A synergistically enhanced fine-grained high-temperature molybdenum-copper based composite material and a preparation method thereof

Through solid solution strengthening, dispersion strengthening and fine crystal strengthening mechanisms, combined with high-energy ball milling and high-current rapid sintering technology, a molybdenum-copper-based composite material with high density and uniform fine crystal structure was prepared, solving the problem of existing molybdenum-copper alloys at high temperatures The problem of insufficient performance is suitable for high-end applications.

CN118406949BActive Publication Date: 2024-11-01CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410531107.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-11-01
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

The density, strength and microstructure uniformity of existing molybdenum-copper alloys are insufficient, making it difficult to meet the high-temperature and high-performance needs in the fields of aerospace and microelectronics.

Method used

A synergistically enhanced fine crystal high-temperature molybdenum-copper-based composite material is used to prepare materials with uniform fine crystal structure and high density through solid solution strengthening, dispersion strengthening and fine crystal strengthening mechanisms, combined with high-energy ball milling and high current rapid sintering technology.

Benefits of technology

It significantly improves the density and hardness of molybdenum-copper-based composite materials, forms a brand new alloy phase, solves the problem of insufficient performance of traditional molybdenum-copper alloys at high temperatures, and is suitable for high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118406949B_ABST
    Figure CN118406949B_ABST
Patent Text Reader

Abstract

The invention discloses a synergistically enhanced fine-grained high-temperature molybdenum-copper-based composite material and a preparation method thereof, and relates to the field of refractory molybdenum-based composite materials and powder metallurgy technology. The composite material comprises the following raw materials in mass percentage: 1-45% copper, 0.1-1% zirconium carbide, 1-15% aluminum, and the balance is molybdenum. The preparation method comprises the following steps: step-by-step ball milling of zirconium carbide, aluminum, molybdenum and copper powder, pressing the mixed powder into a green body, further cold isostatic pressing to improve the green body density, and finally preparing a synergistically enhanced fine-grained high-temperature molybdenum-copper-based composite material at a relatively low temperature under the coupling of heat, electricity and force fields with a specific heating process. The molybdenum-copper-based composite material prepared by the present invention forms a brand-new alloy phase with a uniform fine-grained structure, and utilizes mechanisms such as solid solution strengthening, dispersion strengthening and fine-grained strengthening to synergistically enhance the hardness and strength of the material, effectively solving the problems of insufficient density, insufficient strength and poor uniformity of microstructure of existing molybdenum-copper alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory molybdenum-based composite materials and powder metallurgy, and in particular to a synergistically enhanced fine-grained high-temperature molybdenum-copper-based composite material and a preparation method thereof. Background Art

[0002] Molybdenum copper is a typical binary pseudo alloy, which combines the high melting point and high strength of molybdenum with the high plasticity, high electrical conductivity and high thermal conductivity of copper. It has been widely used in the fields of national economy, military, aerospace and other high-tech fields, such as electrode electrical contact materials, heat sink packaging materials, rocket nozzles, missile nozzle throat liners, gas rudders and other high-temperature components. Compared with similar tungsten copper binary pseudo alloys, the heat resistance, high temperature strength and gas ablation resistance of molybdenum copper materials are not as good as tungsten copper alloys, but molybdenum copper alloys are lighter than tungsten copper alloys and have better heat dissipation rate, stability and machinability than tungsten copper alloys. Therefore, molybdenum copper alloys have more advantages in being used as connectors and heat dissipation components, such as electronic packaging and heat sink materials that require light weight. However, with the rapid development of industrial applications and the emergence of high-end demands, various extreme and harsh service environments have put forward higher requirements on the comprehensive performance of components and devices. At present, it is difficult for traditional molybdenum copper materials to meet the requirements of high performance at high temperatures.

[0003] my country has very rich molybdenum ore resources, which provides a guarantee for my country to vigorously develop molybdenum-based composite materials. However, since molybdenum and copper are immiscible and have poor wettability, and there is a huge difference in the melting points of molybdenum and copper, the melting point of molybdenum is as high as 2622℃ and the melting point of copper is 1083℃, which makes the sintering of molybdenum-copper alloy poor, bringing great challenges to the preparation of molybdenum-copper alloy.

[0004] At present, molybdenum-copper composite materials are mainly prepared by high-temperature liquid phase method, melt infiltration method and field-assisted sintering. However, the high-temperature liquid phase method or melt infiltration method not only has the problems of high sintering temperature, long holding time, uneven distribution of copper phase, grain growth and complex preparation process, but also the prepared molybdenum-copper alloy has the inverse contradiction between density and grain size, and the microstructure uniformity is poor, and the comprehensive performance of the alloy is not high. The prior art prepares molybdenum-copper alloy by field-assisted activation, so that the compact can quickly complete the densification process at a lower temperature, the preparation process is easy to control, and the sintering process does not need to add activation elements, thereby improving the product quality. However, the density, strength and hardness of the molybdenum-copper alloy prepared by this method have no outstanding advantages over the existing molybdenum-copper and tungsten-copper alloys, and still cannot solve the problem of high temperature and high performance in the fields of aerospace and microelectronics, thereby restricting its application in the field of high-tech. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material and a preparation method thereof. The method is simple and easy to implement and has strong pertinence. The obtained fine-grained high-temperature molybdenum-copper based composite material forms a brand-new alloy phase with a uniform fine-grained structure. The hardness and strength of the material are synergistically enhanced by strengthening mechanisms such as solid solution strengthening, dispersion strengthening and fine grain strengthening, thereby effectively solving the problems of insufficient density and strength and poor microstructural uniformity of existing molybdenum-copper alloys.

[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention to solve its technical problem is: to provide a synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material, comprising the following raw materials in mass percentage: 1-45% copper, 0.1-1% zirconium carbide, 1-15% aluminum, and the balance is molybdenum.

[0007] Furthermore, the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material includes the following raw materials in percentage by mass: 30% copper, 0.4% zirconium carbide, 4.6% aluminum and 65% molybdenum.

[0008] Furthermore, the zirconium carbide is a nano-scale powder with a particle size of 100-500 nm.

[0009] Furthermore, aluminum, molybdenum and copper are in the form of micron-sized powders, the particle sizes of aluminum and molybdenum are 2-10 μm, and the particle size of copper is 1-5 μm.

[0010] The preparation method of the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material comprises the following steps:

[0011] S1, ball-milling zirconium carbide powder, aluminum powder and molybdenum powder to obtain mixed powder 1;

[0012] S2, adding copper powder to the mixed powder 1 obtained in step S1 and ball milling to obtain mixed powder 2;

[0013] S3, pressing the mixed powder obtained in step S2 into a green body, and then cold isostatic pressing to increase the density of the green body, and then sintering the green body under the coupling of thermal field, electric field and force field, and cooling to room temperature after sintering to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material.

[0014] Furthermore, in step S1, the ball-to-material ratio is 2.5-15:1.

[0015] Furthermore, the ball milling speed is 450-600 r / min.

[0016] Furthermore, the ball milling was stopped for 20-30 minutes after every 90-120 minutes.

[0017] Furthermore, the total effective ball milling time is 48-120h.

[0018] Furthermore, the wall of the ball mill is scraped and powdered in a glove box every 12-18 hours.

[0019] The beneficial effects of adopting the above further technical solution are: promoting the solid solution of aluminum into the molybdenum particles and the dispersed distribution of zirconium carbide.

[0020] Further, in step S2, the ball milling speed is 100-300 r / min, and the ball milling time is 4-12 h.

[0021] Furthermore, in step S3, the green body is first pressed into a cylindrical green body with a relative density of 65-75%, and then cold isostatic pressing is performed to increase the relative density of the green body to 75-85%.

[0022] Furthermore, the pressure of cold isostatic pressing is 200-500 MPa, and the pressure is maintained for 2-10 minutes.

[0023] Furthermore, during the sintering process, the voltage is 3-10V and the current is 5000-100000A.

[0024] Furthermore, while the temperature is raised, the pressure is increased from 1-10 MPa to 40-80 MPa at a rate of 3-10 MPa / min and then kept constant until the sintering is completed.

[0025] Furthermore, during sintering, the temperature is first raised from room temperature to 180-220°C at a rate of 2-30°C / s and kept for 2-15 minutes, then raised to 600-700°C at a rate of 2-150°C / s and kept for 5-10 minutes, and finally raised to 800-1100°C at a rate of 5-150°C / s and kept for 5-20 minutes.

[0026] In summary, the present invention has the following beneficial effects:

[0027] 1. The density of the molybdenum-copper-based composite material prepared by the method provided by the present invention is greater than 95%, and the average grain size can be controlled below 200-500nm. The composite material can achieve higher strength by means of various strengthening mechanisms such as solid solution strengthening, dispersion strengthening and fine grain strengthening, thereby obtaining a molybdenum-copper-based composite material with high density, uniform fine grain structure and significantly improved hardness.

[0028] 2. The present invention promotes the improvement of material performance from the following aspects: First, the molybdenum, aluminum and zirconium carbide powder particles are subjected to high-energy ball milling to the nanoscale or near-nanoscale. This process promotes the solid dissolution of aluminum into the molybdenum lattice to form a supersaturated solid solution. These solid solutions not only have a strengthening effect, but also because molybdenum has a certain solubility in aluminum, aluminum can also serve as a diffusion channel for molybdenum atoms under the action of thermal-electric-mechanical coupling, thereby effectively promoting the densification of the powder during the sintering process, and at the same time using the dispersed nanocarbide particles to effectively improve the hardness of the material; Second, through the first principle The calculation results show that the solid solution of aluminum also significantly increases the interface bonding energy between molybdenum and copper, forming a tighter bonding interface, improving the interface bonding between molybdenum and copper and promoting the densification of the material; thirdly, the surface energy of the mixed powder particles after high-energy ball milling increases, and the sintering activity increases, which is also conducive to achieving rapid densification at low temperatures; fourthly, on this basis, the present invention makes full use of the characteristics of high-current rapid sintering technology, which has fast heating and cooling speeds and is prone to "field emission effect", generating huge energy in a short time, so that the sintering temperature is instantly higher than the melting point of copper. The sintering mechanism of molybdenum-copper-based composite materials is transformed from traditional solid-phase sintering to "solid-phase sintering with instantaneous liquid phase", thereby obtaining a molybdenum-copper-based composite material with high density, high strength and uniform fine-grained structure.

[0029] 3. The raw material components of the synergistically enhanced fine-grained molybdenum-copper-based composite material provided by the present invention have been subjected to long-term computer simulation and experimental research iterations, and a new optimized component application and a correlation relationship between the proportions have been proposed, a new experimental scheme has been designed, and the phase composition of the molybdenum-copper composite material prepared by the traditional method has been changed. The composite material prepared by the present invention forms a new alloy base phase under a non-equilibrium state. In addition to the molybdenum and copper phases, new phases such as molybdenum-copper, molybdenum-aluminum, and copper-aluminum solid solutions are formed, and these new phases have a significant solid solution strengthening effect; the nano-zirconium carbide particles are dispersed between the molybdenum particles, which can effectively inhibit the growth of molybdenum grains and have a strengthening effect, so that the molybdenum-copper-based composite material prepared by the present invention has significantly improved hardness and strength compared with the traditional micron-scale coarse-grained composite material; the hardness of the molybdenum-copper-based composite material prepared by the present invention is significantly improved under the synergistic strengthening effect of fine grain strengthening, dispersion strengthening and solid solution strengthening, which solves the technical problem of insufficient strength of the molybdenum-copper composite material prepared by the prior art.

[0030] 4. The preparation process of the synergistically reinforced fine-grained molybdenum-copper based composite material provided by the present invention has undergone a new optimal design, and the optimal process parameters have been selected through computer simulation prediction and experimental verification; the present invention calculates the phase stability of the system and the reaction generation temperature based on the first principles, while considering the sintering neck formation temperature of each component in the system (the sintering neck formation temperature of the molybdenum powder particles is 653°C), and heat preservation is performed at different temperatures, so as to control the formation of favorable new phases and the formation and growth of sintering necks, thereby achieving rapid realization of high densification of materials at a relatively low temperature.

[0031] 5. In the preparation method of the synergistically reinforced fine-grained molybdenum-copper based composite material provided by the present invention, in order to prevent the green body from generating defects such as cracks due to excessive loading pressure at the beginning, as the sintering progresses, the strength of the material sintering neck is formed and grows up, and its ability to withstand pressure also gradually increases. Therefore, a gradient pressurization method is adopted to enable the composite material to be further sintered and densified under a greater pressure. Compared with the normal pressure method, the material is densified under a higher pressure, which can effectively improve the density and key performance of the material.

[0032] 6. The present invention provides a method for preparing a synergistically enhanced fine-grained high-temperature molybdenum-copper-based composite material. The method has a wide range of applications and can flexibly adjust the component composition and grain size in the molybdenum-copper-based composite material according to actual performance requirements, thereby achieving "on-demand customization" of the material, thereby meeting the needs of different service occasions and effectively exerting the performance advantages of the new material.

[0033] 7. The method provided by the present invention is efficient, rapid, energy-saving, environmentally friendly, simple and easy to implement, and highly targeted. It is an innovative technology for preparing molybdenum-copper-based composite materials with uniform fine-grained structure, high density and high hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a microstructure morphology of the fine-grained high-temperature molybdenum-copper based composite material prepared in Example 1. DETAILED DESCRIPTION

[0035] The present invention is further described below in conjunction with the embodiments and drawings, but the present invention is not limited thereto.

[0036] Example 1

[0037] A synergistically reinforced fine-grained high-temperature molybdenum-copper matrix composite material comprises the following raw materials in percentage by mass: 30% copper, 0.4% zirconium carbide, 4.6% aluminum and 65% molybdenum.

[0038] The preparation method of the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material comprises the following steps:

[0039] S1. Add zirconium carbide powder, aluminum powder and molybdenum powder with particle sizes of 200 nm, 3 μm and 2 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 10:1, the ball milling speed is 500 r / min, and the ball milling is stopped for 25 minutes after every 100 minutes of ball milling. The total effective ball milling time is 60 hours to obtain mixed powder 1;

[0040] S2, adding copper powder with a particle size of 3 μm to the mixed powder 1 obtained in step S1, and performing low-speed ball milling at a speed of 200 r / min for 6 h until the mixture is uniformly mixed to obtain mixed powder 2;

[0041] S3, the mixed powder obtained in step S2 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%. The pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes. Then the green body is placed in a heating device. The voltage of the sintering process is 3-10V, and the current is 25000A. The green body is heated to 200°C at a rate of 20°C / s and kept warm for 5 minutes, then heated to 675°C at a rate of 60°C / s and kept warm for 5 minutes, then heated to 950°C at a rate of 75°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is 3MPa. While heating, the sintering pressure is increased at a rate of 10MPa / min to 60MPa and then kept constant. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material.

[0042] Example 2

[0043] A synergistically reinforced fine-grained high-temperature molybdenum-copper matrix composite material comprises the following raw materials in percentage by mass: 30% copper, 0.8% zirconium carbide, 4.2% aluminum and 65% molybdenum.

[0044] The preparation method of the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material comprises the following steps:

[0045] S1. Add zirconium carbide powder, aluminum powder and molybdenum powder with particle sizes of 100 nm, 10 μm and 10 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 10:1, the ball milling speed is 500 r / min, and the ball milling is stopped for 25 minutes after every 100 minutes of ball milling. The total effective ball milling time is 60 hours to obtain mixed powder 1;

[0046] S2, adding copper powder with a particle size of 3 μm to the mixed powder 1 obtained in step S1, and performing low-speed ball milling at a speed of 200 r / min for 6 h until the mixture is uniformly mixed to obtain mixed powder 2;

[0047] S3, the mixed powder obtained in step S2 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%. The pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes. Then the green body is placed in a heating device. The voltage of the sintering process is 3-10V, and the current is 25000A. The green body is heated to 200°C at a rate of 20°C / s and kept warm for 5 minutes, then heated to 675°C at a rate of 60°C / s and kept warm for 5 minutes, then heated to 950°C at a rate of 75°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is 3MPa. While heating, the sintering pressure is increased at a rate of 10MPa / min to 60MPa and then kept constant. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material.

[0048] Example 3

[0049] A synergistically reinforced fine-grained high-temperature molybdenum-copper matrix composite material comprises the following raw materials in percentage by mass: 45% copper, 1% zirconium carbide, 15% aluminum and 39% molybdenum.

[0050] The preparation method of the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material comprises the following steps:

[0051] S1. Add zirconium carbide powder, aluminum powder and molybdenum powder with particle sizes of 100 nm, 2 μm and 2 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 2.5:1, the ball milling speed is 450 r / min, and the ball milling is stopped for 20 minutes every 90 minutes. The total effective ball milling time is 48 hours to obtain mixed powder 1;

[0052] S2, adding copper powder with a particle size of 1 μm to the mixed powder 1 obtained in step S1, and performing low-speed ball milling at a speed of 100 r / min for 4 h until the mixture is uniformly mixed to obtain mixed powder 2;

[0053] S3, the mixed powder obtained in step S2 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 75%, the pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes, and then the green body is placed in a heating device. The voltage of the sintering process is 3-10V, and the current is 15000A. The green body is heated to 180°C at a rate of 5°C / s and kept warm for 2 minutes, then heated to 600°C at a rate of 5°C / s and kept warm for 5 minutes, and then heated to 900°C at a rate of 50°C / s and kept warm for 5 minutes. Before the high current is turned on, the pressure is 1MPa. While heating, the sintering pressure is increased at a rate of 5MPa / min to 40MPa and then kept constant. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material.

[0054] Example 4

[0055] A synergistically reinforced fine-grained high-temperature molybdenum-copper matrix composite material comprises the following raw materials in percentage by mass: 1% copper, 0.1% zirconium carbide, 1% aluminum and 97.9% molybdenum.

[0056] The preparation method of the above-mentioned synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material comprises the following steps:

[0057] S1. Add zirconium carbide powder, aluminum powder and molybdenum powder with particle sizes of 200 nm, 10 μm and 10 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 15:1, the ball milling speed is 600 r / min, and the ball milling is stopped for 30 minutes every 120 minutes. The total effective ball milling time is 120 hours to obtain mixed powder 1;

[0058] S2, adding copper powder with a particle size of 5 μm to the mixed powder 1 obtained in step S1, and performing low-speed ball milling at a speed of 300 r / min for 12 h until the mixture is uniformly mixed to obtain mixed powder 2;

[0059] S3, the mixed powder obtained in step S2 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%. The pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes. Then the green body is placed in a heating device. The voltage of the sintering process is 3-10V, and the current is 50000A. The green body is heated to 220°C at a rate of 30°C / s and kept warm for 15 minutes, then heated to 700°C at a rate of 75°C / s and kept warm for 10 minutes, and then heated to 1100°C at a rate of 150°C / s and kept warm for 20 minutes. Before the high current is turned on, the pressure is 10MPa. While heating, the sintering pressure is increased at a rate of 10MPa / min to 80MPa and then kept constant. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper-based composite material.

[0060] Comparative Example 1

[0061] A fine-grained high-temperature molybdenum-copper composite material comprises the following raw materials in percentage by mass: 70% molybdenum and 30% copper.

[0062] The method for preparing the above-mentioned fine-grained high-temperature molybdenum-copper composite material comprises the following steps:

[0063] S1. Add molybdenum powder and copper powder with particle sizes of 3 μm and 2 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 2.5:1, the ball milling speed is 500 r / min, and the total effective ball milling time is 60 h to obtain mixed powder 1;

[0064] S2, the mixed powder obtained in step S1 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%, the pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes, and then the green body is placed in a heating device. During the sintering process, the current is 25000A, the voltage is 3-10V, the green body is heated to 200°C at 20°C / s and then kept warm for 5 minutes, then heated to 675°C at 60°C / s and kept warm for 5 minutes, and then heated to 950°C at 75°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is set to 3MPa, and the sintering pressure is increased at a rate of 10MPa / min to 60MPa and then kept constant. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a fine-grained high-temperature molybdenum-copper composite material.

[0065] Comparative Example 2

[0066] A synergistically reinforced fine-grained high-temperature molybdenum-copper-aluminum composite material comprises the following raw materials in percentage by mass: 65% molybdenum, 30% copper and 5% aluminum.

[0067] The preparation method of the above-mentioned synergistically enhanced fine-grained high-temperature molybdenum-copper-aluminum composite material comprises the following steps:

[0068] S1. Add molybdenum powder and aluminum powder with particle sizes of 3 μm and 2 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 2.5:1, the ball milling speed is 500 r / min, and the total effective ball milling time is 60 h to obtain mixed powder 1;

[0069] S2, adding copper powder with a particle size of 2 μm to the mixed powder 1, and performing low-speed ball milling at 200 r / min for 6 h to mix evenly to obtain mixed powder 2;

[0070] S3, the mixed powder obtained in step S2 is loaded into a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%. The pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes. The green body is placed in a heating device. During the sintering process, the current is 35000A and the voltage is 3-10V. The green body is heated to 200°C at 20°C / s and then kept warm for 5 minutes, then heated to 675°C at 20°C / s and kept warm for 5 minutes, then heated to 950°C at 90°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is set to 3MPa, and the sintering pressure is increased to 60MPa at a rate of 10MPa / min while the temperature is increased. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically enhanced fine-grained high-temperature molybdenum-copper-aluminum composite material.

[0071] Comparative Example 3

[0072] A synergistically enhanced fine-grained high-temperature molybdenum-copper-zirconium carbide composite material comprises the following raw materials in percentage by mass: 69.6% molybdenum, 30% copper and 0.4% zirconium carbide.

[0073] The preparation method of the above-mentioned synergistically enhanced fine-grained high-temperature molybdenum-copper-zirconium carbide composite material comprises the following steps:

[0074] S1. Add molybdenum powder and zirconium carbide powder with particle sizes of 3 μm and 200 nm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 1:1, the ball milling speed is 500 r / min, and the total effective ball milling time is 60 h to obtain mixed powder 1;

[0075] S2, adding copper powder with a particle size of 2 μm to the mixed powder 1, and performing low-speed ball milling at 200 r / min for 6 h to mix evenly to obtain mixed powder 2;

[0076] S3, the mixed powder obtained in step S2 is loaded into a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed to increase the relative density of the green body to 83%. The pressure of the cold isostatic pressing is 350MPa, and the pressure is maintained for 6 minutes. The green body is placed in a heating device. During the sintering process, the current is 20000A and the voltage is 3-10V. The green body is heated to 200°C at 20°C / s and then kept warm for 5 minutes, then heated to 675°C at 20°C / s and kept warm for 5 minutes, then heated to 950°C at 60°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is set to 3MPa, and the sintering pressure is increased to 60MPa at a rate of 10MPa / min while the temperature is increased. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper-zirconium carbide composite material.

[0077] Comparative Example 4

[0078] A synergistically reinforced molybdenum-copper matrix composite material comprises the following raw materials in percentage by mass: 30% copper, 0.4% zirconium carbide, 4.6% aluminum and 65% molybdenum.

[0079] The preparation method of the above-mentioned synergistically reinforced molybdenum-copper based composite material comprises the following steps:

[0080] S1. Add zirconium carbide powder, aluminum powder and molybdenum powder with particle sizes of 200 nm, 3 μm and 2 μm respectively into a ball mill for high-energy vibration ball milling. The ball-to-material ratio is 2.5:1, the ball milling speed is 500 r / min, and the total effective ball milling time is 60 h to obtain mixed powder 1;

[0081] S2, adding copper powder with a particle size of 2 μm to the mixed powder 1 obtained in step S1, and performing low-speed ball milling for 6 hours until the mixture is uniformly mixed to obtain mixed powder 2;

[0082] S3, the mixed powder obtained in step S2 is placed in a mold and pressed into a green body with a cylindrical structure, and the green body is further cold isostatically pressed at a pressure of 200 MPa, and the pressure is maintained for 2 minutes to increase the relative density of the green body to 80%, and then the green body is placed in a heating device. During the sintering process, the current is 10000A and the voltage is 3-10V. The green body is heated to 200°C at 20°C / s and then kept warm for 5 minutes, then heated to 675°C at 20°C / s and kept warm for 5 minutes, then heated to 950°C at 25°C / s and kept warm for 10 minutes. Before the high current is turned on, the pressure is 3MPa, and the sintering pressure is increased to 60MPa at a rate of 10MPa / min while the temperature is increased. Finally, the current is turned off and the furnace is cooled to room temperature to obtain a synergistically reinforced molybdenum-copper based composite material.

[0083] Test Example 1

[0084] During the sintering process, the shape of the green body remains intact, and the obtained fine-grained high-temperature molybdenum-copper-based composite material has a high degree of densification. The fine-grained high-temperature molybdenum-copper-based composite material obtained in Example 1 was observed using a scanning electron microscope. The results are as follows: Figure 1 shown.

[0085] Depend on Figure 1 It can be seen that the fine-grained high-temperature molybdenum-copper-based composite material prepared by the method provided by the present invention has extremely fine grains and the distribution of each phase is very uniform.

[0086] Test Example 2

[0087] The Archimedean method was used to measure the actual density of the fine-grained high-temperature molybdenum-copper based composite materials obtained in Example 1 and Example 2 and the composite materials obtained in Comparative Examples 1-4, and the relative density was calculated. The hardness of the composite materials was measured using a Vickers hardness tester. The results are shown in Table 1.

[0088] Table 1 Performance comparison of different composite materials

[0089]

[0090] It can be seen from Table 1 that the relative density and hardness of the fine-grained high-temperature molybdenum-copper-based composite materials prepared in Example 1 and Example 2 are higher than those of the composite material prepared in the comparative example, which shows that the component composition, ratio, raw material particle size and preparation process all significantly affect the performance of the material. The fine-grained high-temperature molybdenum-copper-based composite material prepared by the method provided by the present invention has greatly improved density and hardness.

[0091] Although the specific implementation of the present invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A synergistically enhanced fine-grained high-temperature molybdenum-copper matrix composite material, It is characterized in that The invention is composed of the following raw materials in percentage by mass: 1-45% copper, 0.1-1% zirconium carbide, 1-15% aluminum and the balance molybdenum.

2. The synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 1, It is characterized in that The invention comprises the following raw materials in percentage by weight: 30% copper, 0.4% zirconium carbide, 4.6% aluminum and 65% molybdenum.

3. The synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 1 or 2, It is characterized in that The zirconium carbide is nanometer-grade powder with a particle size of 100-500nm; the aluminum, molybdenum and copper are micrometer-grade powders with a particle size of 2-10μm and a particle size of 1-5μm.

4. A method for preparing the synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1. Ball mill zirconium carbide powder, aluminum powder and molybdenum powder to obtain mixed powder 1, with a ball-to-material ratio of 2.5-15:1, a ball milling speed of 450-600 r / min, and a stop of 20-30 min for each ball milling of 90-120 min. The total effective ball milling time is 48-120 h; S2, adding copper powder to the mixed powder 1 obtained in step S1 and ball milling to obtain mixed powder 2, the ball milling speed is 100-300r / min, and the ball milling is performed for 4-12h; S3, pressing the mixed powder obtained in step S2 into a green body, and then cold isostatic pressing to increase the density of the green body, and then sintering the green body under the coupling of thermal field, electric field and force field, and cooling to room temperature after sintering to obtain a synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material.

5. The method for preparing the synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 4, It is characterized in that In step S3, the green body is first pressed into a cylindrical green body with a relative density of 65-75%, and then cold isostatically pressed to increase the relative density of the green body to 75-85%.

6. A method for preparing a synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 4 or 5, It is characterized in that The cold isostatic pressing pressure is 200-500 MPa, and the pressure is maintained for 2-10 minutes.

7. The method for preparing the synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 4, It is characterized in that In step S3, during the sintering process, the voltage is 3-10V and the current is 5000-100000A; while the temperature is rising, the pressure is increased from 1-10MPa to 40-80MPa at a rate of 3-10MPa / min and then kept constant until the sintering is completed.

8. The method for preparing the synergistically reinforced fine-grained high-temperature molybdenum-copper based composite material according to claim 4, It is characterized in that In step S3, during sintering, the temperature is first raised from room temperature to 180-220°C at a rate of 2-30°C / s and kept for 2-15 minutes, then raised to 600-700°C at a rate of 2-150°C / s and kept for 5-10 minutes, and finally raised to 800-1100°C at a rate of 5-150°C / s and kept for 5-20 minutes.