A method for preparing a skin-like stretchable electronic system

By preparing rigid island and flexible base materials with different ratios, and using gallium indium alloy/N, N-dimethylformamide ink to enhance the combination of liquid metal and flexible base, we solved the problem of skin-like stretchable electronic systems. It achieves high stretch rate and conductive stability by overcoming the problems of differential modulus ratio and insufficient interface stability.

CN118412176BActive Publication Date: 2024-10-25NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410875318.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-25
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The difference in Young's modulus ratio and interface stability between the rigid island and the flexible substrate in existing skin-like stretchable electronic systems are insufficient, making it difficult for liquid metal to diffuse to the surface of the flexible substrate and deform synchronously with it.

Method used

By preparing precursor liquids of rigid islands and flexible base materials with different ratios of the same raw materials, using photocuring to form a rigid island structure, and using ultrasonic treatment to prepare gallium indium alloy/N, N-dimethylformamide ink, which can be printed on A stretchable conductor is formed on a rigid island structure substrate, and amino and hydroxyl groups are used to form hydrogen bonds with liquid metal to enhance the bonding force.

Benefits of technology

The combination of rigid island and flexible substrate with high Young's modulus ratio difference is achieved, which enhances the mechanical strength of the interface, improves the stretch rate and conductive stability of the stretchable electronic system, and the resistance only increases by 1 times at 600% strain. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118412176B_ABST
    Figure CN118412176B_ABST
Patent Text Reader

Abstract

The present invention relates to a preparation method of a skin-like stretchable electronic system. The method creates a rigid island and a flexible substrate with a large difference in Young's modulus ratio by using different ratios of the same material, effectively protects the functional devices and active substances above the rigid island, solidifies the rigid island on the flexible substrate, and makes a carbon-carbon double bond exist at the interface between the two, which greatly enhances the mechanical strength at the interface; by configuring gallium-indium alloy / N,N-dimethylformamide ink, the ink can expose amino groups and hydroxyl groups on the surface of the substrate when in contact with the substrate, and can form a stable hydrogen bond connection with the oxide shell of the liquid metal, thereby enhancing the bonding force and creating conditions for the interconnection of multi-module integrated devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of component manufacturing of electrical components, and in particular to a method for preparing a skin-like stretchable electronic system. Background Art

[0002] Skin-like stretchable electronic systems that integrate seamlessly with the human body can achieve comfortable and large-scale physiological monitoring, real-time analysis of health status, local treatment, and reconstruction of motor function. Such stretchable electronic systems can become the mainstay in fields such as healthcare, environmental sensing, and human-computer interaction equipment.

[0003] In order to effectively protect the functional devices in this type of stretchable electronic system, it can be constructed into a rigid island structure, and the electronic functional devices can be placed on the corresponding rigid island, and the rigid island is interconnected with the stretchable conductor embedded in the elastic substrate, so that the functional devices are protected. However, the performance of stretchable electronic systems with this structure is constrained by the stiffness of rigid and flexible components and interface engineering. This constraint is reflected in that to achieve robust large-scale deformation capabilities, the rigid island and the flexible substrate must have a large difference in Young's modulus ratio and strong interface bonding force (i.e., stability). However, how to simultaneously enhance the difference in Young's modulus ratio between the rigid island and the flexible substrate and the interface stability between the two remains an existing technical problem.

[0004] In addition, in this type of stretchable electronic system, in order to achieve excellent electronic performance under large-scale deformation conditions, a highly conductive material that is insensitive to strain is required as a stretchable conductor to achieve interconnection of related devices. Although liquid metals (LM) such as gallium-indium alloys (EGaIn) have high conductivity and stretchability and are ideal candidate materials for stretchable conductors. However, the surface energy of LM droplets is high and their affinity with the substrate surface is poor. Therefore, it is still very difficult to diffuse LM onto the surface of a flexible substrate and make LM deform together with the flexible substrate when strain is applied. Summary of the invention

[0005] The technical problems to be solved by the present invention are:

[0006] First, how to simultaneously enhance the difference in Young's modulus ratio between the rigid island and the flexible substrate and the interface stability between the two in skin-like stretchable electronic systems;

[0007] Second, how to make liquid metal diffuse to the surface of flexible substrate in skin-like stretchable electronic system and make the liquid metal produce large deformation synchronously with the flexible substrate and stably conduct.

[0008] In order to overcome the above defects of the prior art, the present invention provides a method for preparing a skin-like stretchable electronic system, which comprises the following steps:

[0009] S1: preparing a rigid island precursor solution and a flexible substrate material precursor solution with the same raw materials but different ratios;

[0010] S2: curing the flexible substrate material precursor liquid by photocuring to obtain a flexible substrate, injecting the rigid island precursor liquid into a preset position on the flexible substrate and curing it by ultraviolet light to obtain a rigid island structure substrate;

[0011] S3: Gallium-indium alloy / N, N-dimethylformamide ink was prepared by ultrasonic treatment;

[0012] S4: printing the ink obtained in step S3 into an area outside the preset position on the rigid island structure substrate, and scraping the printed and dried ink droplets in the area with a glass rod to obtain a stretchable conductor;

[0013] S5: Based on the stretchable conductor, a predetermined circuit structure is set at the preset location to obtain a skin-like stretchable electronic system, and the skin-like stretchable electronic system is packaged.

[0014] In response to the first technical problem, the preparation method of the skin-like stretchable electronic system of the present invention, after obtaining the rigid island precursor liquid and the flexible substrate material precursor liquid respectively, solidifies the flexible substrate material precursor liquid to obtain a flexible substrate, and then injects the rigid island precursor liquid into the preset position on the flexible substrate and solidifies it, and a rigid island structure is formed at the predetermined position. Furthermore, by using different ratios of the same material, two parts with a large difference in Young's modulus ratio (7880) are created - a rigid island and a flexible substrate. The rigid island is formed at a predetermined position in the flexible matrix, and the Young's modulus of the two differs by nearly four orders of magnitude, which means that the rigid area will not deform under large stretching, effectively protecting the functional devices and active substances above it. At the same time, after the rigid island is solidified in the predetermined area of ​​the flexible substrate, there is a carbon-carbon double bond at the interface between the two. Under the ultraviolet light during curing, it polymerizes into a long molecular chain that shuttles between the rigid island and the flexible substrate. This will greatly enhance the mechanical strength at the interface, allowing the stretchable electronic system to have a high stretchability of 560% and maintain stable performance during up to 1,000 cycles, providing a feasible and high-performance material type for the production of rigid island structure substrates.

[0015] In addition, in order to solve the problem of the difficulty in diffusing liquid metal, the preparation method of the skin-like stretchable electronic system of the present invention configures gallium-indium alloy / N, N-dimethylformamide ink through step S3. The ink can expose the amino and hydroxyl groups on the surface of the substrate when in contact with the substrate. These groups can form stable hydrogen bonds with the oxide shell of the liquid metal (gallium-indium alloy), thereby enhancing the bonding force between the two. This interconnection line exhibits high conductivity and resistance stability under stretching conditions, and its resistance only increases by 1 times at 600% strain, thereby creating conditions for the interconnection of multi-module integrated devices.

[0016] In a possible implementation, step S1 includes the following steps:

[0017] S11: adding isobornyl acrylate, benzyl acrylate, and polyurethane acrylate into a beaker in a first mass ratio, and then adding diphenylphosphine oxide as a photoinitiator to obtain a first mixture;

[0018] S12: using a mechanical stirrer to stir the first mixture for 6-8 hours to obtain a transparent and uniform solution, which is the rigid island precursor solution;

[0019] S13: adding isobornyl acrylate, benzyl acrylate and polyurethane acrylate into another beaker in a second mass ratio, wherein the second mass ratio is different from the first mass ratio, and then adding diphenylphosphine oxide as a photoinitiator to obtain a second mixture;

[0020] S14: using a mechanical stirrer to stir the second mixture for 6-8 hours to obtain a transparent and uniform solution, which is the flexible substrate material precursor solution;

[0021] Compared with the existing technology, the above technical scheme can ensure the formation of a rigid island and a flexible substrate with a large difference in Young's modulus ratio while preparing the precursor solutions of the rigid island and the flexible substrate materials respectively, and further ensure that after the rigid island is solidified in the predetermined area of ​​the flexible substrate in the later stage, there are carbon-carbon double bonds at the interface between the rigid island and the flexible substrate to meet the stability requirements.

[0022] In a possible implementation, the mass ratio of isobornyl acrylate, benzyl acrylate, and polyurethane acrylate in step S11 is 5:2:3; the mass ratio of isobornyl acrylate, benzyl acrylate, and polyurethane acrylate in step S13 is 2:5:3;

[0023] Thereby achieving the goal of using different ratios of the same material to manufacture two parts (rigid island and flexible substrate) with huge differences in Young's modulus, so that there can be a strong bonding force between the two and they are not easily damaged under large strains.

[0024] In a possible implementation manner, step S2 includes the following steps:

[0025] S21: curing the flexible substrate material precursor liquid into a shape by digital photocuring printing, and then drying it in an oven to obtain the flexible substrate;

[0026] S22: injecting the rigid island precursor liquid into a preset position on the flexible substrate, curing the rigid island precursor liquid by ultraviolet light to form a rigid island area on the flexible substrate, thereby obtaining the rigid island structure substrate;

[0027] In this way, a rigid island is formed on the flexible substrate, and there is a carbon-carbon double bond at the interface between the two. By using ultraviolet light curing, it is polymerized into a long molecular chain that shuttles between the rigid island and the flexible substrate, greatly enhancing the mechanical strength at the interface.

[0028] In a possible implementation manner, after executing step S21 and before executing step S22, the following steps need to be performed:

[0029] Cleaning the flexible substrate with anhydrous ethanol having a purity greater than 99.7%;

[0030] The cleanliness of the flexible substrate is thereby ensured, and the rigid island structure is formed after the rigid island precursor liquid is injected onto the flexible substrate, thereby enhancing the stability of the interface between the rigid island and the flexible substrate.

[0031] In a possible implementation manner, step S3 includes the following steps:

[0032] S31: placing the gallium-indium alloy into N, N-dimethylformamide to obtain a third mixture;

[0033] S32: ultrasonically treating the third mixture by a dot ultrasonic machine until the gallium-indium alloy is uniformly and stably dispersed in the third mixture, thereby obtaining the gallium-indium alloy / N, N-dimethylformamide ink;

[0034] Furthermore, gallium-indium alloy / N, N-dimethylformamide ink can be obtained, providing a guarantee for solving the problem of liquid metal being difficult to pattern.

[0035] In a possible implementation, the maximum power of the ultrasonic machine used in step S32 is 75%, and the ultrasonic time is 10 min. This solution can ensure that the gallium-indium alloy and N, N-dimethylformamide are fully mixed and uniformly formed into a uniform ink.

[0036] In a possible implementation manner, step S4 includes the following steps:

[0037] S41: moving the ink obtained in step S32 to a mortar for grinding to obtain ground ink;

[0038] S42: Printing the ground ink onto the area outside the rigid island area on the rigid island structure substrate by using an extrusion-type three-dimensional printer, and drying it in an oven;

[0039] S43: scraping the ink droplets dried in step S42 on the rigid island structure substrate with a glass rod to obtain the stretchable conductor;

[0040] This scheme enables the ink to be printed onto a flexible substrate and dried, and by using a glass rod to scratch the dried ink on the substrate, the oxide shell of the liquid metal (gallium indium alloy) droplet can be broken to become a stretchable conductor.

[0041] In a possible implementation, during the drying in step S42, the oven drying temperature is 60° C. and the drying time is more than 6 hours. This solution can fully volatilize the N, N-dimethylformamide, leaving only the conductive gallium-indium alloy as a stretchable conductor.

[0042] In a possible implementation manner, step S5 includes the following steps:

[0043] S51: fixing all functional devices involved in the predetermined circuit structure on the rigid island area, and printing gallium-indium alloy on the stretchable conductor to connect all the functional devices according to the predetermined circuit structure;

[0044] S52: Reinforcing the connection contacts between the gallium-indium alloy and each of the functional devices by silver paste respectively, obtaining the skin-like stretchable electronic system, and then encapsulating it;

[0045] This solution can achieve the purpose of forming interconnecting wires connecting all functional electronic components with gallium-indium alloy, ensuring circuit connectivity, and thus ensuring normal and efficient operation of the circuit. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is a flow chart of a method for preparing a skin-like stretchable electronic system according to an embodiment of the present invention;

[0047] Figure 2 This is a flow chart of step S1 of an embodiment of the present invention;

[0048] Figure 3 This is a flow chart of step S2 of an embodiment of the present invention;

[0049] Figure 4 This is a flow chart of step S3 of an embodiment of the present invention;

[0050] Figure 5 This is a flow chart of step S4 of an embodiment of the present invention;

[0051] Figure 6 This is a flow chart of step S5 of an embodiment of the present invention;

[0052] Figure 7 The stress-strain curves and Young's modulus images of the rigid island and the flexible substrate according to the embodiment of the present invention;

[0053] Figure 8 Comparison of stress-strain curves of the rigid island structure substrate of the embodiment of the present invention and two existing rigid island structure substrates;

[0054] Fig. 9 The stress-strain curve of the rigid island structure substrate of the embodiment of the present invention after being stretched 200% and cycled for 1000 times;

[0055] Fig.10 Schematic diagram of comparison of contact angles of a liquid metal droplet and a liquid metal ink on a flexible substrate before and after treatment with N, N-dimethylformamide according to an embodiment of the present invention;

[0056] Fig.11 The SEM image and EDS image of the liquid metal ink on the flexible substrate according to the embodiment of the present invention;

[0057] Fig.12 A graph showing the tensile conductivity of liquid metal ink on a flexible substrate according to an embodiment of the present invention;

[0058] Fig.13 A circuit diagram of a solar cell / micro supercapacitor / LED display / wireless coil multi-module integrated device according to an embodiment of the present invention;

[0059] Fig.14 These are curve graphs and physical pictures of the light charging function, wireless charging function, and display function of the solar cell / micro supercapacitor / LED display / wireless coil multi-module integrated device according to an embodiment of the present invention. DETAILED DESCRIPTION

[0060] First, those skilled in the art should understand that these implementations are only used to explain the technical principles of the embodiments of the present application, and are not intended to limit the protection scope of the embodiments of the present application. Those skilled in the art can make adjustments to them as needed to adapt to specific application scenarios.

[0061] In the embodiments of the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0062] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0063] See also Figure 1 to Figure 14 As shown, the present invention discloses a method for preparing a skin-like stretchable electronic system, see Figure 1 As shown, the method comprises the following steps:

[0064] S1: Prepare a rigid island material precursor solution and a flexible substrate material precursor solution with the same raw materials but different ratios respectively.

[0065] See also Figure 2 As shown, in this embodiment, step S1 includes the following steps:

[0066] S11: Add isobornyl acrylate, benzyl acrylate, and polyurethane acrylate into a beaker at a first mass ratio, and then add 1% by mass of diphenylphosphine oxide as a photoinitiator to obtain a first mixture. The first ratio is:

[0067] The mass of isobornyl acrylate: the mass of benzyl acrylate: the mass of polyurethane acrylate = 5: 2: 3.

[0068] S12: Use a mechanical stirrer to stir the first mixture for 6-8 hours to obtain a transparent and uniform solution, which is the rigid island precursor solution.

[0069] S13: Add isobornyl acrylate, benzyl acrylate and polyurethane acrylate in a second mass ratio to another beaker, and then add 1% by mass of diphenylphosphine oxide as a photoinitiator to obtain a second mixture. The second ratio is:

[0070] The mass of isobornyl acrylate: the mass of benzyl acrylate: the mass of polyurethane acrylate = 2: 5: 3.

[0071] S14: using a mechanical stirrer to stir the second mixture for 6-8 hours to obtain a transparent and uniform solution, which is the precursor solution of the flexible substrate material.

[0072] In short, step S1 of this embodiment is intended to prepare the precursor solution of rigid island and flexible substrate materials. In the specific process, isobornyl acrylate, benzyl acrylate, and polyurethane acrylate are added to a beaker in a certain proportion, and then 1% by mass of diphenyl (2, 4, 6-trimethylbenzoyl) phosphine oxide (TPO for short) is added as a photoinitiator, and the mixture is stirred for 6-8 hours using a mechanical stirrer to obtain a transparent and uniform solution, which is the rigid island precursor solution. As for the raw materials and preparation process of the precursor solution of the flexible substrate material, they are the same as those of the rigid island precursor solution, except that the proportions of isobornyl acrylate, benzyl acrylate, and polyurethane acrylate are different.

[0073] S2: Curing the precursor liquid of the flexible substrate material by photocuring to obtain a flexible substrate, injecting a rigid island precursor liquid into a preset position on the flexible substrate and curing it by ultraviolet light to obtain a rigid island structure substrate.

[0074] See also Figure 3 As shown, in this embodiment, step S2 includes the following steps:

[0075] S21: The flexible substrate material precursor liquid is solidified into a shape by digital photocuring printing, and then dried in an oven to obtain a flexible substrate.

[0076] S22: Clean the flexible substrate with anhydrous ethanol having a purity greater than 99.7%.

[0077] S23: Injecting a rigid island precursor liquid into a preset area on the flexible substrate, and curing the rigid island precursor liquid by a 365 nm ultraviolet lamp to form a rigid island area on the flexible substrate, thereby obtaining a rigid island structure substrate.

[0078] Step S2 is actually the production of a rigid island structure substrate. The production of a flexible substrate uses digital photocuring printing (DLP) to solidify the flexible substrate material precursor liquid into shape, and then dry it in an oven and clean it. Subsequently, a rigid island precursor liquid is injected into the preset position on the flexible substrate, and a 365 nm ultraviolet lamp is used to solidify it to form a rigid island area. At this point, the preset position becomes a rigid island area, and the non-preset position on the flexible substrate is a flexible area in comparison. Thus, a rigid island structure substrate that is locally rigid and overall stretchable is prepared.

[0079] Figure 7 The stress-strain curves and Young's modulus images of the rigid island and the flexible substrate of this embodiment are shown in FIG. Figure 7As shown, the Young's modulus of the flexible substrate of this embodiment is 0.01 MPa, while the Young's modulus of the rigid island is 78.8 MPa. The ratio of the Young's moduli of the two reaches more than 7880, which means that when the flexible substrate is stretched to produce strain, the rigid island will only produce 1 / 7880 of the strain, which will effectively protect the devices in the rigid island area from being affected by the overall strain, thereby achieving the purpose of strain isolation.

[0080] Figure 8 The maximum strains that the heterogeneous rigid island structure substrate (referred to as heterogeneous PET and Ecoflex rigid island structure substrate in the figure) and the homogeneous rigid island structure substrate (referred to as homogeneous PDMS rigid island structure substrate in the figure) of the prior art combined by polyethylene terephthalate (referred to as PET) and Ecoflex materials before breaking are 310% and 80%, respectively. In contrast, the homogeneous rigid island structure substrate (referred to as homogeneous IBA rigid island structure substrate in the figure) combined by isobornyl acrylate, benzyl acrylate, and polyurethane acrylate (referred to as IBA) in this embodiment will not break until the applied strain reaches 560%, thereby showing excellent mechanical properties.

[0081] The rigid island structure substrate obtained in this embodiment also has excellent fatigue resistance. Fig. 9 The stress-strain curve of the rigid island structure substrate of this embodiment is shown in FIG. Fig. 9 As shown in the figure, in the 1000-cycle test at 200% strain, the rigid island structure substrate showed neither interface damage nor significant change in Young's modulus. It can be seen that the rigid island structure substrate can effectively inhibit the propagation of cracks.

[0082] S3: Gallium-indium alloy / N, N-dimethylformamide ink was prepared by ultrasonic treatment.

[0083] See also Figure 4 As shown, in this embodiment, step S3 includes the following steps:

[0084] S31: Put 2 g of gallium-indium alloy into 3 ml of N, N-dimethylformamide to obtain a third mixture.

[0085] S32: ultrasonically treating the third mixture by a dot ultrasonic machine until the gallium-indium alloy is uniformly and stably dispersed in the third mixture, thereby obtaining a gallium-indium alloy / N, N-dimethylformamide ink. The maximum power of the dot ultrasonic machine used is 75%, the ultrasonic time is 10 min, and the model is JY92-IIN.

[0086] Step S3 is the preparation of gallium-indium alloy / N, N-dimethylformamide ink. First, 2 g of gallium-indium alloy is placed in 3 ml of N, N-dimethylformamide, and then the mixture is ultrasonicated using a point ultrasonicator until the gallium-indium alloy is uniformly and stably dispersed in the solution, thereby obtaining ink.

[0087] S4: Print the ink obtained in step S3 into an area outside the preset position on the rigid island structure substrate, that is, a flexible area on the rigid island structure substrate, and use a glass rod to scrape the printed and dried ink droplets in the area to obtain a stretchable conductor.

[0088] See also Figure 5 As shown, in this embodiment, step S4 includes the following steps:

[0089] S41: The ink obtained in step S32 is transferred to a mortar and ground for 30 minutes to obtain ground ink.

[0090] S42: Print the ground ink onto the area outside the rigid island area on the rigid island structure substrate, that is, the flexible area on the rigid island structure substrate, through an extrusion-type three-dimensional printer, and dry it in an oven. During the drying process, the oven drying temperature is 60° C., and the drying time is more than 6 hours.

[0091] S43: Scrape the ink droplet dried in step S42 on the rigid island structure substrate with a glass rod to obtain a stretchable conductor.

[0092] Step S4 is actually to print the gallium-indium alloy / N, N-dimethylformamide ink onto the flexible area on the rigid island structure substrate to obtain a stretchable conductor. First, the ink is transferred to a mortar and ground for 30 minutes to increase the viscosity of the ink. Then, the ink is printed onto the flexible area using an extrusion-type stereo printer and dried in an oven. Finally, a glass rod is used to scrape the dried ink droplets on the flexible area to break the oxide shell of the gallium-indium alloy to form a stretchable conductor.

[0093] Fig.10 The figure shows the contact angle comparison of gallium-indium alloy droplets and gallium-indium alloy ink on flexible substrates before and after N, N-dimethylformamide treatment. From left to right, they are the contact angle of gallium-indium alloy droplets on flexible substrates that have not been treated with N, N-dimethylformamide, the contact angle of gallium-indium alloy droplets on flexible substrates that have been treated with N, N-dimethylformamide, and the contact angle of gallium-indium alloy / N, N-dimethylformamide ink droplets of this embodiment on flexible substrates. Fig.10As shown, the contact angle of the gallium-indium alloy droplet on the untreated flexible substrate is 128.47°, showing the characteristics of poor wettability, while the contact angle of the gallium-indium alloy droplet on the flexible substrate treated with N, N-dimethylformamide is 82.93°, and its wettability is significantly improved. When the gallium-indium alloy / N, N-dimethylformamide ink droplet of this embodiment is dropped on the flexible substrate, the contact angle is only 47.03°, which further strongly proves the improvement of the affinity between the gallium-indium alloy and the flexible substrate induced by the interfacial hydrogen bond, which can ensure that the gallium-indium alloy and the flexible substrate are deformed together during stretching, thereby ensuring the stability of the resistance.

[0094] Fig.11 The SEM image (left) and EDS image (right) of the gallium-indium alloy ink on a flexible substrate are shown. Fig.11 It can be seen that although Ga, In, C, and O elements all penetrate into the interface between the gallium-indium alloy and the flexible substrate, no obvious interface boundary is observed, which further reveals the close interface bonding between the gallium-indium alloy / N, N-dimethylformamide ink of this embodiment and the flexible substrate.

[0095] Fig.12 The graph of the stretched conductivity of gallium-indium alloy ink on a flexible substrate is shown. Fig.12 As shown, the resistance of the gallium indium alloy (abbreviated as EGaIn in the figure) on the flexible substrate increases five times when the strain is 500%, while the resistance of the gallium indium alloy on the substrate treated with N, N-dimethylformamide (abbreviated as DMF in the figure) increases four times when the strain is 600%. In contrast, the resistance of the gallium indium alloy / N, N-dimethylformamide ink (abbreviated as EGaIn / DMF in the figure) printed on the flexible substrate (manufactured in this embodiment) only increases by 1 time when the strain is 600%, thereby showing a more excellent conductive stability during the stretching process.

[0096] S5: Based on the stretchable conductor, a predetermined circuit structure is arranged on the rigid island area to obtain a skin-like stretchable electronic system, and the skin-like stretchable electronic system is packaged.

[0097] See also Figure 6 As shown, in this embodiment, step S5 includes the following steps:

[0098] S51: Fix all functional devices involved in the predetermined circuit structure on the rigid island area, and print gallium-indium alloy on the stretchable conductor to connect all functional devices according to the predetermined circuit structure.

[0099] S52: The connecting contacts between the gallium-indium alloy and each functional device are reinforced with silver paste respectively to obtain a skin-like stretchable electronic system, which is then packaged. The material used for packaging the skin-like stretchable electronic system is a flexible substrate material precursor liquid, which can be obtained through steps S13 and S14.

[0100] Step S5 is actually to set the circuit structure on the rigid island region of the stretchable conductor obtained in step S4. As a specific example, this embodiment takes the energy device circuit as an example. Fig.13 The circuit diagram of the electronic system of solar cell / micro supercapacitor / LED display / wireless coil prepared in this specific example is shown. On the left side are three solar cells connected in series; on the left side in the middle are three groups of supercapacitor arrays connected in parallel, each group of supercapacitor arrays is composed of three microcapacitors connected in series; on the right side in the middle is an array of 19 LED bulbs connected in parallel; on the far right is the wireless charging coil. Fig.14 The actual pictures of the electronic system performing solar charging, wireless charging and lighting up the LED, as well as the voltage and current changes, can prove that the various modules of the electronic system can function normally, and can effectively collect and utilize energy from short UV-visible light waves to long radio waves, demonstrating the potential of electronic skin with energy autonomy and long-term continuous operation.

[0101] The preparation method of the skin-like stretchable electronic system disclosed in this embodiment develops a rigid island structure substrate with a high modulus ratio and high stretch rate, wherein the rigid island area and the flexible area not only have a large modulus ratio difference, but also have a strong mechanical strength at the interface of the two parts. The rigid island structure substrate produced has a stretch rate of up to 560%, and maintains stable performance during a cycle of up to 1000 times, providing a feasible and high-performance material type for the production of rigid island structures. At the same time, it also solves the problem that liquid metal is difficult to pattern. By configuring gallium indium alloy / N, N-dimethylformamide ink, the ink can expose the amino and hydroxyl groups on the surface of the substrate when in contact with the substrate. These groups will form stable hydrogen bonds with the oxide shell of the liquid metal, enhancing the binding force between the two.

[0102] In the description of the embodiments of the present application, it should be noted that in the description of the present application, terms such as "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is only for the convenience of description, and does not indicate or imply that the device or component must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present application.

[0103] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0104] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. A method for preparing a skin-like stretchable electronic system, It is characterized in that The steps include: S1: preparing a rigid island precursor solution and a flexible substrate material precursor solution with the same raw materials but different ratios; S2: curing the flexible substrate material precursor liquid by photocuring to obtain a flexible substrate, injecting the rigid island precursor liquid into a preset position on the flexible substrate and curing it by ultraviolet light to obtain a rigid island structure substrate; S3: Gallium-indium alloy / N, N-dimethylformamide ink was prepared by ultrasonic treatment; S4: printing the ink obtained in step S3 into an area outside the preset position on the rigid island structure substrate, and scraping the printed and dried ink droplets in the area with a glass rod to obtain a stretchable conductor; S5: Based on the stretchable conductor, a predetermined circuit structure is arranged at the preset location to obtain a skin-like stretchable electronic system, and the skin-like stretchable electronic system is packaged; The step S1 comprises the following steps: S11: adding isobornyl acrylate, benzyl acrylate, and polyurethane acrylate into a beaker in a first mass ratio, and then adding diphenylphosphine oxide as a photoinitiator to obtain a first mixture; S12: using a mechanical stirrer to stir the first mixture for 6-8 hours to obtain a transparent and uniform solution, which is the rigid island precursor solution; S13: adding isobornyl acrylate, benzyl acrylate, and polyurethane acrylate into another beaker in a second mass ratio, where the second mass ratio is different from the first mass ratio, and then adding 1% of the total mass of diphenylphosphine oxide as a photoinitiator to obtain a second mixture; S14: using a mechanical stirrer to stir the second mixture for 6-8 hours to obtain a transparent and uniform solution, which is the flexible substrate material precursor solution; The mass ratio of isobornyl acrylate, benzyl acrylate and polyurethane acrylate in step S11 is 5:2:3; the mass ratio of isobornyl acrylate, benzyl acrylate and polyurethane acrylate in step S13 is 2:5:

3.

2. The method for preparing a skin-like stretchable electronic system according to claim 1, It is characterized in that The step S2 comprises the following steps: S21: curing the flexible substrate material precursor liquid into a shape by digital photocuring printing, and then drying it in an oven to obtain the flexible substrate; S22: injecting the rigid island precursor liquid into a preset position on the flexible substrate, curing the rigid island precursor liquid by ultraviolet light to form a rigid island area on the flexible substrate, thereby obtaining the rigid island structure substrate.

3. The method for preparing a skin-like stretchable electronic system according to claim 2, It is characterized in that After executing step S21 and before executing step S22, the following steps need to be performed: The flexible substrate is cleaned with anhydrous ethanol having a purity greater than 99.7%.

4. The method for preparing a skin-like stretchable electronic system according to claim 3, It is characterized in that The step S3 comprises the following steps: S31: placing the gallium-indium alloy into N, N-dimethylformamide to obtain a third mixture; S32: ultrasonically treating the third mixture by a dot ultrasonic machine until the gallium-indium alloy is uniformly and stably dispersed in the third mixture, thereby obtaining the gallium-indium alloy / N, N-dimethylformamide ink.

5. The method for preparing a skin-like stretchable electronic system according to claim 4, It is characterized in that The maximum power of the ultrasound machine used in step S32 is 75%, and the ultrasound time is 10 min.

6. The method for preparing a skin-like stretchable electronic system according to claim 5, It is characterized in that The step S4 comprises the following steps: S41: moving the ink obtained in step S32 to a mortar for grinding to obtain ground ink; S42: Printing the ground ink onto the area outside the rigid island area on the rigid island structure substrate by using an extrusion-type three-dimensional printer, and drying it in an oven; S43: Scratching the ink droplets dried in step S42 on the rigid island structure substrate with a glass rod to obtain the stretchable conductor.

7. The method for preparing a skin-like stretchable electronic system according to claim 6, It is characterized in that When drying is performed in step S42, the oven drying temperature is 60° C. and the drying time is more than 6 hours.

8. The method for preparing a skin-like stretchable electronic system according to claim 7, It is characterized in that The step S5 comprises the following steps: S51: fixing all functional devices involved in the predetermined circuit structure on the rigid island area, and printing gallium-indium alloy on the stretchable conductor to connect all the functional devices according to the predetermined circuit structure; S52: Reinforcing the connection contacts between the gallium-indium alloy and each of the functional devices by silver paste respectively to obtain the skin-like stretchable electronic system, and then encapsulating it.