melting point, high acid resistance, and high toughness. Its microstructure reveals a large number of orderly arranged micropores on its surface, exhibiting high regularity and precise reproducibility in its three-dimensional structures (such as pores, ridges, or tubular structures) at the nanometer to micrometer scale. The unique natural macroporous / mesoporous pore structure of diatomaceous earth gives it a strong adsorption capacity. The abundant active SiO2 in diatomaceous earth reacts with OH- in highly alkaline solutions in concrete. - The activation of diatomaceous earth triggers a volcanic ash reaction, forming a large amount of hydrated silicate gel, which improves the later-stage strength of concrete and reduces porosity. On the other hand, diatomaceous earth has a porous structure and, after fine grinding, has a large specific surface area, capable of adsorbing large amounts of moisture and gas, thus regulating the internal humidity of concrete and reducing its drying shrinkage. Chinese patent CN109704632B discloses a concrete anti-seepage and crack-resistant agent and its preparation method, composed of expansive soil, calcium magnesium ore powder, polyurethane fiber, diatomaceous earth, and organic copolymers. However, diatomaceous earth is a porous material, and without any modification, it will affect the workability of the concrete. Chinese patent CN108863149A discloses a method for preparing a high-strength concrete expansive agent material, using a starch-fatty acid composite to precipitate and coat diatomaceous earth particles under acidic conditions, forming starch-fatty acid modified diatomaceous earth aggregates. However, this preparation process is complex, and the purpose and effect of fatty acid coating on modified diatomaceous earth cannot be clearly understood.

[0007] Therefore, the main technical problems with the above-mentioned technology are as follows: 1. Due to the thin thickness of the steel pipe encased in concrete, the coupling of shrinkage deformation and hygrothermal deformation leads to a large driving force for internal microcracks, making it prone to cracking; 2. The hydration of expansive materials requires a reaction with water, and the low water content in high-strength concrete (the strength grade of steel pipe encased concrete is generally above C50) affects the expansion performance of the expansive materials; 3. Directly adding diatomaceous earth to adjust the internal humidity of the concrete will affect the workability of the concrete. How to increase the tensile strength and toughness of concrete, compensate for its shrinkage, and reduce tensile stress from a material perspective is a problem that urgently needs to be solved for steel pipe encased concrete. Summary of the Invention

[0008] This application provides a special crack-resistant agent for concrete encased in steel pipes, its preparation method, and its application. The crack-resistant agent of this application not only significantly improves the internal humidity of hardened concrete, controls concrete temperature rise, and significantly compensates for shrinkage, but also significantly increases the tensile strength of concrete, achieving a toughening effect.

[0009] In the first aspect, this application provides a special crack-resistant agent for steel pipes encased in concrete, employing the following technical solution:

[0010] A special anti-cracking agent for steel pipe concrete coating is made from raw materials including calcium-magnesium composite expansion component, diatomaceous earth with aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and sealing material; the diatomaceous earth particles with aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores are coated with a coating film formed by the sealing material; the calcium-magnesium composite expansion component particles are coated with a coating film formed by the sealing material; the mass ratio of the calcium-magnesium composite expansion component, the diatomaceous earth with aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and the sealing material is (20-55):(40-70):(5-10).

[0011] By adopting the above technical solution, this application achieves the basic water retention function of diatomaceous earth by adsorbing an aqueous solution of polyvinyl alcohol (PVA) and carbon nanotubes into the pores of the diatomaceous earth. This not only mitigates the impact of directly adding diatomaceous earth on concrete workability, but also addresses the issue of directly adding carbon nanotubes affecting concrete performance. Furthermore, the combined use of PVA and carbon nanotubes, due to the large number of alcohol groups in PVA, allows for hydrogen bonding with various organic and inorganic substances, resulting in good compatibility. The presence of PVA liquid also facilitates the dispersion of carbon nanotubes. The use of a sealing material, combined with the porosity of diatomaceous earth, effectively stores carbon nanotubes, PVA, and water within the pores, resulting in diatomaceous earth with an aqueous solution containing PVA and carbon nanotubes adsorbed within the pores and a film coating on the surface. The aforementioned crack-resistant agent, when added to concrete, not only does not affect the concrete's workability; but also, under conditions of temperature rise and alkalinity in the concrete, the coating film can be damaged, allowing for the effective release of carbon nanotubes, polyvinyl alcohol, and water. Specifically, the pores within the diatomaceous earth release moisture, regulating the internal humidity of the concrete; the diatomaceous earth also simultaneously releases carbon nanotubes and polyvinyl alcohol, and with the release of water, the carbon nanotubes are randomly distributed within the polyvinyl alcohol film, effectively improving the tensile strength and toughness of the concrete without affecting its workability. A large amount of active SiO2 in the diatomaceous earth reacts with OH- in the highly alkaline concrete solution. - Under the stimulation of [the environment], a volcanic ash reaction occurs, forming a large amount of hydrated silicate (CSH) gel, which improves the later-stage strength of concrete and reduces porosity. Therefore, guided by the technical approach of this application, and in combination with the above components, the resulting crack-resistant agent not only significantly improves the internal humidity of hardened concrete, controls concrete temperature rise, and significantly compensates for shrinkage, but also significantly increases the tensile strength of concrete, achieving a toughening effect.

[0012] Further, in the diatomaceous earth raw material in which an aqueous solution containing polyvinyl alcohol and carbon nanotubes is adsorbed within the pores, the mass ratio of the aqueous solution containing polyvinyl alcohol and carbon nanotubes to the diatomaceous earth is (40-70):(30-60). Further, in the aqueous solution containing polyvinyl alcohol and carbon nanotubes, the mass ratio of polyvinyl alcohol, carbon nanotubes, and water is (30-40):(5-10):(55-60).

[0013] Furthermore, the specific surface area of ​​the diatomaceous earth is 50–65 m². 2 / g, SiO2 content ≥90wt%, density 2.1~2.6g / cm³ 3 The water absorption rate is 200%–400% of its self-generated volume, and the residue on an 80μm square-hole sieve is ≤5.0%. The polyvinyl alcohol has an average degree of polymerization of 500–2500 and a degree of alcoholysis of 78–98 mol%. The carbon nanotubes have a diameter of 5–10 nm, an aspect ratio of 0.5–5 μm, and a specific surface area of ​​200–500 m² / g. 2 / g.

[0014] By adopting the above technical solution, the aqueous solution containing polyvinyl alcohol and carbon nanotubes can be more stably and effectively adsorbed into the pore structure of diatomaceous earth, and then released stably and effectively.

[0015] Further, the sealing material comprises a mixture of dextrin and paraffin in a mass ratio of (30-50):(50-70), wherein the number average molecular weight of the dextrin is 10,000–20,000 g / mol, and the phase transition temperature of the paraffin is 45–60°C. The specific surface area of ​​the concrete-specific crack-resistant agent for steel pipe encapsulation is 150–300 m² / g. 2 / kg.

[0016] By adopting the above technical solutions, dextrin is easily soluble in water, while paraffin is not. Using a composite film of paraffin and dextrin can improve film quality and more effectively protect the polyvinyl alcohol, carbon nanotubes, and water within the pores of diatomaceous earth from leakage. Furthermore, under the conditions of rising concrete temperature and alkalinity, paraffin can dissolve and dextrin can decompose, allowing the polyvinyl alcohol, carbon nanotubes, and water within the diatomaceous earth pores to be effectively released as the internal humidity of the concrete decreases. Further, in this application, paraffin can also be used as a temperature-sensitive material, and dextrin as a hydration heat regulating component; the combination of the two can better control the cement hydration rate and reduce temperature rise.

[0017] Secondly, this application provides a method for preparing a special crack-resistant agent for concrete encasing steel pipes, employing the following technical solution:

[0018] A method for preparing a special crack-resistant agent for steel pipe encased in concrete includes the following steps:

[0019] Polyvinyl alcohol, carbon nanotubes and water are stirred and mixed at 65-75℃ to obtain an aqueous solution containing polyvinyl alcohol and carbon nanotubes.

[0020] Diatomaceous earth was added to an aqueous solution containing polyvinyl alcohol and carbon nanotubes and mixed and reacted to obtain diatomaceous earth powder with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores.

[0021] The sealing material is atomized into droplets, and then adsorbed onto the surface of calcium-magnesium composite expansion components and diatomaceous earth particles containing aqueous solutions of polyvinyl alcohol and carbon nanotubes through physical adsorption and chemical reaction to form a film, thus obtaining an anti-crack agent.

[0022] Furthermore, a method for preparing a special crack-resistant agent for concrete encasing steel pipes includes the following steps:

[0023] (1) Preparation of high-temperature calcined diatomaceous earth powder by suspension kiln calcination: The ground diatomaceous earth is fed into the kiln through the feed inlet by a belt conveyor. Under the action of high-temperature airflow of 500℃~600℃, the material is in a suspended boiling state in the kiln, and the calcination time is controlled at 60~120s. The calcined diatomaceous earth powder is collected by a multi-stage cyclone separator.

[0024] (2) Polyvinyl alcohol and carbon nanotubes are slowly added to a reaction vessel containing water. The mass ratio of polyvinyl alcohol, carbon nanotubes, and water in the aqueous solution is (30-40):(5-10):(55-60). The solution temperature in the reaction vessel is controlled at 65-75℃, and the stirring speed of the impeller in the reaction vessel is 400-500 r / min. An ultrasonic device is installed in the reaction vessel, and the ultrasonic frequency is controlled at 40000-50000 Hz.

[0025] (3) After stirring the above-mentioned aqueous solution of polyvinyl alcohol and carbon nanotubes for 10-30 minutes, the calcined diatomaceous earth powder can be added to the reaction vessel. The mass ratio of the aqueous solution containing polyvinyl alcohol and carbon nanotubes to the diatomaceous earth powder is controlled to be (40-70):(30-60) to obtain diatomaceous earth powder with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores.

[0026] (4) The calcium-magnesium composite expansion component and the diatomaceous earth powder containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores are added to their respective powder feeders in the fluidized bed. The particles are transported into the fluidized bed by compressed air at a pressure of 0.3–0.8 MPa, and the particles are uniformly dispersed in the hot air flow within the fluidized bed. The equipment is sealed to form a closed space within the fluidized bed, allowing the above components to fully boil. Dextrin and paraffin are melted into a liquid phase at 75–85°C. The spray device in the fluidized bed is turned on. The liquid phase is atomized into micro-liquid droplets with a diameter of 10–50 μm. The micro-liquid droplets, fully boiling in the fluidized bed, use the calcium-magnesium composite expansion component and the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores as carriers. Dextrin and paraffin are adsorbed onto the surface of the calcium-magnesium composite expansion component and the diatomaceous earth particles through physical adsorption and chemical reaction to form a film.

[0027] (5) The calcium-magnesium composite expansion component that forms a film on the surface of diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes is rapidly separated from the pores that are rapidly film-forming in the airflow, thus obtaining a special anti-cracking agent for steel pipe concrete.

[0028] Furthermore, the reaction temperature of the calcium-magnesium composite expansion component, the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and the sealing material, i.e. the internal temperature of the fluidized bed, is controlled at 45-70℃.

[0029] By employing the above technical solution, utilizing the porosity of calcined diatomaceous earth particles, an aqueous solution containing polyvinyl alcohol and carbon nanotubes is pre-adsorbed and stored within the pores of the diatomaceous earth particles through physical adsorption and chemical reaction. A fluidized bed preparation process is then used to coat the surface of the calcium-magnesium composite expansion component particles with dextrin and paraffin wax, forming a film on the surface of the diatomaceous earth particles containing the aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within their pores. This results in a special crack-resistant agent for concrete-clad steel pipes. The method is simple to operate, requires no special process equipment, significantly reduces production costs, and yields substantial socio-economic benefits.

[0030] Thirdly, this application provides an application of a special anti-cracking agent for steel pipes encased in concrete, employing the following technical solution:

[0031] An application of a special crack-resistant agent for steel-pipe encased concrete is disclosed. This agent is suitable for steel-pipe encased concrete structures with a pour temperature of 15℃ or higher and a strength grade of C50 or higher. The crack-resistant agent is incorporated into C50–C120 concrete at a dosage of 4%–10% of the total mass of the cementitious materials.

[0032] In summary, this application has the following beneficial effects:

[0033] (1) The steel pipe-wrapped concrete toughening, temperature and humidity control high-efficiency crack-resistant agent prepared in this application overcomes the adverse effects of internal curing materials on the workability of concrete; improves the whole-process shrinkage compensation effect of calcium-magnesium composite expansion component; releases moisture from the pores inside diatomite, regulating the internal humidity of concrete; polyvinyl alcohol and carbon nanotubes released from the pores inside diatomite increase the tensile strength of concrete and achieve toughening effect; the temperature-sensitive material absorbs heat by dissolving, and the hydration heat control material regulates the temperature rise rate of concrete, ultimately achieving the synergistic effect of toughening and shrinkage compensation, and improving the crack resistance of concrete.

[0034] (2) The steel pipe-wrapped concrete toughening, temperature and humidity control high-efficiency crack-resistant agent prepared in this application has carbon nanotubes and polyvinyl alcohol released from the diatomaceous earth pores. As moisture is released, the carbon nanotubes are randomly distributed in the polyvinyl alcohol film, which effectively improves the tensile strength of the concrete without affecting the workability of the concrete.

[0035] (3) The steel pipe-clad concrete-specific toughening, temperature and humidity controlled, high-efficiency crack-resistant agent prepared in this application reacts with a large amount of active SiO2 in diatomaceous earth in the highly alkaline concrete solution. - The activation of the volcanic ash reaction results in the formation of a large amount of hydrated silicate gel, which improves the later strength of concrete and reduces porosity.

[0036] (4) The preparation method of the special toughening, temperature and humidity control high-efficiency crack-resistant agent for steel pipe outer concrete provided in this application is simple to operate, requires no special process equipment, greatly reduces production costs, and has significant social and economic benefits. Attached Figure Description

[0037] Figure 1 The temperature drop deformation of concrete prepared in Examples 1-3 is as follows: concrete with steel pipe outer-coated concrete crack-resistant agent, concrete with calcined diatomaceous earth, and concrete with calcium-magnesium composite expansion component of the same composition. 1# is the standard C60 concrete, 2# is concrete with 4.0% calcined diatomaceous earth, 3# is concrete with 5.5% calcium-magnesium composite expansion component, and 4# is the steel pipe outer-coated concrete crack-resistant agent of Example 3.

[0038] Figure 2 The figures show the drying shrinkage deformation of concrete prepared in Examples 4-6, including concrete with steel pipe outer casing, concrete with calcined diatomaceous earth, and concrete with the same calcium-magnesium composite expansion component. 1# is the reference C50 concrete; 2# is the concrete with the special crack-resistant agent from Example 6 of Examples 4-6; 3# is concrete with 4.0% calcined diatomaceous earth; and 4# is concrete with 5.5% calcium-magnesium composite expansion component. Positive values ​​in the figure represent expansion deformation, and negative values ​​represent shrinkage deformation. Detailed Implementation

[0039] The following specific embodiments further illustrate the technical features of the special anti-cracking agent for steel pipe encased in concrete described in this application, its preparation method, and its application, but are not limited to the embodiments.

[0040] This application provides a special anti-cracking agent for steel pipe-coated concrete, which is made from raw materials including a calcium-magnesium composite expansion component, diatomaceous earth with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and a sealing material. The diatomaceous earth is coated with a film formed by the sealing material, which de-seals under conditions of concrete temperature rise and alkalinity. Similarly, the calcium-magnesium composite expansion component particles are coated with a film formed by the sealing material, which de-seals under conditions of concrete temperature rise and alkalinity.

[0041] Further, the mass ratio of the calcium-magnesium composite expansion component, the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and the sealing material is (20-55):(40-70):(5-10). In the raw material of diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within its pores, the mass ratio of the aqueous solution of polyvinyl alcohol and carbon nanotubes to diatomaceous earth is (40-70):(30-60). In the aqueous solution containing polyvinyl alcohol and carbon nanotubes, the mass ratio of polyvinyl alcohol, carbon nanotubes, and water is (30-40):(5-10):(55-60). The sealing material comprises a mixture of dextrin and paraffin in a mass ratio of (30-50):(50-70).

[0042] Furthermore, the calcium-magnesium composite expansive component is a concrete expansive agent composed of lightly calcined magnesia expansive material and calcium oxide, or lightly calcined magnesia expansive material and calcium sulfoaluminate-calcium oxide expansive material, in a certain proportion. The lightly calcined magnesite material is prepared by grinding and lightly calcining magnesite powder, with an activity reaction time in the range of 100s to 250s. The calcium-magnesium composite expansive component meets the requirements of Type II in standard T / CECS10082-2020 "Calcium-Magnesium Composite Expansive Agent for Concrete".

[0043] Diatomaceous earth is obtained by high-temperature calcination, and the specific surface area of ​​the calcined diatomaceous earth is 50-65 m². 2 / g, SiO2 content ≥90wt%, density 2.1~2.6g / cm³ 3 The water absorption rate is 200% to 400% of its own volume, and the residue on an 80μm square hole sieve is ≤5.0%.

[0044] The average degree of polymerization of polyvinyl alcohol is 500–2500, and the degree of alcoholysis is 78–98 mol%.

[0045] Carbon nanotubes have a diameter of 5–10 nm, an aspect ratio of 0.5–5 μm, a tensile strength of 150–200 GPa, and a specific surface area of ​​200–500 m². 2 / g.

[0046] Pure water is preferred to meet the requirements of JGJ 63-2006 "Standard for Water Used in Concrete".

[0047] The number-average molecular weight of dextrin is between 10,000 and 20,000 g / mol, and the phase transition temperature of paraffin is between 45 and 60 °C.

[0048] This application also provides a method for preparing a special crack-resistant agent for concrete encasing steel pipes, comprising the following steps:

[0049] (1) Preparation of high-temperature calcined diatomaceous earth powder by suspension kiln calcination: The ground diatomaceous earth is fed into the kiln through the feed inlet by a belt conveyor. Under the action of high-temperature airflow of 500℃~600℃, the material is in a suspended boiling state in the kiln, and the calcination time is controlled at 60~120s. The calcined diatomaceous earth powder is collected by a multi-stage cyclone separator.

[0050] (2) Polyvinyl alcohol and carbon nanotubes are slowly added to a reaction vessel containing water. The mass ratio of polyvinyl alcohol, carbon nanotubes, and water in the aqueous solution is (30-40):(5-10):(55-60). The solution temperature in the reaction vessel is controlled at 65-75℃, and the stirring speed of the impeller in the reaction vessel is 400-500 r / min. An ultrasonic device is installed in the reaction vessel, and the ultrasonic frequency is controlled at 40000-50000 Hz.

[0051] (3) After stirring the above-mentioned aqueous solution of polyvinyl alcohol and carbon nanotubes for 10-30 minutes, the calcined diatomaceous earth powder can be added to the reaction vessel. The mass ratio of the aqueous solution containing polyvinyl alcohol and carbon nanotubes to the diatomaceous earth powder is controlled to be (40-70):(30-60) to obtain diatomaceous earth powder with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores.

[0052] (4) The calcium-magnesium composite expansion component and the diatomaceous earth powder containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores are added to their respective powder feeders in the fluidized bed. The particles are transported into the fluidized bed by compressed air at a pressure of 0.3–0.8 MPa, and the particles are uniformly dispersed in the hot air flow within the fluidized bed. The equipment is sealed to form a closed space within the fluidized bed, allowing the above components to fully boil. Dextrin and paraffin are melted into a liquid phase at 75–85°C. The spray device in the fluidized bed is turned on. The liquid phase is atomized into micro-liquid droplets with a diameter of 10–50 μm. The micro-liquid droplets, fully boiling in the fluidized bed, use the calcium-magnesium composite expansion component and the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores as carriers. Dextrin and paraffin are adsorbed onto the surface of the calcium-magnesium composite expansion component and the diatomaceous earth particles through physical adsorption and chemical reaction to form a film.

[0053] (5) The calcium-magnesium composite expansion component that forms a film on the surface of diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes is rapidly separated from the pores that are rapidly film-forming in the airflow, thus obtaining a special anti-cracking agent for steel pipe concrete.

[0054] Furthermore, the reaction temperature of the calcium-magnesium composite expansion component, the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and the sealing material is 45-70℃, that is, the internal temperature of the fluidized bed is controlled at 45-70℃, preferably 60-70℃.

[0055] This application also provides an application of a special anti-cracking agent for steel pipe-encased concrete. The anti-cracking agent is suitable for steel pipe-encased concrete structures with a pouring temperature of 15°C or higher and a strength grade of C50 or higher. Furthermore, the amount of the above-mentioned anti-cracking agent added to C50 to C120 concrete accounts for 4% to 10% of the total mass of cementitious materials.

[0056] The following is an illustration through specific examples.

[0057] Examples 1-3

[0058] (I) Preparation of a special crack-resistant agent for steel pipe encased in concrete

[0059] Examples 1-3 provide a special anti-cracking agent for steel pipes encased in concrete, made from raw materials including a calcium-magnesium composite expansion component, diatomaceous earth with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and a sealing material. The diatomaceous earth is coated with a film formed by the sealing material, which de-seals under conditions of concrete temperature rise and alkalinity. The calcium-magnesium composite expansion component particles are also coated with a film formed by the sealing material, which de-seals under conditions of concrete temperature rise and alkalinity. Specific raw materials are as follows:

[0060] The calcium-magnesium composite expansion component was prepared by Jiangsu Subote New Material Co., Ltd. (the MgO content in the expansion component is 30%, and the balance is calcium oxide, calcium sulfoaluminate, and anhydrite-like substances), meeting the requirements of Type II in standard T / CECS 10082-2020 "Calcium-Magnesium Composite Expansion Agent for Concrete". The diatomaceous earth was prepared by Qingdao Shengtai Silicon Industry Co., Ltd., with a SiO2 content of 90wt%.

[0061] Polyvinyl alcohol is commercially available, with an average degree of polymerization of 500 and a degree of alcoholysis of 88 mol%. Carbon nanotubes are commercially available, with a diameter of 10 nm, a major diameter of 5 μm, a tensile strength of 150 GPa, and a specific surface area of ​​200 m². 2 / g. Dextrin was prepared by Jiangsu Subote New Material Co., Ltd., with a number-average molecular weight of 10,000 g / mol. Paraffin was commercially available, with a phase transition temperature of 45-55℃.

[0062] The mass ratio of the calcium-magnesium composite expansion component, the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within its pores, and the sealing material is (20-55):(40-70):(5-10). In the raw material of diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within its pores, the mass ratio of the aqueous solution of polyvinyl alcohol and carbon nanotubes to diatomaceous earth is 40:60. In the aqueous solution containing polyvinyl alcohol and carbon nanotubes, the mass ratio of polyvinyl alcohol, carbon nanotubes, and water is 40:5:55. The sealing material comprises a mixture of dextrin and paraffin in a mass ratio of 30:70.

[0063] A method for preparing a special crack-resistant agent for steel pipe encased in concrete includes the following steps:

[0064] (1) High-temperature calcined diatomaceous earth powder was prepared by calcination in a suspension kiln. The ground diatomaceous earth was fed into the kiln via a belt conveyor through the feed inlet. Under the action of a 500℃ high-temperature airflow, the material was in a suspended boiling state within the kiln, and the calcination time was controlled at 60 seconds. The calcined diatomaceous earth powder was collected by a multi-stage cyclone separator. The specific surface area of ​​the calcined diatomaceous earth was 50 m². 2 / g, SiO2 content 90.0%, density 2.1g / cm³ 3 The water absorption rate is 260% of its own volume, and the residue on an 80μm square hole sieve is 4.3%.

[0065] (2) Polyvinyl alcohol and carbon nanotubes were slowly added to a reaction vessel containing water. The solution temperature inside the reaction vessel was controlled at 65°C, and the stirring speed of the stirrer inside the reaction vessel was 400 r / min. An ultrasonic device was installed inside the reaction vessel, and the ultrasonic frequency was controlled at 40000 Hz.

[0066] (3) After stirring the aqueous solution of polyvinyl alcohol and carbon nanotubes for 10 minutes, the calcined diatomaceous earth powder was added to the reactor. The solution temperature in the reactor was controlled at 65℃, and the stirring speed of the stirring paddle in the reactor was 400 r / min. The ultrasonic device installed in the reactor was controlled at an ultrasonic frequency of 40000 Hz. The calcined diatomaceous earth was stirred together with the aqueous solution of polyvinyl alcohol and carbon nanotubes for 10 minutes to obtain diatomaceous earth powder with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores.

[0067] (4) The calcium-magnesium composite expansion component and the diatomaceous earth powder containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores are respectively added to their respective powder feeders in the fluidized bed. The particles are transported into the fluidized bed by compressed air at a pressure of 0.3 MPa, and the particles are uniformly dispersed in the hot air flow within the fluidized bed. The equipment is sealed to form a closed space within the fluidized bed, allowing the above components to fully boil. Dextrin and paraffin are melted into a liquid phase at 75°C. The spray device in the fluidized bed is turned on. The liquid phase is atomized into micro-liquid droplets with a diameter of 10 μm. The micro-liquid droplets, fully boiling in the fluidized bed, use the calcium-magnesium composite expansion component and the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed within the pores as carriers. Dextrin and paraffin are adsorbed onto the surface of the calcium-magnesium composite expansion component and the diatomaceous earth particles through physical adsorption and chemical reaction to form a film. The internal temperature of the fluidized bed is controlled at 60°C.

[0068] (5) The calcium-magnesium composite expansion component that forms a film on the surface of the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes is rapidly separated from the pores that are rapidly film-forming in the airflow, thus obtaining the special anti-cracking agent for concrete wrapped around the steel pipe.

[0069] The differences between Examples 1-3 are: the amount of calcium-magnesium composite expansion component, diatomaceous earth powder containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and the amount of sealing material are different, as detailed in Table 1.

[0070] Table 1. Raw material component dosage in Examples 1-3

[0071]

[0072] (II) Workability Test of Special Crack-Resistant Agent for Steel Pipe Encased in Concrete

[0073] The effect of a special anti-cracking agent for steel pipe-encased concrete on the flowability of cementitious paste was evaluated using a paste test. The test method for the flowability of the cementitious paste followed the relevant provisions of GB 80770-2000 "Test Methods for Homogeneity of Concrete Admixtures"; the water-cement ratio of the cementitious paste was 0.35. The water-reducing agent was PCA polycarboxylate water-reducing agent prepared by Jiangsu Subote New Material Co., Ltd. The cement used was PI 42.5 standard cement. The calcium-magnesium composite expansion component was the same as that in Examples 1-3, and the calcined diatomaceous earth was the same as that in Examples 1-3. The test results are shown in Table 2. Samples 4, 8, and 12 were simple mixtures of the components listed in the table.

[0074] Table 2. Test results on the effect of Examples 1-3 on the flow properties of cementitious paste.

[0075]

[0076]

[0077] Comparison of the test results of samples 5, 9, and 13 with those of sample 1, and comparison of the test results of the remaining samples with those of sample 1, reveals that the use of simple calcium-magnesium composite expansion components, calcined but uncoated diatomaceous earth, single-component polyvinyl alcohol, single-component carbon nanotubes, and simple mixtures of materials in the same proportions as in the examples all have a certain impact on the fluidity of cement paste. The high-efficiency crack-resistant agent prepared in this application can effectively improve the initial fluidity of cement paste and significantly enhance its fluidity retention ability after 60 minutes. This indicates that this application successfully adsorbs an aqueous solution containing polyvinyl alcohol and carbon nanotubes into the pore structure of diatomaceous earth, and this operation can effectively improve the impact of directly adding diatomaceous earth on the workability of cementitious materials.

[0078] (III) Strength testing of concrete with steel pipe-wrapped special crack-resistant agent

[0079] Table 3 shows the reference mix proportions for C60 and C80 concrete used in a certain project. In the relevant samples, the mineral powder in the reference components was replaced by the corresponding components, such as: crack-resistant agent to replace mineral powder, calcium-magnesium composite expansion component to replace mineral powder, calcined diatomaceous earth to replace mineral powder, polyvinyl alcohol to replace mineral powder, and carbon nanotubes to replace mineral powder.

[0080] The cement used is Conch P·Ⅱ52.5 cement; the fly ash comes from Huaneng Power Plant in Nanjing, Jiangsu; the mineral powder comes from Nanjing Meibao Company; the sand is medium sand from the Ganjiang River; the gravel is produced by the Hexian Quarry in Ma'anshan, Anhui; and the water-reducing agent used is Jiangsu Subote polycarboxylate water-reducing agent (without retarder component).

[0081] Table 3. Mix Proportion Table for C60 and C80 Standard Concrete (Unit: (kg / m³)) 3 ))

[0082] Intensity level cement coal ash Mineral powder sand Xiaoshi Dashi water W / C C60 386 114 70 852 236 551 171 0.30 C80 402 104 103 746 412 618 141 0.23

[0083] According to the test method of standard GB / T 50081 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the splitting tensile strength of the above-mentioned concrete mix was tested.

[0084] Table 4 compares the splitting tensile strength of C60 concrete from Examples 1-3 with that from the selected calcium-magnesium composite expansion component and calcined diatomaceous earth. The dosage of the crack-resistant agent in the concrete was 10%. In Example 1, the calcium-magnesium composite expansion component content was 20%. Therefore, 2% calcium-magnesium composite expansion component was directly added to C60 concrete to verify the effect of direct addition on strength. Calcined diatomaceous earth was also directly added to C60 concrete to verify the effect of direct addition on concrete strength.

[0085] Table 4 compares the splitting tensile strength of C60 concrete made from Examples 1-3 with the selected calcium-magnesium composite expansion component and calcined diatomaceous earth.

[0086]

[0087] Table 4 shows that the crack-resistant agent prepared in this application has a significant effect on improving the splitting tensile strength of concrete.

[0088] Table 5 compares the splitting tensile strength of C60 concrete from Example 3 with that of the selected calcium-magnesium composite expansion component, calcined diatomaceous earth, and polyvinyl alcohol.

[0089]

[0090] Table 5 shows that the crack-resistant agent prepared in this application has a significant effect on improving the splitting tensile strength of concrete.

[0091] Table 6 compares the splitting tensile strength of C80 concrete made from Examples 1-3 and the selected calcium-magnesium composite expansion component and calcined diatomaceous earth.

[0092] Table 6

[0093]

[0094] Table 6 shows that the crack-resistant agent prepared in this application has a significant effect on improving the splitting tensile strength of concrete.

[0095] Table 7 compares the splitting tensile strength of the C80 concrete of the example with that of the selected calcium-magnesium composite expansion component, calcined diatomaceous earth, and polyvinyl alcohol.

[0096] Table 7

[0097]

[0098] Table 7 shows that the crack-resistant agent prepared in this application has a significant effect on improving the splitting tensile strength of concrete.

[0099] Tables 4, 5, 6, and 7 show that the steel pipe-encased concrete-specific crack-resistant agent of Examples 1-3 can significantly improve the splitting tensile strength of concrete. While the addition of polyvinyl alcohol or carbon nanotubes can improve the splitting tensile strength of concrete, the improvement is significantly lower than that of the crack-resistant agent prepared in this application.

[0100] (iv) Temperature control effect test of special crack-resistant agent for concrete wrapped with steel pipe

[0101] According to the test methods of the standards "Test Procedure for Hydraulic Concrete" DL / T 5150-2001 and "Test Method for Performance of Ordinary Concrete Mixtures" GB / T 50080-2016, the adiabatic temperature rise test was carried out on the above-mentioned concrete mix.

[0102] Table 8 compares the temperature control effects of Example 1 with those of the selected C60 concrete containing calcium-magnesium composite expansion component, calcined diatomaceous earth, paraffin wax, and hydration heat regulation component.

[0103]

[0104] Table 8 shows that the calcium-magnesium composite expansion component increased the temperature rise of concrete; calcined diatomaceous earth had lower activity than mineral powder, resulting in a slight decrease in the 7-day adiabatic temperature rise of the concrete; the hydration heat regulating component reduced the early temperature rise but did not reduce the 7-day temperature rise; paraffin could reduce the overall temperature rise of concrete, but its effect on regulating the temperature rise rate was not significant. The 1-day temperature rise in Example 1 accounted for 44.8% of the 7-day temperature rise. The crack-resistant agent in Example 1 not only significantly regulated the hydration rate of concrete but also reduced the overall temperature rise of the concrete.

[0105] Table 9 compares the temperature control effects of Example 3 with those of the selected C80 concrete containing calcium-magnesium composite expansion component, calcined diatomaceous earth, paraffin wax, and hydration heat regulation component.

[0106]

[0107] Table 9 shows that the calcium-magnesium composite expansion component increased the temperature rise of concrete; after calcination, diatomaceous earth had lower activity than mineral powder, and its 7-day adiabatic temperature rise of concrete was slightly reduced; the hydration heat regulating component reduced the early temperature rise, but did not reduce the 7-day temperature rise; paraffin could reduce the overall temperature rise of concrete, but its effect on regulating the temperature rise rate was not significant. Example 3's crack-resistant agent not only significantly regulated the hydration rate of concrete, but also reduced the overall temperature rise of concrete.

[0108] (V) Moisture test of concrete with special anti-cracking agent for steel pipe encasing concrete.

[0109] The internal humidity changes of concrete were tested using a commercially available embedded humidity sensor. The humidity of the prepared C60 concrete was tested, with 10% of the mineral powder replaced by a high-efficiency crack-resistant agent and 10% by a simple mixture. The molded concrete specimens were 150mm × 150mm × 150mm in size. The curing temperature in the curing room was 20±2℃, and the relative humidity was RH (65±5)%.

[0110] Table 10 shows the internal humidity of concrete after 3 days, 28 days, and 90 days (unit: RH / %).

[0111]

[0112] Table 10 shows that the high-efficiency crack-resistant agent prepared using the process described in this application can regulate the internal humidity of concrete, effectively reduce internal drying caused by cement hydration, and reduce the autogenous shrinkage and drying shrinkage of concrete.

[0113] (vi) Test on the expansion properties of concrete with special anti-cracking agent for steel pipe-encased concrete.

[0114] An environmental simulation chamber was used, with the temperature controlled at 25.0℃ for the first 6 hours after pouring, then increased to 67℃, with a temperature drop rate of approximately 3℃ / day. The aforementioned C60 concrete was poured using Ф110mm×400mm PVC pipes and placed in the environmental simulation chamber. Starting from initial setting, the actual temperature history of the aforementioned C60 concrete, including the baseline, 4.0% calcined diatomaceous earth, 5.5% calcium-magnesium composite expansion component, and 10% of the prepared crack-resistant agent from samples 1-3, was simulated. Strain gauges were used to monitor temperature and deformation. The concrete used was the baseline C60 mix proportion shown in Table 3 of Examples 1-3. Monitoring results during the temperature drop phase (see...) Figure 1 ).

[0115] Figure 1 Test results show that the above-prepared steel pipe outer concrete-specific toughening, temperature and humidity controlled high-efficiency crack-resistant agent improves the compensation effect of calcium-magnesium composite expansion component during the temperature drop stage.

[0116] Examples 4-6

[0117] (I) Preparation of a special crack-resistant agent for steel pipe encased in concrete

[0118] The calcium-magnesium composite expansive component was prepared by Tianjin Baoming Co., Ltd., and meets the requirements for Type II products in standard T / CECS 10082-2020 "Calcium-Magnesium Composite Expansive Agent for Concrete". Diatomaceous earth is a commercially available product. Polyvinyl alcohol is commercially available, with an average degree of polymerization of 2500 and a degree of alcoholysis of 98 mol%. Carbon nanotubes are commercially available, with a diameter of 5 nm, a major diameter of 5 μm, a tensile strength of 200 GPa, and a specific surface area of ​​500 m². 2 / g. The hydration heat regulating component was prepared by Jiangsu Subote New Material Co., Ltd., with a dextrin number-average molecular weight of 20,000 g / mol. Paraffin was commercially available, with a phase transition temperature of 45-60℃.

[0119] High-temperature calcined diatomaceous earth powder was prepared using a suspension kiln. The ground diatomaceous earth was conveyed into the kiln via a belt conveyor. Under the influence of a 600℃ high-temperature airflow, the material was in a suspended boiling state within the kiln, with the calcination time controlled at 120 seconds. The calcined diatomaceous earth powder was collected by a multi-stage cyclone separator. The specific surface area of ​​the calcined diatomaceous earth was 65 m² / s. 2 / g, SiO2 content 90.0%, density 2.6g / cm³ 3The water absorption rate is 350% of its own volume, and the residue on an 80μm square hole sieve is 2.3%.

[0120] Polyvinyl alcohol (PVA) and carbon nanotubes (CNTs) were slowly added to a reaction vessel containing water. The mass ratio of PVA, CNTs, and water in the aqueous solution was 30:10:60. The solution temperature inside the reaction vessel was controlled at 75°C, and the stirring speed of the impeller was 500 r / min. An ultrasonic device was installed inside the reaction vessel, with the ultrasonic frequency controlled at 50,000 Hz.

[0121] After stirring the aqueous solution of polyvinyl alcohol and carbon nanotubes for 30 minutes, the calcined diatomaceous earth powder was added to the reactor. The mass ratio of the aqueous solution containing polyvinyl alcohol and carbon nanotubes to the diatomaceous earth powder was controlled at 70:30 to obtain diatomaceous earth powder with pores containing polyvinyl alcohol and carbon nanotubes.

[0122] Calcium-magnesium composite expansion components and diatomaceous earth powder containing an aqueous solution of polyvinyl alcohol and carbon nanotubes within pores are separately added to their respective powder feeders in a fluidized bed. The particles are transported into the fluidized bed using compressed air at a pressure of 0.8 MPa, and the particles are uniformly dispersed in the hot air flow within the fluidized bed. The equipment is sealed to create a closed space within the fluidized bed, allowing the components to fully boil. A hydration heat regulating component and paraffin component are melted into a liquid phase at 85°C. The spray device in the fluidized bed is activated, atomizing the liquid phase into micro-droplets with a diameter of 50 μm. These fully boiling micro-droplets, using the calcium-magnesium composite expansion components and the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes within pores as carriers, are adsorbed onto the surfaces of the calcium-magnesium composite expansion components and diatomaceous earth particles through physical adsorption and chemical reaction, forming a film. The internal temperature of the fluidized bed is controlled at 70°C. The mass ratio of dextrin to paraffin in the composite material containing the hydration heat regulating component and the temperature-sensitive component is 50:50.

[0123] The diatomaceous earth containing polyvinyl alcohol and carbon nanotubes in an aqueous solution that forms a film rapidly in the airflow, and the calcium-magnesium composite expansion component that forms a film on the surface are rapidly separated to obtain the special anti-cracking agent for concrete wrapped around steel pipes.

[0124] Table 11 shows the proportions of the calcium-magnesium composite expansion component, the diatomaceous earth component containing polyvinyl alcohol and carbon nanotubes in the aqueous solution, and the surface-coated composite material containing hydration heat regulation component and temperature-sensitive component in the anti-cracking agent prepared above.

[0125]

[0126]

[0127] (II) Workability Test of Special Crack-Resistant Agent for Steel Pipe Encased in Concrete

[0128] The effect of a special anti-cracking agent for steel-pipe-encased concrete on the flowability of cementitious paste was evaluated using a neat paste test. The flowability test method for the cementitious paste was performed according to the relevant provisions of GB80770-2000 "Test Method for Homogeneity of Concrete Admixtures"; the water-cement ratio of the cementitious paste was 0.35 for all samples. The water-reducing agent was a powdered polycarboxylate water-reducing agent manufactured by Jiangsu Subote New Material Co., Ltd.

[0129] Table 12 compares the properties of crack-resistant agents, calcium-magnesium composite expansion components, diatomaceous earth, hydration heat regulating components, and paraffin materials.

[0130]

[0131]

[0132] The test results in Table 12 show that the special crack-resistant agent prepared in this application can effectively improve the initial fluidity of cement paste and significantly enhance its fluidity retention ability after 60 minutes. The use of simple calcium-magnesium composite expansion components, calcined but uncoated diatomaceous earth, and single-component polyvinyl alcohol all have a certain impact on the fluidity of cement paste.

[0133] (III) Strength testing of concrete with steel pipe-encased concrete-specific crack-resistant agent

[0134] Table 13 shows the standard mix proportions for C50 concrete used in a certain project, with high-efficiency crack-resistant agent replacing mineral powder, calcium-magnesium composite expansion component replacing mineral powder, calcined diatomaceous earth replacing mineral powder, and polyvinyl alcohol replacing mineral powder.

[0135] The cement used is Conch P·Ⅱ52.5 cement; the fly ash comes from Huaneng Power Plant in Nanjing, Jiangsu; the mineral powder comes from Nanjing Meibao Company; the sand is medium sand from the Ganjiang River; the gravel is produced by the Hexian Quarry in Ma'anshan, Anhui; and the water-reducing agent used is Jiangsu Subote water-reducing agent (without retarding component).

[0136] Table 13 shows the mix proportions of C50 standard concrete (kg / m³). 3 )

[0137] Intensity level cement coal ash Mineral powder sand Xiaoshi Dashi water W / C C50 260 90 100 750 310 740 145 0.33

[0138] According to the test method of standard GB / T 50081 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the splitting tensile strength and compressive strength of the above-mentioned concrete mix were tested.

[0139] Table 14 compares the splitting tensile strength of C50 concrete made from Examples 4-5 with the selected calcium-magnesium composite expansion component and calcined diatomaceous earth.

[0140]

[0141] Table 14 shows that the crack-resistant agent prepared by this method has a significant effect on improving the splitting tensile strength of concrete.

[0142] Table 15 compares the splitting tensile strength of C50 concrete from Example 6 with that of the selected calcium-magnesium composite expansion component, calcined diatomaceous earth, and polyvinyl alcohol.

[0143]

[0144]

[0145] Table 15 shows that the crack-resistant agent prepared by this method has a significant effect on improving the splitting tensile strength of concrete. Table 15 also shows that the crack-resistant agent sample 6, specifically designed for concrete with steel pipe encapsulation, significantly improves the splitting tensile strength of concrete, with the 7-day and 28-day splitting tensile strengths increasing by 28.0% and 22.9% respectively compared to the baseline. While adding polyvinyl alcohol alone can improve the splitting tensile strength of concrete, the increase is significantly lower than that of the crack-resistant agent prepared in this way.

[0146] Table 16 compares the compressive strength of the C50 concrete of the example with that of the selected calcium-magnesium composite expansion component, calcined diatomaceous earth, and polyvinyl alcohol.

[0147]

[0148] Table 16 shows that this special crack-resistant agent can improve the compressive strength of concrete in the later stages. The amorphous silica in calcined diatomaceous earth is active and can react with substances such as calcium hydroxide in concrete to form CSH gel, thereby enhancing the later strength of concrete.

[0149] (iv) Temperature control effect test of special crack-resistant agent for concrete wrapped with steel pipe

[0150] According to the test methods of the standards "Test Procedure for Hydraulic Concrete" DL / T 5150-2001 and "Test Method for Performance of Ordinary Concrete Mixtures" GB / T 50080-2016, the adiabatic temperature rise test was carried out on the above-mentioned concrete mix.

[0151] Table 17 compares the splitting tensile strength of C50 concrete from Example 4 with that of the selected single-component calcium-magnesium composite expansion component, single-component calcined diatomaceous earth, single-component paraffin, and single-component hydration heat regulating component.

[0152]

[0153] Table 17 shows that the calcium-magnesium composite expansion component increased the temperature rise of concrete; after calcination, diatomaceous earth had lower activity than mineral powder, and its 7-day adiabatic temperature rise of concrete was slightly reduced; the hydration heat regulating component reduced the early temperature rise, but did not reduce the 7-day temperature rise; paraffin could reduce the overall temperature rise of concrete, but its effect on regulating the temperature rise rate was not significant. Example 4's crack-resistant agent not only significantly regulated the hydration rate of concrete, but also reduced the overall temperature rise of concrete.

[0154] (V) Moisture test of concrete with special anti-cracking agent for steel pipe encasing concrete.

[0155] The internal humidity changes of concrete were tested using a commercially available embedded humidity sensor. The humidity of the prepared C50 concrete was tested, with 10% of the mineral powder replaced by a high-efficiency crack-resistant agent and 10% of the mineral powder replaced by a simple mixture. The dimensions of the molded concrete specimens were 150mm × 150mm × 150mm. The curing temperature in the curing room was 20±2℃, and the relative humidity was RH (65±5)%.

[0156] Table 18 shows the internal humidity of concrete after 3 days, 28 days, and 90 days (unit: RH / %).

[0157]

[0158] The test results in Table 18 show that the special crack-resistant agent prepared by the above process can regulate the internal humidity of concrete, effectively reduce internal drying caused by cement hydration, and reduce the autogenous shrinkage and drying shrinkage of concrete.

[0159] (vi) Testing the Deformation Performance of Concrete with Special Crack-Resistant Agent for Steel Pipe Encasing

[0160] According to the test method of standard T / CECS10082-2020 "Calcium-magnesium composite expansion agent for concrete", the mortar restricted expansion rate was tested on the above-prepared high-efficiency crack-resistant agent, the same calcium-magnesium composite expansion component, calcined diatomaceous earth and a simple mixed compound sample with the same proportion as the crack-resistant agent.

[0161] Table 19 shows the restricted expansion rate (in %) of the mortar samples from the examples and the selected calcined diatomaceous earth, calcium-magnesium composite expansion components, etc.

[0162]

[0163]

[0164] The test results in Table 19 show that the calcined diatomaceous earth does not have an expansion effect; the above process improves the expansion performance of the crack-resistant agent over 7 days, and when placed in dry air, it can effectively inhibit the drying shrinkage caused by moisture loss.

[0165] According to the test method of standard GB / T 50082-2009 "Test Method for Long-term Performance and Durability of Ordinary Concrete", the drying shrinkage performance of the above-mentioned concrete mix was tested.

[0166] The drying shrinkage deformation of the above-mentioned C50 concrete, including the reference, calcined diatomaceous earth, calcium-magnesium composite expansion component, and sample 6 anti-cracking agent (mixed with 10%), was measured. The concrete mix proportions were the reference C50 mix proportions shown in Table 13 of Examples 4-6. Concrete drying shrinkage test results (see...) Figure 2 ).

[0167] Figure 2 Test results show that the above-prepared anti-cracking agent for steel pipe-encased concrete effectively inhibits the drying shrinkage of C50 concrete.

Claims

1. A special crack-resistant agent for concrete encasing steel pipes, characterized in that: The crack-resistant agent is made of a calcium-magnesium composite expansion component, diatomaceous earth with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in its pores, and a sealing material; the diatomaceous earth particles with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in their pores are coated with a film formed by the sealing material; the calcium-magnesium composite expansion component particles are coated with a film formed by the sealing material; the mass ratio of the calcium-magnesium composite expansion component, the diatomaceous earth with an aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in its pores, and the sealing material is (20-55):(40-70):(5-10).

2. The special crack-resistant agent for steel pipe encased in concrete according to claim 1, characterized in that: In the raw material of diatomaceous earth in which an aqueous solution containing polyvinyl alcohol and carbon nanotubes is adsorbed in the pores, the mass ratio of the aqueous solution containing polyvinyl alcohol and carbon nanotubes to the diatomaceous earth is (40-70):(30-60).

3. The special crack-resistant agent for steel pipe encased in concrete according to claim 2, characterized in that: In the aqueous solution containing polyvinyl alcohol and carbon nanotubes, the mass ratio of polyvinyl alcohol, carbon nanotubes and water is (30-40):(5-10):(55-60).

4. The special crack-resistant agent for steel pipe encased in concrete according to claim 1, characterized in that: The sealing material comprises a mixture of dextrin and paraffin in a mass ratio of (30-50):(50-70), wherein the number average molecular weight of the dextrin is 10,000-20,000 g / mol and the phase transition temperature of the paraffin is 45-60°C.

5. The special crack-resistant agent for steel pipe encased in concrete according to claim 2, characterized in that: The diatomaceous earth has a specific surface area of ​​50~65m2 / g, a SiO2 content of ≥90wt%, a density of 2.1~2.6g / cm3, a water absorption rate of 200%~400% of its own volume, and a sieve residue of ≤5.0% on an 80μm square hole sieve.

6. The special crack-resistant agent for steel pipe encased in concrete according to claim 3, characterized in that: The polyvinyl alcohol has an average degree of polymerization of 500-2500 and a degree of alcoholysis of 78-98 mol.

7. The special crack-resistant agent for steel pipe encased in concrete according to claim 3, characterized in that: The carbon nanotubes have a diameter of 5-10 nm, an aspect ratio of 0.5-5, and a specific surface area of ​​200-500 m² / g.

8. A method for preparing a special crack-resistant agent for steel pipe encased in concrete as described in any one of claims 1-7, characterized in that, Includes the following steps: Polyvinyl alcohol, carbon nanotubes and water are stirred and mixed at 65-75℃ to obtain an aqueous solution containing polyvinyl alcohol and carbon nanotubes. Diatomaceous earth was added to an aqueous solution containing polyvinyl alcohol and carbon nanotubes and mixed to react, thus obtaining diatomaceous earth powder with the aqueous solution containing polyvinyl alcohol and carbon nanotubes adsorbed in the pores. The sealing material is atomized into droplets, and then adsorbed onto the surface of calcium-magnesium composite expansion components and diatomaceous earth particles containing aqueous solutions of polyvinyl alcohol and carbon nanotubes through physical adsorption and chemical reaction to form a film, thus obtaining an anti-crack agent.

9. The preparation method of a special crack-resistant agent for steel pipe encased in concrete according to claim 8, characterized in that, The calcium-magnesium composite expansion component, the diatomaceous earth containing an aqueous solution of polyvinyl alcohol and carbon nanotubes adsorbed in the pores, and the reaction temperature of the sealing material are 45-70℃.

10. The application of a special crack-resistant agent for steel pipe encased in concrete as described in any one of claims 1-7, characterized in that: The crack-resistant agent is suitable for steel pipe-encased concrete structures with a pouring temperature of 15°C or higher and a strength grade of C50 or higher.

Citation Information

Patent Citations

  • Preparation method of high-strength concrete expansive agent material

    CN108863149A

  • A concrete seepage-proof and crack-resistant agent and its preparation method

    CN109704632B

  • Magnesium, temperature-controlled and humidity-controlled efficient anti-cracking agent for cement concrete as well as preparation method and application of the magnesium, temperature-controlled and humidity-controlled efficient anti-cracking agent

    CN111377648A