Chemical mechanical polishing composition and its application in chemical mechanical polishing of tungsten

By using a specific composition in tungsten chemical mechanical polishing, combined with the first and second corrosion inhibitors and homopiperazine derivatives, the composition of the polishing composition is optimized, solving the problem of polishing defect control in the existing technology, and achieving high efficiency. polishing rate and low defect balance.

CN118406439BActive Publication Date: 2024-10-18WANHUA CHEM GRP ELECTRONIC MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410873230.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-18
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

Existing tungsten chemical mechanical polishing technology is difficult to significantly reduce EOE, dishing and erosion defects while maintaining the metal removal rate, and the corrosion inhibitor has limited control effect on polishing defects.

Method used

A chemical mechanical polishing composition is used, which includes a dispersion medium, an abrasive, a catalyst, an oxidant, a first corrosion inhibitor, a second corrosion inhibitor and an EOE improver. Paired with oxazine derivatives, the ingredients of the composition are optimized to achieve both polishing speed and defect control.

Benefits of technology

It is possible to achieve lower EOE, Disshing and Erosion defect levels in tungsten chemical mechanical polishing while maintaining a good polishing rate and reducing the contact resistance of metal interconnections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the technical field of chemical mechanical polishing, and provides a chemical mechanical polishing composition and its application in tungsten chemical mechanical polishing. The chemical mechanical polishing composition provided by the present invention can take into account both good polishing rate and low defect level. The composition includes a dispersion medium, an abrasive, a catalyst, an oxidant, a first corrosion inhibitor, a second corrosion inhibitor and an EOE improver, and optionally includes a stabilizer and a pH adjuster; wherein the first corrosion inhibitor is selected from one or more compounds in which the total number of amino and imino groups in the molecule is 1-4 and at least one carboxyl group is contained; the second corrosion inhibitor is selected from one or more compounds in which the total number of amino and imino groups in the molecule is 2 and at least one amide group is contained, and does not contain a carboxyl group, a hydroxyl group, an alkenyl group and an alkynyl group; the EOE improver is selected from one or more of homopiperazine and its derivatives.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical mechanical polishing, and further to a chemical mechanical polishing composition and application thereof, in particular to application in chemical mechanical polishing of tungsten. Background Art

[0002] Chemical mechanical polishing is the process of polishing a material surface by using chemical action, mechanical action, or a combination of the two actions generated by the friction between a polishing pad and a polishing liquid containing an abrasive. In this process, the surface of the polished material reacts with the chemical substances to form a soft layer, which is then removed by mechanical action, ultimately achieving the removal and flattening of excess material on the surface of the material. Chemical mechanical polishing (CMP) is the core technology that can achieve global flattening in the current integrated circuit manufacturing process. Tungsten is an important metal plug material in IC manufacturing, and chemical mechanical polishing is a key process in the manufacture of tungsten plugs. The chemical mechanical polishing composition involved is an important consumable in this process.

[0003] Chemical mechanical polishing compositions involving tungsten are generally composed of chemical components such as catalysts, oxidants, stabilizers, corrosion inhibitors, pH regulators dissolved in an aqueous system and colloidal abrasives suspended therein. Abrasives generally include three types: fumed silica, colloidal silica, and aluminum oxide. The polishing objects of the composition include metal W, barrier layers Ti, TiN, and dielectric layers TEOS, PSG, BPSG, SiN, SiON, etc. Polishing mainly focuses on metal removal rate, selectivity, and defects (including Dishing (dish-shaped defects), Erosion (erosion defects), EOE (edge ​​over-erosion defects), etc.).

[0004] Generally speaking, the components of the polishing composition directly affect the polishing effect, among which the corrosion inhibitor has a significant effect on polishing defects. Patent publications CN1272221A and CN116134110A mention that some amino acids can be used as corrosion inhibitors for polishing compositions involving tungsten; Patent publications CN108350318A and CN116333686A mention that adding some cationic substances (such as aliphatic ammonium salts) to polishing compositions involving tungsten can also be used as corrosion inhibitors.

[0005] Although these technologies have solved the polishing defect problem of tungsten plugs to a certain extent, as the feature size of IC manufacturing continues to shrink, the requirements for polishing effects, mainly polishing defects, are also increasing. For example, how to significantly reduce polishing defects while maintaining a certain degree of metal W removal rate to reduce the contact resistance of metal interconnections, etc., there is still much room for improvement. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a chemical mechanical polishing composition and application thereof. The chemical mechanical polishing composition of the present invention is used in tungsten chemical mechanical polishing, which can take into account lower EOE, Dishing and Erosion defect levels while having a good polishing rate.

[0007] To achieve the purpose, the present invention provides the following technical solutions:

[0008] The present invention provides a chemical mechanical polishing composition, which comprises a dispersion medium, an abrasive, a catalyst, an oxidant, a first corrosion inhibitor, a second corrosion inhibitor and an EOE improver, and optionally comprises a stabilizer and a pH adjuster;

[0009] wherein the first corrosion inhibitor is selected from one or more compounds having a total of 1 to 4 amino and imino groups in the molecule and at least one carboxyl group;

[0010] The second corrosion inhibitor is selected from one or more compounds having a total of 2 amino and imino groups in the molecule, at least one amide group, and no carboxyl group, hydroxyl group, alkenyl group, or alkynyl group;

[0011] The EOE improving agent is selected from one or more of homopiperazine and its derivatives;

[0012] Based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.01 wt%-2.0 wt%, and the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 1-299; the content of the EOE improver is 15 ppm-300 ppm.

[0013] In some embodiments, based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.1 wt%-1.0 wt%;

[0014] And / or, based on the total mass of the composition, the content of the EOE improver is 50 ppm-200 ppm.

[0015] In some embodiments, the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 49-199.

[0016] In some embodiments, the second corrosion inhibitor is selected from one or more of glycinamide, Boc-glycinamide, N-isopropylglycinamide, N-valeroylglycinamide, prolineamide, alaninamide, Boc-L-alaninamide, N-acetyl-L-alaninamide, L-phenylalaninamide, Boc-L-isoleucinamide, Boc-L-leucinamide, Boc-D-valinamide, and N-benzoyl-L-tyrosinamide.

[0017] In some embodiments, the first corrosion inhibitor is selected from the group consisting of tryptophan, 1-methyl-DL-tryptophan, 6-methyl-DL-tryptophan, 7-methyl-DL-tryptophan, N-formyl-DL-tryptophan, N-acetyl-DL-tryptophan, glycyl-DL-tryptophan, 5-hydroxytryptophan, lysine, N-acetyl-L-lysine, trifluoroacetyl-lysine, L-histidine, D-histidine, DL-histidine, Boc-histidine, N-acetyl-L-histidine, 1-methyl-L-histidine, arginine, homoarginine, N-Boc-L-arginine, N-ω-propyl-L-arginine, Nα-acetyl-L-arginine, leucine, isoleucine, glycyl-D-leucine, glycyl-DL-leucine, L-phenylalanine, D-phenylalanine, One or more of 2-methyl-L-phenylalanine, 4-methyl-L-phenylalanine, 4-methoxy-L-phenylalanine, N-acetyl-L-phenylalanine, glycyl-DL-phenylalanine, 4-amino-L-phenylalanine, tyrosine, 3-amino-L-tyrosine, glycyl-L-tyrosine, 3-hydroxy-L-tyrosine, N-acetyl-L-tyrosine, N-methyl-L-tyrosine, methyltyrosine, O-methyl-D-tyrosine, O-tert-butyl-L-tyrosine, glycine, BOC-glycine, N-phenylglycine, L-trifluoroacetylglycine, N-formylglycine, N-acetylglycine, cyclopentylglycine, glutamic acid, L-methionine, D-methionine, DL-methionine, threonine, cysteine, and N-acetyl-L-cysteine;

[0018] And / or, the EOE improver is selected from one or more of homopiperazine, 1-methyl homopiperazine, 1-ethyl homopiperazine, 1-Boc-homopiperazine, 1-formyl homopiperazine, 1-acetyl homopiperazine, 1,7-dimethyl-1,4-homopiperazine, 1-(2-methoxyethyl)homopiperazine, 1-benzyl homopiperazine, 1-(2-aminoethyl)-4-methylhomopiperazine, 1-isobutyl-1,4-homopiperazine, 1-pyrazin-2-yl-1,4-homopiperazine, 1-(4-methylbenzyl)homopiperazine, and 1-Boc-5-methyl-1,4-homopiperazine.

[0019] In some embodiments, the dispersion medium is deionized water;

[0020] And / or, the abrasive is fumed silica colloidal;

[0021] And / or, the catalyst is ferric nitrate nonahydrate;

[0022] And / or, the oxidant is hydrogen peroxide;

[0023] And / or, the stabilizer is one or more selected from acetic acid, citric acid, tartaric acid, oxalic acid, lactic acid, malic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, maleic acid, glycolic acid, diglycolic acid, glyceric acid, and succinic acid;

[0024] And / or, the pH adjuster is selected from one or more of an inorganic acid, an inorganic base and an organic base.

[0025] In some embodiments, the average particle size of the abrasive is 100nm-250nm;

[0026] And / or, the specific surface area of ​​the abrasive is 60m 2 / g -200m 2 / g;

[0027] And / or, the abrasive surface has a permanent positive charge.

[0028] In some embodiments, the content of the abrasive in the composition is 1.0 wt %-9.0 wt % based on the solid content of the abrasive;

[0029] and / or, the content of the catalyst in the composition is 0.01 wt%-0.5wt%;

[0030] and / or, the content of the oxidant in the composition is 2 wt%-10 wt%;

[0031] And / or, the content of the stabilizer in the composition is 0.05 wt%-1.2 wt%.

[0032] In some embodiments, the pH value of the composition is 2-4.

[0033] The present invention also provides use of the chemical mechanical polishing composition described above in chemical mechanical polishing of tungsten.

[0034] The technical solution provided by the present invention has the following beneficial effects:

[0035] The chemical mechanical polishing composition provided by the present invention uses a first corrosion inhibitor and a second corrosion inhibitor in combination, and the two are used in a specific mass ratio, and high piperazine and / or high piperazine derivatives in a specific content range are used in combination. The polishing composition is used in tungsten chemical mechanical polishing, which can take into account lower EOE, Dishing and Erosion defect levels, and has a good polishing rate. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The term "and / or" as may be used herein includes any and all combinations of one or more of the related listed items. The terms "first", "second", "third", etc. are used for descriptive purposes only and are not to be construed as indicating or implying relative importance.

[0038] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0039] The present invention provides a chemical mechanical polishing composition, which comprises a dispersion medium, an abrasive dispersed in the dispersion medium, a catalyst, an oxidant, a first corrosion inhibitor, a second corrosion inhibitor and an EOE improver, and optionally a stabilizer and a pH adjuster;

[0040] wherein the first corrosion inhibitor is selected from one or more compounds having a total of 1 to 4 amino and imino groups in the molecule and at least one carboxyl group;

[0041] The second corrosion inhibitor is selected from one or more compounds having a total of 2 amino and imino groups in the molecule, at least one amide group, and no carboxyl group, hydroxyl group, alkenyl group, or alkynyl group;

[0042] The EOE improving agent is selected from one or more of homopiperazine and its derivatives;

[0043] Based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.01 wt%-2.0 wt%, and the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 1-299; the content of the EOE improver is 15 ppm-300 ppm.

[0044] In the chemical mechanical polishing composition provided by the present invention, a first corrosion inhibitor and a second corrosion inhibitor are used in combination, and the two are used in a specific mass ratio. At the same time, high piperazine and / or high piperazine derivatives within a specific content range are used in combination. The polishing composition is used in tungsten chemical mechanical polishing, and can take into account the advantages of good polishing rate and low defects.

[0045] In a preferred embodiment, based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is preferably 0.1 wt%-1.0 wt%. By using the preferred amount, the application effect of the obtained polishing composition in tungsten chemical mechanical polishing can be further improved.

[0046] The inventors have found that in the formulation system of the present invention, on the basis of the combined use of the first and second corrosion inhibitors, the addition of the above-mentioned 15-300 ppm homopiperazine and / or homopiperazine derivatives as EOE improvers can effectively control the depth of EOE (Erosion edge depression) generated by polishing. In a preferred embodiment, based on the total mass of the composition, the content of the EOE improver is 50 ppm-200 ppm. The use of the preferred amount is conducive to further improving the application effect of the obtained polishing composition in tungsten chemical mechanical polishing.

[0047] The inventors have found that in the formulation system of the present invention, the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is controlled to be 1-299, and the two can play a good synergistic role and significantly reduce the defects caused by polishing, such as the depth of Dishing and Erosion. More preferably, the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 49-199; the use of the first and second corrosion inhibitors in combination with the preferred ratio is conducive to further improving the application effect of the obtained polishing composition in tungsten chemical mechanical polishing.

[0048] Conventional corrosion inhibitors, such as polyamino compounds and cationic polymers, have a strong adsorption effect on the tungsten surface during the chemical mechanical polishing of tungsten. Although a small amount can achieve a strong inhibition of the removal rate, it is often difficult to balance the polishing rate and defect control. In addition, such substances are also very easy to remain on the surface of the wafer and the polishing pad, resulting in difficulty in cleaning. The inventors have found that in a chemical mechanical polishing composition, a first corrosion inhibitor having a total of 1 to 4 amino and imino groups in the molecule and at least one carboxyl group is used in combination, and a second corrosion inhibitor having a total of 2 amino and imino groups in the molecule and at least one amide group and no carboxyl groups, hydroxyl groups, alkenyl groups and alkynyl groups is used, and homopiperazine and its derivatives are used in combination, so that a good balance between good polishing rate and low defects can be achieved.

[0049] In the present invention, the first corrosion inhibitor used is a substance in which the total number of amino groups and imino groups in the molecule is not less than 1 and not more than 4, and at least one carboxyl group is also present. In addition to amino groups / imino groups and carboxyl groups, the molecular structure of this type of substance may also contain other groups, for example, any one or more groups of alkyl groups, acyl groups, phenyl groups, hydroxyl groups, and halogen atoms. In the polishing composition, the amino groups and imino groups of this type of substance are protonated and positively charged, so this type of substance is easily adsorbed on the surface of the polished tungsten substrate through electrostatic action. Adding this type of substance to the composition has a significant inhibitory effect on the catalytic oxidation reaction during the polishing process, and can effectively inhibit the polishing rate. The total number of amino groups or imino groups in the selected molecules of this type of substance is not more than 4, which can prevent it from remaining on the surface of the wafer and the polishing pad. Although the first corrosion inhibitor has a significant adsorption effect on the tungsten surface, it has been found that under the condition of high-speed polishing, as the polishing temperature continues to increase during the polishing process, its adsorption effect gradually weakens, so its control of Dishing and Erosion at positions with larger line widths is not ideal.

[0050] In the present invention, the second corrosion inhibitor used is a substance having a total of 2 amino and imino groups in the molecule, at least one amide group and no carboxyl, hydroxyl, alkenyl and alkynyl groups. The molecular structure of this substance contains amino / imino groups and amide groups, but no carboxyl, hydroxyl, alkenyl and alkynyl groups. In the polishing composition, the amino and imino groups are also protonated and carry positive charges, so they can also be adsorbed on the surface of the polished tungsten substrate through electrostatic action. However, since the unshared electron pairs on the amino N in the molecule form a conjugated system with the π electrons of the carbonyl group, the electron cloud density on N is reduced, and the ability to accept protons is significantly weakened, so the adsorption effect of this type of substance on the surface of the tungsten substrate is relatively weak. During the polishing process, as the polishing temperature rises, the coverage ability of this type of substance at the position with a smaller line width is not enough, and it is easy to form larger Dishing and Erosion defects.

[0051] However, the inventors unexpectedly discovered during the research process that in the composition of the present invention, by compounding the first corrosion inhibitor and the second corrosion inhibitor of the present invention in a certain ratio, the depths of Dishing and Erosion at different line widths can be significantly reduced through synergistic effect while maintaining a suitable tungsten polishing rate.

[0052] In some embodiments, the second corrosion inhibitor is selected from one or more of glycineamide, Boc-glycineamide, N-isopropylglycineamide, N-valeroylglycineamide, prolineamide, alaninamide, Boc-L-alaninamide, N-acetyl-L-alaninamide, L-phenylalaninamide, Boc-L-isoleucinamide, Boc-L-leucinamide, Boc-D-valinamide, and N-benzoyl-L-tyrosinamide. Preferably, the second corrosion inhibitor is preferably one or more of glycineamide, prolineamide, alaninamide, and L-phenylalaninamide. The use of the preferred second corrosion inhibitor is conducive to further improving the application performance of the polishing composition in tungsten chemical mechanical polishing.

[0053] In some embodiments, the first corrosion inhibitor is selected from, for example, tryptophan, 1-methyl-DL-tryptophan, 6-methyl-DL-tryptophan, 7-methyl-DL-tryptophan, N-formyl-DL-tryptophan, N-acetyl-DL-tryptophan, glycyl-DL-tryptophan, 5-hydroxytryptophan, lysine, N-acetyl-L-lysine, trifluoroacetyl-lysine, L-histidine, D-histidine, DL-histidine, Boc-histidine, N-acetyl-L-histidine, 1-methyl-L-histidine, arginine, homoarginine, N-Boc-L-arginine, N-ω-propyl-L-arginine, Nα-acetyl-L-arginine, leucine, isoleucine, glycyl-D-leucine, glycyl-DL-leucine, L-phenylalanine, D-phenylalanine , 2-methyl-L-phenylalanine, 4-methyl-L-phenylalanine, 4-methoxy-L-phenylalanine, N-acetyl-L-phenylalanine, glycyl-DL-phenylalanine, 4-amino-L-phenylalanine, tyrosine, 3-amino-L-tyrosine, glycyl-L-tyrosine, 3-hydroxy-L-tyrosine, N-acetyl-L-tyrosine, N-methyl-L-tyrosine, methyltyrosine, O-methyl-D-tyrosine, O-tert-butyl-L-tyrosine, glycine, BOC-glycine, N-phenylglycine, L-trifluoroacetylglycine, N-formylglycine, N-acetylglycine, cyclopentylglycine, glutamic acid, L-methionine, D-methionine, DL-methionine, threonine, cysteine, N-acetyl-L-cysteine ​​or one or more thereof. Preferably, the first corrosion inhibitor is one or more of 5-hydroxytryptophan, Nα-acetyl-L-arginine, leucine, L-phenylalanine, methyltyrosine, and glycine. The use of the preferred first corrosion inhibitor is beneficial to further improve the application performance of the polishing composition in tungsten chemical mechanical polishing.

[0054] In the present invention, based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.01 wt%-2.0 wt%, such as 0.01 wt%, 0.05 wt%, 0.1 wt%, 0.2 wt%, 0.3 wt%, 0.4 wt%, 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, 1.0 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt%, 1.6 wt%, 1.7 wt%, 1.8 wt%, 1.9 wt%, 2.0 wt%, etc.; preferably 0.1 wt%-1.0wt%, such as 0.1 wt%, 0.15 wt%, 0.2 wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4 wt%, 0.45 wt%, 0.5 wt%, 0.55 wt%, 0.6 wt%, 0.65 wt%, 0.7 wt%, 0.75 wt%, 0.8 wt%, 0.85 wt%, 0.9wt%, 0.95 wt%, 1.0 wt%, etc.

[0055] In the present invention, the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 1-299, for example, 1, 5, 9, 49, 99, 149, 199, 249, 299, etc.; more preferably, it is 49-199, for example, 49, 59, 69, 79, 89, 99, 109, 119, 129, 139, 149, 159, 169, 179, 189, 199, etc.

[0056] Generally speaking, although the depth of EOE defects is lower than that of Erosion defects, they also have a significant impact on the contact resistance of tungsten plug metal interconnects. Therefore, it is necessary to further control EOE defects on the basis of controlling Dishing and Erosion defects. The inventors have found that in the formulation system of the present invention, homopiperazine and / or homopiperazine derivatives are used as EOE improvers, and are used in combination with the first and second corrosion inhibitors to effectively improve the EOE defects generated by polishing.

[0057] In some embodiments, the EOE improver is selected from, for example, homopiperazine, 1-methyl homopiperazine, 1-ethyl homopiperazine, 1-Boc-homopiperazine, 1-formyl homopiperazine, 1-acetyl homopiperazine, 1,7-dimethyl-1,4-homopiperazine, 1-(2-methoxyethyl) homopiperazine, 1-benzyl homopiperazine, 1-(2-aminoethyl)-4-methyl homopiperazine, 1-isobutyl-1,4-homopiperazine, 1-pyrazine-2-yl-1,4-homopiperazine, 1-(4-methylbenzyl) homopiperazine, and 1-Boc-5-methyl-1,4-homopiperazine. Preferably, the EOE improver is preferably one or more of homopiperazine and 1-methyl homopiperazine. The use of the preferred EOE improver is conducive to further improving the application performance of the polishing composition in tungsten chemical mechanical polishing.

[0058] In the present invention, based on the total mass of the composition, the content of the EOE improver is 15ppm-300ppm, for example, including but not limited to 15ppm, 30ppm, 50ppm, 70ppm, 90ppm, 110ppm, 130ppm, 150ppm, 170ppm, 190ppm, 210ppm, 230ppm, 250ppm, 270ppm, 300ppm, etc.; preferably 50ppm-200ppm, for example, including but not limited to 50ppm, 60ppm, 70ppm, 80ppm, 90ppm, 100ppm, 110ppm, 120ppm, 130ppm, 140ppm, 150ppm, 160ppm, 170ppm, 180ppm, 190ppm, 200ppm, etc.

[0059] In some embodiments, the dispersion medium is, for example, deionized water. In the composition, the sum of the mass fractions of other components and the dispersion medium is 100%. For example, the total mass fraction of the dispersion medium, the abrasive, the first corrosion inhibitor, the second corrosion inhibitor, the EOE improver, the catalyst, the oxidant, the optional stabilizer, and the optional pH adjuster is 100wt%.

[0060] In some embodiments, the abrasive is, for example, fumed silica colloid. In some embodiments, from the perspective of polishing rate and polished surface quality, the fumed silica colloid used in the composition, its average particle size is preferably 100nm-250nm, such as 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 145nm, 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, 180nm, 185nm, 190nm, 195nm, 200nm, 205nm, 210nm, 215nm, 220nm, 225nm, 230nm, 235nm, 240nm, 245nm, 250nm etc. The mass concentration of the abrasive is, for example, 25wt%. The specific surface area of ​​the abrasive is, for example, 60m 2 / g - 200m 2 / g. The fumed silica colloid used can be commercial electronic grade fumed silica purchased from the market; it can be ground and dispersed before use. For reference, the specific grinding method is as follows: the speed of the sand mill is 6000-8000rpm; the grinding beads are zirconium oxide, and the particle size of the grinding beads is 0.1-0.4mm; grinding for 30-60min.

[0061] In some embodiments, the surface of the abrasive preferably carries a permanent positive charge to improve the suspension stability of the abrasive. The abrasive with a permanent positive charge can be obtained by conventional methods well known in the art. For example, the fumed silica colloid used as the abrasive is modified with a silane coupling agent (such as an aminosilane compound), which is beneficial to improve the suspension stability of the abrasive in the composition and make the abrasive easy to disperse in the composition. For example, when modifying the abrasive, an aminosilane compound can be used, such as but not limited to N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-aminopropylmethyldiethoxysilane, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, etc. One or more. The above modification can be carried out by any suitable method for modifying fumed silica colloid. For example, the above abrasive can be modified by a modification method known to those skilled in the art. For reference, for example, documents such as "Preparation and characterization of silica sol with surface modification" and "Preparation of high PMMA grafted particle SiO2 using surface initiated free radical polymerization" all record the basic principles and general steps of modifying silica sol with aminosilane coupling agents. For example, the fumed silica sol can be treated with an aminosilane compound before mixing it with other components of the polishing composition. As a specific example, the modification includes the following steps: Step 1), adjust the pH value of deionized water to 6 with nitric acid, add silane coupling agent to deionized water, keep a constant temperature water bath at 60°C, and continue magnetic stirring for 30 minutes, then stand at room temperature for 4 hours to return to room temperature (25°C); Step 2), add a certain amount of fumed silica colloid to the solution of step 1), magnetically stir for 1 hour, and then stand at room temperature for 24 hours; Step 3): adjust the pH value of the fumed silica abrasive in step 2) to 2-4 (for example, pH=3.5) with nitric acid, and stand by. The mass amount of the above-mentioned silane coupling agent, for example, accounts for 5% of the solid content of the abrasive, and the mass concentration of the modified fumed silica colloid is, for example, 25wt%, and the surface has a permanent positive charge, and the Zeta potential is, for example, about 35mV. The fumed silica colloid as an abrasive has a permanent positive charge on its surface in the pH range of 2~4 after the above-mentioned modification.The above is only a specific example for reference. Those skilled in the art may also adopt other methods well known in the art to obtain abrasives with permanent positive charge. The abrasives may have the Zeta potential of abrasives with permanent positive charge conventionally used in the art, and there is no particular limitation on this.

[0062] In the present invention, the fumed silica colloid as an abrasive mainly plays a mechanical grinding role in the composition. Tungsten metal itself is a high-density, high-hardness material, and needs to undergo a catalytic oxidation reaction to form a metal oxide film (including WO2, WO3, W2O5, etc.) on its surface. The metal oxide film has a relatively lower hardness and is more loose, and is more easily removed layer by layer by mechanical action. After tungsten is catalytically oxidized to form a soft layer, the film layer is polished and removed under the mechanical action of the abrasive and the polishing pad. In the actual polishing process, in order to completely remove the deposited tungsten layer, it is necessary to perform over polishing after the endpoint detection (Endpoint). In this process, defects such as Dishing, Erosion, and EOE will inevitably occur, and these defects will cause a large contact resistance between the tungsten plug and the subsequently deposited interconnect metal; the inventors have found that by adding the first and second corrosion inhibitors and EOE improvers specified in the present invention, a good balance can be achieved between the polishing rate and the polishing surface quality.

[0063] In some embodiments, the specific surface area of ​​the fumed silica colloid used as the abrasive is 60 m 2 / g-200m 2 / g, for example 60m 2 / g, 65m 2 / g, 70m 2 / g, 75m 2 / g, 80m 2 / g, 85m 2 / g, 90m 2 / g, 95m 2 / g、100m 2 / g、105m 2 / g, 110m 2 / g, 115m 2 / g, 120m 2 / g, 125m 2 / g, 130m 2 / g, 135m 2 / g, 140m 2 / g, 145m 2 / g, 150m 2 / g, 155m 2 / g, 160m 2 / g, 165m 2 / g, 170m2 / g, 175m 2 / g, 180m 2 / g, 185m 2 / g, 190m 2 / g, 195m 2 / g, 200m 2 / g, etc.; it is beneficial to improve the polishing surface quality, such as reducing surface residue.

[0064] In some embodiments, the catalyst is, for example, ferric nitrate nonahydrate. The ferric nitrate nonahydrate can provide trivalent iron ions, Fe 3+ The decomposition of the oxidant is promoted by a Fenton-like reaction, thereby generating oxidizing radicals which react with the tungsten substrate to form an oxide layer.

[0065] In some embodiments, the oxidant is, for example, hydrogen peroxide. The hydrogen peroxide is used as an oxidant in the presence of a catalyst (e.g., Fe 3+ ) is decomposed into oxygen and other oxygen-containing free radicals under the catalytic action of tungsten. These decomposition products react with the surface of the tungsten substrate to form a loose oxide layer of tungsten (including WO3, WO2, W2O5 and other components), which is more easily removed by mechanical action.

[0066] In some embodiments, based on the solid content of the abrasive, the content of the abrasive in the composition is 1.0 wt%-9.0 wt%, such as 1.0 wt%, 2.0 wt%, 3.0 wt%, 4.0 wt%, 5.0 wt%, 6.0 wt%, 7.0 wt%, 8.0 wt%, 9.0 wt%, etc. Preferably, it is 3.5 wt%-7.0 wt%, such as 3.5 wt%, 4.0 wt%, 4.5 wt%, 5.0 wt%, 5.5 wt%, 6.0 wt%, 6.5 wt%, 7.0 wt%, etc.

[0067] In some embodiments, the content of the catalyst in the composition is 0.01 wt%-0.5wt%, for example, 0.01 wt%, 0.02 wt%, 0.05wt%, 0.1 wt%, 0.15wt%, 0.2wt%, 0.25 wt%, 0.3 wt%, 0.35 wt%, 0.4wt%, 0.45 wt%, 0.5wt%, etc.; preferably, 0.1 wt%-0.3wt%, for example, 0.1 wt%, 0.12wt%, 0.14wt%, 0.16 wt%, 0.18 wt%, 0.2wt%, 0.22 wt%, 0.24 wt%, 0.26 wt%, 0.28 wt%, 0.3 wt%, etc.

[0068] In some embodiments, the content of the oxidant in the composition is 2 wt%-10 wt%, for example 2.0 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, 5 wt%, 5.5 wt%, 6 wt%, 6.5 wt%, 7 wt%, 7.5 wt%, 8 wt%, 8.5 wt%, 9 wt%, 9.5 wt%, 10 wt%, etc.; preferably 4 wt%-8 wt%, for example 4 wt%, 4.2 wt%, 4.4 wt%, 4.6 wt%, 4.8 wt%, 5.0 wt%, 5.2 wt%, 5.4 wt%, 5.6 wt%, 5.8 wt%, 6.0 wt%, 6.2wt%, 6.4 wt%, 6.6 wt%, 6.8 wt%, 7.0 wt%, 7.2 wt%, 7.4 wt%, 7.6 wt%, 7.8 wt%, 8 wt%, etc.

[0069] In addition to the main components of abrasive, first corrosion inhibitor, second corrosion inhibitor, EOE improver, catalyst and oxidant, the present invention does not limit any other additives added to the polishing composition. Those skilled in the art can add other additives suitable for various conventional tungsten chemical mechanical polishing liquid systems as needed. For example, according to the requirements of improving the stability of the composition and improving the surface quality of tungsten, one or more stabilizers and pH adjusters can be arbitrarily selected to be added to the polishing composition.

[0070] In some embodiments, the stabilizer is an organic carboxylic acid, for example, selected from one or more of acetic acid, citric acid, tartaric acid, oxalic acid, lactic acid, malic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, maleic acid, glycolic acid, diglycolic acid, glyceric acid, succinic acid, preferably one or more of citric acid and malonic acid. In some embodiments, the content of the stabilizer in the composition is 0.05 wt%-1.2 wt%, preferably 0.4 wt%-0.8 wt%. The stabilizer is conducive to enhancing the placement stability of the composition. For the catalyst using iron ions, the above-mentioned stabilizer can react with the iron ions in the composition to form a colorless or light-colored complex, so that the iron ions remain stable, and the compression of the free iron ions on the abrasive double electric layer can also be reduced, thereby helping to improve the placement stability of the composition.

[0071] In some embodiments, the pH regulator is selected from one or more of inorganic acids, inorganic bases and organic bases, preferably selected from one or more of phosphoric acid, sulfuric acid, nitric acid, hydrochloric acid, potassium hydroxide, potassium carbonate, potassium bicarbonate, sodium hydroxide, ammonium hydroxide, tetramethylammonium hydroxide, preferably nitric acid and / or potassium hydroxide. The amount of the pH regulator is based on the pH of the composition being controlled at 2-4, preferably the pH of the composition being controlled at 2.3-3.

[0072] In some embodiments, the pH value of the composition is 2-4, such as 2, 2.2, 2.4, 2.6, 2.8, 3, 3.2, 3.4, 3.6, 3.8, 4, etc. In this pH range, it is beneficial to form a more stable passivation layer on the surface of the polished tungsten substrate through a catalytic oxidation reaction, which is beneficial to further improve the polishing rate and surface quality. Preferably, it is 2.3-3, such as 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, etc.

[0073] In some embodiments, based on the total mass of the composition, the following components are included in the following mass contents: 1.0 wt%-9.0 wt%, preferably 3.5 wt%-7.0 wt% of abrasive; 0.01 wt%-0.5 wt%, preferably 0.1 wt%-0.3 wt% of catalyst; 2 wt%-10 wt%, preferably 4 wt%-8 wt% of oxidant; 0.05 wt%-1.2 wt%, preferably 0.4 wt%-0.8 wt% of stabilizer; 0.01 wt%-2.0 wt%, preferably 0.1 wt%-1.0 wt% of the first corrosion inhibitor and the second corrosion inhibitor; 15 ppm-300 ppm, preferably 50 ppm-200 ppm of EOE improver; The pH regulator is used in an amount that makes the pH of the composition 2-4, preferably 2.3-3; the balance is a dispersion medium; wherein the mass amount of the second corrosion inhibitor is not less than the mass amount of the first corrosion inhibitor, and preferably the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 1-299, more preferably 49-199.

[0074] The polishing composition of the present invention can be prepared by a material mixing method known in the art, specifically, for example, including the step of mixing an abrasive (such as fumed silica colloid) with other additives. In some examples, the first corrosion inhibitor, the second corrosion inhibitor, the EOE improver, the catalyst, the oxidant, and the optional stabilizer, and deionized water are first fully mixed and dispersed to obtain a mixed material; then, the abrasive is added to the mixed material, and the pH value of the composition is adjusted to the desired pH with a pH adjuster as needed, and finally the polishing composition is formed after being fully stirred and dispersed. The dispersion means in this process include but are not limited to any one or more of mechanical stirring, ultrasonic dispersion, magnetic stirring, etc.

[0075] The polishing composition can be diluted in different multiples according to actual application requirements before use. For example, the dilution multiple calculated by mass ratio can be 1, 2, 3, 4, or 5 times, and the preferred dilution multiple is 3 times.

[0076] The present invention also provides use of the chemical mechanical polishing composition described above in chemical mechanical polishing of tungsten.

[0077] The present invention is further explained below by way of examples, but it should not be understood that the present invention is limited thereto.

[0078] In the following embodiments, the equipment and parameters for wafer polishing test are as follows:

[0079] Polishing machine: Ebara F-REX300 polishing machine;

[0080] Polishing pad: IC1010 type (Dupont);

[0081] Polishing materials and process parameters:

[0082] 1. Blanket wafer (unpatterned wafer)

[0083] a) 300mm W wafer (chemical vapor deposition W film thickness 10000Å);

[0084] b) 300mm PETEOS wafer (low pressure chemical vapor deposition TEOS thickness 5000 Å);

[0085] c) Polishing conditions:

[0086] Polishing upper and lower disc speed: 81 / 80rpm;

[0087] Polishing pressure: 4.0psi;

[0088] Flow rate: 300ml / min;

[0089] Polishing time: 60s;

[0090] The above-mentioned polishing conditions were used to perform polishing on the above-mentioned W wafer and PETEOS wafer, respectively, and the removal rate (MRR) was tested.

[0091] 2. Patterned wafer

[0092] a) Type 754, 300mm (Ramco Technology)

[0093] b) Polishing conditions:

[0094] Polishing upper and lower disc speed: 81 / 80rpm;

[0095] Polishing pressure: 4.0psi;

[0096] Flow rate: 300ml / min;

[0097] Polishing time: endpoint detection + over-polishing (10%) (i.e. Endpoint + OP (10%));

[0098] The polishing liquid used is filtered and then transported to the polishing disc by a peristaltic pump. A diamond dresser is used to dress and maintain the polishing pad after each polishing, and pre-polishing is performed before each polishing.

[0099] Polishing was performed on the above-mentioned patterned wafer using the above-mentioned polishing conditions and dishing measurement was performed.

[0100] Removal rate test:

[0101] 1) The sheet resistance Rs of the W wafer before and after polishing was measured using a four-probe resistivity tester (NAPSON RT3000). According to the formula: d = (ρ / Rs)×10 9 (where ρ is the resistivity of W, in Ω·cm; d is the film thickness, in Å; Rs is the sheet resistance, in Ω / sq), the difference in film thickness of the W wafer before and after polishing can be calculated, and then the removal rate --- MRR (Å / min) can be calculated based on the polishing time.

[0102] 2) An optical interferometry film thickness gauge (Nano SpecⅡ) was used to measure the film thickness of the PETEOS wafer before and after polishing, and the removal rate (MRR) (Å / min) was calculated based on the polishing time.

[0103] Dip measurement: The depth of the dip is measured with a step profiler (Bruker-Dektak XT) in Å. Table 2 shows the Dishing defect test results at line / space positions of 100µm / 100µm and 10µm / 10µm, the Erosion defect test results at line / space positions of 5µm / 5µm, 1µm / 1µm and 0.18µm / 0.18µm, and the EOE defect test results at line / space positions of 5µm / 5µm, 1µm / 1µm and 0.18µm / 0.18µm.

[0104] Unless otherwise specified, the raw materials and reagents used in the examples and comparative examples of the present invention can be purchased from commercial sources. For example, 5-hydroxytryptophan, leucine, L-phenylalanine, methyltyrosine, glycine, L-histidine, glycinamide, alaninamide, prolineamide, L-phenylalaninamide, N-isopropylglycinamide, homopiperazine, 1-methylhomopiperazine, and 1-formylhomopiperazine can all be purchased from Aladdin, and Nα-acetyl-L-arginine can be purchased from Sigma-Aldrich.

[0105] Preparation example:

[0106] Preparation of abrasive A:

[0107] Step 1): Adjust the pH value of deionized water to 6 with nitric acid, add 5g of N-cyclohexyl-γ-aminopropylmethyldimethoxysilane to 145g of deionized water, keep the water bath at 60°C, and continue magnetic stirring for 30min, then let it stand at room temperature for 4h to return to room temperature (25°C); Step 2): Add 250g of fumed silica colloid (40wt% solid content, average particle size 100nm, specific surface area 200m 2 / g) is added to the solution of step 1), and then magnetically stirred for 1 hour, and then placed at room temperature for 24 hours; step 3): the pH value of the fumed silica abrasive in step 2) is adjusted to 3.5 with nitric acid and set aside. The prepared modified fumed silica colloid has a solid content of 25wt% and a Zeta potential of about +35mV, i.e., abrasive A.

[0108] Preparation of abrasive B:

[0109] Step 1): Adjust the pH value of deionized water to 6 with nitric acid, add 5g of N-cyclohexyl-γ-aminopropylmethyldimethoxysilane to 145g of deionized water, keep the water bath at 60°C, and continue magnetic stirring for 30min, then let it stand at room temperature for 4h to return to room temperature (25°C); Step 2): Add 250g of fumed silica colloid (40wt% solid content, average particle size 180nm, specific surface area 140m 2 / g) is added to the solution of step 1), and then magnetically stirred for 1 hour, and then placed at room temperature for 24 hours; step 3): the pH value of the fumed silica abrasive in step 2) is adjusted to 3.5 with nitric acid and set aside. The prepared modified fumed silica colloid has a solid content of 25wt% and a Zeta potential of about +35mV, i.e., abrasive B.

[0110] Preparation of abrasive C:

[0111] Step 1): Adjust the pH value of deionized water to 6 with nitric acid, add 5g of N-cyclohexyl-γ-aminopropylmethyldimethoxysilane to 145g of deionized water, keep the water bath at 60°C, and continue magnetic stirring for 30min, then let it stand at room temperature for 4h to return to room temperature (25°C); Step 2): Add 250g of fumed silica colloid (40wt% solid content, average particle size 250nm, specific surface area 60m 2 / g) is added to the solution of step 1), and then magnetically stirred for 1 hour, and then placed at room temperature for 24 hours; step 3): the pH value of the fumed silica abrasive in step 2) is adjusted to 3.5 with nitric acid and set aside. The prepared modified fumed silica colloid has a solid content of 25wt% and a Zeta potential of about +35mV, i.e., abrasive C.

[0112] Example 1

[0113] The polishing composition was prepared by the following steps: 0.1 g of 5-hydroxytryptophan (first corrosion inhibitor), 0.1 g of glycineamide (second corrosion inhibitor), 0.03 g of homopiperazine (EOE improver), 0.2 g of ferric nitrate nonahydrate (catalyst), 100 g of hydrogen peroxide (40 wt %), and 1 g of citric acid (stabilizer) were added to 1750 g of deionized water (accounting for about 95% of the total amount of deionized water), stirred evenly, and then 80 g of abrasive A (25 wt % solid content, average particle size 100 nm, specific surface area 200 m 2 / g, pH value 3.5, Zeta potential of about +35mV) is added to the solution, and the pH value of the composition is adjusted to 2 with nitric acid under stirring, and the remaining amount of deionized water is continued to be added until the total mass of the dispersion is 2kg, and magnetic stirring is continued for 30min, and the solution is packaged for use.

[0114] Examples 2 to 17 and Comparative Examples 1 to 9 were prepared with reference to Example 1 for the preparation of polishing compositions. The raw materials, raw material amounts and pH values ​​of the polishing compositions of the various examples and comparative examples are shown in Table 1 below.

[0115] Table 1 Raw materials, raw material amounts and pH values ​​of the polishing compositions of the examples and comparative examples

[0116]

[0117] Table 1

[0118]

[0119] Table 1

[0120]

[0121] Table 1

[0122]

[0123] Note: Abrasive A, Abrasive B, and Abrasive C in Table 1 above are all prepared by the aforementioned preparation examples, as follows:

[0124] Abrasive A: modified fumed silica colloid, 25wt% solid content, average particle size 100nm, specific surface area 200m 2 / g, pH 3.5, Zeta potential about +35mV;

[0125] Abrasive B: modified fumed silica colloid, 25wt% solid content, average particle size 180nm, specific surface area 140m 2 / g, pH 3.5, Zeta potential about +35mV;

[0126] Abrasive C: modified fumed silica colloid, 25wt% solid content, average particle size 250nm, specific surface area 60m 2 / g, pH value 3.5, Zeta potential is about +35mV.

[0127] In Table 1, the amount of deionized water used as "balance" refers to the amount required to make the total mass of the polishing composition obtained be 2 kg.

[0128] The polishing compositions obtained in the examples and comparative examples were diluted with deionized water at a dilution multiple of 3 times according to the mass ratio and then subjected to polishing tests. The polishing test results are shown in Table 2 below:

[0129] Table 2 Polishing test results

[0130]

[0131] Table 2

[0132]

[0133] Table 2

[0134]

[0135] Comparing Comparative Example 1 and Example 4 in Table 2 above, where the comparative example does not contain a corrosion inhibitor, it can be found that the removal rate of W and PETEOS in Comparative Example 1 is significantly increased compared with Example 4; after calculation, the selectivity ratio of the removal rate of W and PETEOS in Comparative Example 1 and Example 4 is close, but the Dishing and Erosion at different line widths in Comparative Example 1 are greatly deteriorated. This shows that the first corrosion inhibitor and the second corrosion inhibitor used in the present invention can be effectively adsorbed on the surface of the polished tungsten substrate to form a protective film layer, and the catalytic oxidation process during the polishing process is inhibited through synergistic action, thereby effectively reducing the Dishing and Erosion defects.

[0136] Comparing Comparative Example 2 with Example 4 in Table 2 above, where Comparative Example 2 only contains the same amount of the first corrosion inhibitor as Example 4, it can be found that the removal rate of Comparative Example 2 for W and PETEOS is slightly higher than that of Example 4, but the depth of Dishing and Erosion produced by Comparative Example 2 is much higher than that of Example 4 (more than 1 times higher). Comparing Comparative Example 4 with Example 4 in Table 2 above, where the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor in Comparative Example 4 is 0.25, and the total amount of the two is equal to that of Example 4, it can be found that the removal rate of Comparative Example 4 for W is significantly lower than that of Example 4, but the depth of Dishing and Erosion is still higher than that of Example 4. This shows that the first corrosion inhibitor can be strongly adsorbed on the surface of the polished tungsten substrate, and it is easy to achieve a strong suppression of the removal rate, but its control of the polishing defects Dishing and Erosion is not enough. The reason may be that with the rapid temperature rise during the polishing process, the adsorption film layer formed by this type of substance is not dense and stable enough.

[0137] Comparing Comparative Example 3 with Example 4 in Table 2 above, where Comparative Example 3 only contains the same amount of the second corrosion inhibitor as Example 4, it can be found that the removal rate of W in Comparative Example 3 is slightly higher than that in Example 4, but the depth of Dishing and Erosion produced by Comparative Example 3 is much higher than that in Example 4. Comparing Comparative Example 5 with Example 4 in Table 2 above, where the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor in Comparative Example 5 is 799, and the total amount of the two is equal to that in Example 4, it can be found that the removal rate of W in Comparative Example 5 is close to that in Example 4, but the defect level is still significantly higher than that in Example 4. This shows that the second corrosion inhibitor is relatively weakly adsorbed on the surface of the tungsten substrate. Although the removal rate can be suppressed at a high content, the control of defects Dishing and Erosion is still not ideal. The reason may be that the film layer formed by this type of substance is not dense enough and the protection of the tungsten substrate is insufficient.

[0138] Comparing Comparative Example 6 with Example 4 in Table 2 above, where Comparative Example 6 does not contain an EOE improver, it can be found that the depth of Dishing and Erosion between Comparative Example 6 and Example 4 is relatively small, but the EOE depth of Comparative Example 6 is significantly higher than that of Example 4. This shows that under the condition of containing the first and second corrosion inhibitors, the addition of homopiperazine and its derivatives can effectively reduce the EOE defects caused by polishing. Compared with Example 4, Comparative Examples 7 and 8 are mainly different in the content of EOE improver, and the others are consistent. From the comparison results, the EOE improver content is too low, and the improvement effect on EOE is not obvious. If the EOE improver content is too high, it is not only difficult to further improve the EOE defect depth, but also the inhibition of the removal rate is more serious. Compared with Example 4, Comparative Example 9 reflects the obvious advantages of homopiperazine and its derivatives as EOE improvers compared with general heterocyclic organic amines.

[0139] From the experimental results in Table 1, it can be seen that the polishing composition of the present invention contains both a first corrosion inhibitor and a second corrosion inhibitor, which are used in combination at a suitable ratio, and a suitable amount of an EOE improver is used in combination. The resulting polishing composition can achieve a good balance between a good polishing rate and relatively low defects (Dishing, Erosion and EOE defects). It can not only control the polishing rate well, but also have relatively low defects (Dishing, Erosion) at positions with larger line widths and positions with smaller line widths. At the same time, it can reduce the EOE depth and reduce the contact resistance at the edge position.

[0140] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.

Claims

1. A chemical mechanical polishing composition, characterized in that The composition comprises a dispersion medium, an abrasive, a catalyst, an oxidant, a first corrosion inhibitor, a second corrosion inhibitor and an EOE improver, and optionally further comprises a stabilizer and a pH adjuster; wherein the first corrosion inhibitor is selected from one or more compounds having a total of 1 to 4 amino and imino groups in the molecule and at least one carboxyl group; The second corrosion inhibitor is selected from one or more compounds having a total of 2 amino and imino groups in the molecule, at least one amide group, and no carboxyl group, hydroxyl group, alkenyl group, or alkynyl group; The EOE improving agent is selected from one or more of homopiperazine and its derivatives; Based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.01 wt%-2.0 wt%, and the mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 1-299; the content of the EOE improver is 15 ppm-300 ppm.

2. The chemical mechanical polishing composition according to claim 1, characterized in that Based on the total mass of the composition, the total content of the first corrosion inhibitor and the second corrosion inhibitor is 0.1 wt%-1.0 wt%; And / or, based on the total mass of the composition, the content of the EOE improver is 50 ppm-200 ppm.

3. The chemical mechanical polishing composition according to claim 1, characterized in that The mass ratio of the second corrosion inhibitor to the first corrosion inhibitor is 49-199.

4. The chemical mechanical polishing composition according to any one of claims 1 to 3, characterized in that The second corrosion inhibitor is selected from one or more of glycinamide, Boc-glycinamide, N-isopropylglycinamide, N-valeroylglycinamide, prolineamide, alaninamide, Boc-L-alaninamide, N-acetyl-L-alaninamide, L-phenylalaninamide, Boc-L-isoleucinamide, Boc-L-leucinamide, Boc-D-valinamide, and N-benzoyl-L-tyrosinamide.

5. The chemical mechanical polishing composition according to any one of claims 1 to 3, characterized in that The first corrosion inhibitor is selected from the group consisting of tryptophan, 1-methyl-DL-tryptophan, 6-methyl-DL-tryptophan, 7-methyl-DL-tryptophan, N-formyl-DL-tryptophan, N-acetyl-DL-tryptophan, glycyl-DL-tryptophan, 5-hydroxytryptophan, lysine, N-acetyl-L-lysine, trifluoroacetyl-lysine, L-histidine, D-histidine, DL-histidine, Boc-histidine, N-acetyl-L-histidine, 1-methyl-L-histidine, arginine, homoarginine, N-Boc-L-arginine, N-ω-propyl-L-arginine, Nα-acetyl-L-arginine, leucine, isoleucine, glycyl-D-leucine, glycyl-DL-leucine, L-phenylalanine, D-phenylalanine, 2-methyl -L-phenylalanine, 4-methyl-L-phenylalanine, 4-methoxy-L-phenylalanine, N-acetyl-L-phenylalanine, glycyl-DL-phenylalanine, 4-amino-L-phenylalanine, tyrosine, 3-amino-L-tyrosine, glycyl-L-tyrosine, 3-hydroxy-L-tyrosine, N-acetyl-L-tyrosine, N-methyl-L-tyrosine, methyltyrosine, O-methyl-D-tyrosine, O-tert-butyl-L-tyrosine, glycine, BOC-glycine, N-phenylglycine, L-trifluoroacetylglycine, N-formylglycine, N-acetylglycine, cyclopentylglycine, glutamic acid, L-methionine, D-methionine, DL-methionine, threonine, cysteine, N-acetyl-L-cysteine; And / or, the EOE improver is selected from one or more of homopiperazine, 1-methyl homopiperazine, 1-ethyl homopiperazine, 1-Boc-homopiperazine, 1-formyl homopiperazine, 1-acetyl homopiperazine, 1,7-dimethyl-1,4-homopiperazine, 1-(2-methoxyethyl)homopiperazine, 1-benzyl homopiperazine, 1-(2-aminoethyl)-4-methylhomopiperazine, 1-isobutyl-1,4-homopiperazine, 1-pyrazin-2-yl-1,4-homopiperazine, 1-(4-methylbenzyl)homopiperazine, and 1-Boc-5-methyl-1,4-homopiperazine.

6. The chemical mechanical polishing composition according to any one of claims 1 to 3, characterized in that The dispersion medium is deionized water; And / or, the abrasive is fumed silica colloidal; And / or, the catalyst is ferric nitrate nonahydrate; And / or, the oxidant is hydrogen peroxide; and / or, the stabilizer is selected from one or more of acetic acid, citric acid, tartaric acid, oxalic acid, lactic acid, malic acid, malonic acid, succinic acid, glutaric acid, pimelic acid, suberic acid, maleic acid, glycolic acid, diglycolic acid, glyceric acid, and succinic acid; And / or, the pH adjuster is selected from one or more of an inorganic acid, an inorganic base and an organic base.

7. The chemical mechanical polishing composition according to claim 6, characterized in that: The average particle size of the abrasive is 100nm-250nm; And / or, the specific surface area of ​​the abrasive is 60m 2 / g -200m 2 / g; And / or, the abrasive surface has a permanent positive charge.

8. The chemical mechanical polishing composition according to any one of claims 1 to 3, characterized in that The content of the abrasive in the composition is 1.0 wt%-9.0 wt% based on the solid content of the abrasive; and / or, the content of the catalyst in the composition is 0.01 wt%-0.5wt%; and / or, the content of the oxidant in the composition is 2 wt%-10 wt%; And / or, the content of the stabilizer in the composition is 0.05 wt%-1.2 wt%.

9. The chemical mechanical polishing composition according to any one of claims 1 to 3, characterized in that The pH value of the composition is 2-4.

10. Use of the chemical mechanical polishing composition according to any one of claims 1 to 9 in chemical mechanical polishing of tungsten.

Citation Information

Patent Citations

  • Tungsten-processing slurry with cationic surfactant and cyclodextrin

    CN108350318A

  • Chemical mechanical polishing composition comprising anionic and cationic inhibitors

    CN116134110A

  • Chemical mechanical polishing composition and polishing method

    CN116333686A

  • Polishing composition including inhibitor of tungsten etching

    CN1272221A

  • Tungsten buff polishing compositions with improved topography

    CN111566175A