A radar / infrared compatible stealth composite aerogel and its preparation method
By loading cobalt nanoparticles onto three-dimensional porous chitosan aerogel, the problems of single loss mechanism and poor impedance matching in existing radar/infrared compatible stealth composite aerogels are solved, achieving high-efficiency radar/infrared compatible stealth performance and reducing thermal conductivity, making it suitable for mass production.
Patent Information
- Application Number
- CN202410636829.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-05-22
AI Technical Summary
Existing radar/infrared compatible stealth composite aerogels suffer from a single loss mechanism, poor impedance matching, insufficient reflection loss, narrow absorption frequency band, and poor adaptability to service environments, making it difficult to achieve radar/infrared compatible stealth.
Using three-dimensional porous chitosan aerogel as a carbon-based framework, cobalt salt-derived cobalt nanoparticles are loaded and carbonized at high temperature after directional freezing and freeze-drying to form a composite aerogel with high porosity and high graphitization.
It improves radar and infrared stealth performance, achieving radar/infrared compatible stealth of the material. Moreover, the preparation method is simple and low-cost, making it suitable for mass production.
Smart Images

Figure CN118416797B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a radar-infrared compatible stealth composite aerogel, and also to a method for preparing the aforementioned composite aerogel. Background Technology
[0002] Carbon-based aerogels possess excellent dielectric loss capability, extremely high specific surface area, lightweight three-dimensional network structure, strong chemical stability, and high designability, making them promising candidates for radar / infrared compatible stealth applications and gradually becoming an important research target for both academia and industry. For example, Wang et al. constructed a heterostructured nickel / MnO-carbon aerogel using ice templates and in-situ growth methods, which exhibits dual functions of radar stealth (strongest reflection loss: -64.09dB, effective absorption bandwidth: 7.36GHz) and infrared stealth (infrared emissivity value: 0.8744) (Wang, SJ; Zhang, X.; Hao, SY; Qiao, J.; Wang, Z.; Wu, LL; Liu, JR; Wang, FL; Nitrogen-doped magnetic-dielectric-carbon aerogel for high-efficiency electromagnetic waveabsorption, Nano-Micro Lett. 16 (2024) 16). Recent studies have found that chitosan, prepared by deacetylation of naturally abundant chitin, serves as the carbon-based framework for aerogels. This not only extends the effective path for electromagnetic wave transmission loss and expands the multiple scattering space, but also exhibits good chemical stability and recyclability, thus contributing to radar stealth. Furthermore, the abundant porosity and low density of the aerogel are crucial for reducing the thermal conductivity of the composite, effectively lowering the surface temperature conduction rate in practical applications. This makes aerogels a promising candidate for radar stealth applications.
[0003] The problems with existing radar / infrared compatible stealth composite aerogels are: (1) the loss mechanism of single-structure aerogel materials is simple and the impedance matching is poor; (2) the reflection loss is insufficient, the absorption frequency band is narrow and the service environment is poor; (3) the radar / infrared compatible stealth mechanism is contradictory and it is difficult to achieve compatible stealth in the same material. Summary of the Invention
[0004] Objective of the invention: The present invention aims to provide a radar / infrared compatible stealth composite aerogel, which has good radar / infrared compatible stealth performance; another objective of the present invention is to provide a method for preparing the above-mentioned composite aerogel.
[0005] Technical solution: The radar / infrared compatible stealth composite aerogel of the present invention uses three-dimensional porous chitosan aerogel as a carbon-based framework, and cobalt salt-derived cobalt nanoparticles are loaded on the carbon-based framework.
[0006] The size of the loaded cobalt nanoparticles is 400–500 nm.
[0007] The loading of cobalt nanoparticles is 10-15% of the mass of the composite aerogel.
[0008] The porosity of the three-dimensional porous carbon network structure is 85%–86%, its total pore volume is 5.8–8.5 mL / g, and its average pore size is 41–62 μm. The formation of cobalt nanoparticles reduces the porosity. In addition, due to the presence of metal, it acts as a catalyst for high-temperature carbonization, resulting in a higher degree of graphitization and a greater degree of shrinkage in the size of the three-dimensional porous network structure.
[0009] The preparation method of the above-mentioned composite aerogel includes the following steps:
[0010] (1) Chitosan and cobalt acetate tetrahydrate (Co(Ac)2·4H2O) were mixed and added to deionized water and stirred to obtain a mixed solution;
[0011] (2) Add glacial acetic acid to the mixed solution in step (1) and stir to obtain a high-viscosity transparent and clear solution;
[0012] (3) A high-viscosity transparent clear solution was placed on a semiconductor cooling chip and directionally frozen, and then freeze-dried in a freeze dryer to obtain a cobalt-containing chitosan aerogel.
[0013] (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, and an inert gas was passed through it. After calcination, a radar / infrared compatible stealth composite aerogel was obtained.
[0014] In step (1), the mass ratio of chitosan to cobalt acetate tetrahydrate is 1:1 to 1.5.
[0015] In step (1), the mass-to-volume ratio of chitosan to cobalt acetate tetrahydrate (solid) to deionized water is 1 to 1.25 g / 15 mL.
[0016] In step (1), the stirring time is 1 to 1.5 hours and the stirring rate is 800 to 850 r / min.
[0017] In step (2), the volume ratio of the mixed solution to glacial acetic acid is 51-52:1; the stirring time is 3-4 hours and the stirring rate is 800-850 r / min.
[0018] In step (3), the temperature of the semiconductor cooling chip is -50 to -60°C, and the directional freezing time is 3 to 3.5 hours; the freeze-drying time of the sample in the freeze dryer is 24 to 26 hours.
[0019] In step (4), the inert gas is argon, the heating rate is 2 to 2.5 °C / min, the high-temperature annealing temperature is 750 to 800 °C, and the carbonization time is 2 to 2.5 h.
[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant effects: (1) Compared with single carbon aerogel materials, the composite aerogel of the present invention uses three-dimensional porous chitosan aerogel as a carbon-based skeleton, and cobalt nanoparticles derived from cobalt salt are loaded on the carbon-based skeleton; the three-dimensional porous carbon-based network structure provides an effective transmission path and multiple scattering spaces for the absorption and dissipation of incident electromagnetic waves, strengthens the dielectric loss capability of electromagnetic waves in the composite aerogel, and helps to improve radar stealth performance; at the same time, the loading of magnetic cobalt nanoparticles on the three-dimensional porous network structure can improve the magnetic loss capability of the composite aerogel and optimize its impedance matching mechanism. The construction of heterogeneous structures can also enrich polarization loss behavior, further helping to achieve radar stealth of materials. (2) The network skeleton formed by directional freezing and subsequent freeze-drying processes has a high porosity structure, which can effectively reduce the thermal conductivity coefficient of the material, greatly reduce the heat radiation generated during electromagnetic wave loss, and help to achieve infrared stealth; therefore, the composite aerogel of the present invention exhibits excellent radar / infrared compatible stealth performance. (3) The preparation method of the present invention is simple and low in cost, does not require complex synthesis equipment, and is suitable for large-scale mass production. Attached Figure Description
[0021] Figure 1 SEM images of CC1 obtained in Example 1 and CC1.5 obtained in Example 2;
[0022] Figure 2 The X-ray diffraction patterns of CC1 prepared in Example 1 and CC1.5 prepared in Example 2 are shown.
[0023] Figure 3 Raman spectra of CC1 obtained in Example 1 and CC1.5 obtained in Example 2;
[0024] Figure 4 Hysteresis loop diagrams of CC1 obtained in Example 1 and CC1.5 obtained in Example 2;
[0025] Figure 5 Mercury intrusion porosimetry curves of CC1 obtained in Example 1 and CC1.5 obtained in Example 2;
[0026] Figure 6The reflection loss diagrams are for CC1 prepared in Example 1 and CC1.5 prepared in Example 2.
[0027] Figure 7 Infrared thermal images of CC1 obtained in Example 1 and CC1.5 obtained in Example 2. Detailed Implementation
[0028] Example 1
[0029] The method for preparing the composite aerogel of the present invention includes the following steps:
[0030] (1) Mix 1g of chitosan with 1g of cobalt acetate tetrahydrate Co(Ac)2·4H2O, add to 30mL of deionized water, and stir at 800r / min for 1h to obtain a mixed solution;
[0031] (2) Add 0.6 mL of glacial acetic acid to the homogeneous mixed solution in step (1) (the volume of the mixed solution is 31 mL), and continue to stir at 800 r / min for 3 h to obtain a high viscosity transparent clear solution;
[0032] (3) Place the high-viscosity transparent clear solution on a semiconductor cooling chip set at -50℃ and freeze it for 3 hours. Then freeze-dry it in a freeze dryer for 24 hours to obtain chitosan aerogel containing cobalt.
[0033] (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, argon gas was introduced, the heating rate was 2℃ / min, and it was kept at a high-temperature annealing temperature of 800℃ for 2h to obtain a radar / infrared compatible stealth composite aerogel, denoted as CC1.
[0034] Example 2
[0035] The method for preparing the composite aerogel of the present invention includes the following steps:
[0036] (1) Mix 1g of chitosan with 1.5g of cobalt acetate tetrahydrate Co(Ac)2·4H2O, add to 30mL of deionized water, and stir at 800r / min for 1h to obtain a mixed solution;
[0037] (2) Add 0.6 mL of glacial acetic acid to the homogeneous mixed solution in step (1) and continue stirring at 800 r / min for 3 h to obtain a high-viscosity transparent clear solution;
[0038] (3) Place the high-viscosity transparent clear solution on a semiconductor cooling chip set at -50℃ and freeze it for 3 hours. Then freeze-dry it in a freeze dryer for 24 hours to obtain chitosan aerogel containing cobalt.
[0039] (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, argon gas was introduced, the heating rate was 2℃ / min, and it was kept at a high-temperature annealing temperature of 800℃ for 2h to obtain a radar / infrared compatible stealth composite aerogel, denoted as CC1.5.
[0040] Comparative Example 1
[0041] A method for preparing a composite aerogel includes the following steps:
[0042] (1) Mix 1g of chitosan with 1g of cobalt chloride (CoCl2), add to 30mL of deionized water, and stir at 800r / min for 1h to obtain a mixed solution;
[0043] (2) Add 0.6 mL of hydrochloric acid to the homogeneous mixed solution in step (1) and continue stirring at 800 r / min for 3 h to obtain a high-viscosity transparent clear solution;
[0044] (3) Place the high-viscosity transparent clear solution on a semiconductor cooling chip set at -50℃ and freeze it for 3 hours. Then freeze-dry it in a freeze dryer for 24 hours to obtain chitosan aerogel containing cobalt.
[0045] (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, argon gas was introduced, the heating rate was 2℃ / min, and it was kept at a high-temperature annealing temperature of 800℃ for 2h to obtain a radar / infrared compatible stealth composite aerogel, denoted as CH1.
[0046] Comparative Example 2
[0047] A method for preparing a composite aerogel includes the following steps:
[0048] (1) Mix 1g of chitosan with 1g of nickel acetate tetrahydrate Ni(Ac)2·4H2O, add to 30mL of deionized water, and stir at 800r / min for 1h to obtain a mixed solution;
[0049] (2) Add 0.6 mL of glacial acetic acid to the homogeneous mixed solution in step (1) and continue stirring at 800 r / min for 3 h to obtain a high-viscosity transparent clear solution;
[0050] (3) Place the high-viscosity transparent clear solution on a semiconductor cooling chip set at -50℃ and freeze it for 3 hours. Then freeze-dry it in a freeze dryer for 24 hours to obtain chitosan aerogel containing cobalt.
[0051] (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, argon gas was introduced, the heating rate was 2℃ / min, and it was kept at a high-temperature annealing temperature of 800℃ for 2h to obtain a radar / infrared compatible stealth composite aerogel, denoted as CN1.
[0052] Figure 1 SEM images of CC1 obtained in Example 1 and CC1.5 obtained in Example 2, from... Figure 1 It can be seen that the product CC1 obtained in Example 1 and the product CC1.5 obtained in Example 2, which are obtained by freeze drying and high temperature carbonization, both have a three-dimensional porous carbon network structure and cobalt nanoparticles derived from cobalt salt are loaded on the carbon-based framework. The average size of the cobalt nanoparticles loaded on the surface of CC1 sample is 445 nm, and the average size of the cobalt nanoparticles loaded on the surface of CC1.5 is 460 nm.
[0053] Figure 2 The X-ray diffraction patterns of CC1 obtained in Example 1 and CC1.5 obtained in Example 2 are shown below. Figure 2 It can be seen that both samples have a relatively broad carbon diffraction peak at a 2Theta angle of 23.6°, representing the (002) crystal plane of graphitized carbon. Both samples also have characteristic cobalt diffraction peaks at 2Theta angles of 44.83°, 52.23° and 76.81°, representing the (111), (200) and (220) crystal planes of cobalt, respectively. This proves that the prepared material is a radar / infrared compatible stealth composite aerogel made of cobalt salt / chitosan.
[0054] Figure 3 The Raman spectra of CC1 obtained in Example 1 and CC1.5 obtained in Example 2 are shown below. Figure 3 It can be seen that the product CC1 obtained in Example 1 and the product CC1.5 obtained in Example 2 have different I values. D / I G The values are 1.01 and 0.95, respectively, indicating that the radar / infrared compatible stealth composite aerogel made of cobalt salt / chitosan has a high degree of graphitization after high-temperature annealing heat treatment. Due to the increase in cobalt salt content, CC1.5 has a higher degree of graphitization than CC1.
[0055] Figure 4 Hysteresis loop diagrams of CC1 obtained in Example 1 and CC1.5 obtained in Example 2 are shown below. Figure 4 It can be seen that the saturation magnetization of product CC1 obtained in Example 1 and product CC1.5 obtained in Example 2 are 43.7 emu / g and 51.0 emu / g, respectively. The higher saturation magnetization value leads to the higher magnetic permeability value.
[0056] Figure 5 The mercury intrusion porosimetry curves are for CC1 obtained in Example 1 and CC1.5 obtained in Example 2. Figure 5It can be seen that the porosity of the CC1 sample obtained in Example 1 is 86.94% and the total pore volume is 8.47 mL / g, while the porosity of the CC1.5 sample obtained in Example 2 is 85.46% and the total pore volume is 5.90 mL / g. This indicates that the radar / infrared compatible stealth composite aerogel prepared from cobalt salt / chitosan has high porosity and lightweight characteristics. Compared with the CC1.5 product, the CC1 product has higher porosity and larger total pore volume.
[0057] Figure 6 The reflection loss diagrams are for CC1 obtained in Example 1 and CC1.5 obtained in Example 2. Figure 6 As can be seen, the CC1 sample prepared in Example 1 exhibits good radar stealth performance. When the matching thickness is 1.20 mm (the CC1 content in the mixture of CC1 and paraffin is 25 wt%), it achieves the strongest reflection loss value of -44.70 dB, and when the matching thickness is 1.35 mm, it achieves the widest effective absorption bandwidth of 5.45 GHz. Compared to the CC1 product, the electromagnetic wave loss capability of the CC1.5 product is somewhat reduced. When the matching thickness is 1.80 mm, it achieves the strongest reflection loss value of -13.45 dB, and when the matching thickness is 1.35 mm, it achieves the widest effective absorption bandwidth of 4.00 GHz. In contrast, the CH1 sample prepared in Comparative Example 1 achieves the strongest reflection loss value of -27.3 dB when the matching thickness is 1.5 mm, and the widest effective absorption bandwidth of 2.81 GHz when the matching thickness is 1.65 mm. The CN1 prepared in Comparative Example 2 achieved the strongest reflection loss of -24.5 dB and the widest effective absorption bandwidth of 4.2 GHz at a matching thickness of 1.8 mm. In the above tests, the composite aerogel content in the mixture of composite aerogel and paraffin was 25 wt%.
[0058] Figure 7 Infrared thermal images of CC1 obtained in Example 1 and CC1.5 obtained in Example 2 are shown below. Figure 7 As can be seen, the products CC1 and CC1.5 prepared in Example 1 were placed on a heating platform with a set temperature of 70°C, and infrared thermal images of the samples were acquired after 1 minute. The detection temperature on the surface of CC1 was 25.8°C, and the detection temperature on the surface of CC1.5 was 26.3°C. The room temperature during the test was 23°C, indicating that both have good infrared stealth performance, demonstrating that the composite aerogel prepared in this invention can be applied in scenarios requiring infrared stealth. The detection temperature on the surface of CH1 prepared in Comparative Example 1 was 26.6°C, and the detection temperature on the surface of CN1 prepared in Comparative Example 2 was 27.1°C. Compared with CN1, CH1, and CC1.5, the surface temperature of CC1 increased at a slower rate, indicating that CC1, with its lower cobalt content, has better infrared stealth performance.
[0059] This invention relates to a radar / infrared compatible stealth composite aerogel prepared from cobalt salt / chitosan. First, chitosan and cobalt salt are mixed in deionized water. Then, acetic acid solution is used as a solvent to guide the self-aggregation and adsorption of chitosan macromolecules to form a viscous solution. Next, a cobalt salt-containing chitosan aerogel is prepared through directional freezing. Finally, the desired radar / infrared compatible stealth composite aerogel is obtained by carbonization in a high-temperature inert atmosphere. The radar / infrared compatible stealth composite aerogel prepared from cobalt salt / chitosan of this invention possesses a three-dimensional porous carbon-based network structure, with cobalt salt-derived cobalt nanoparticles loaded on this carbon-based framework. The three-dimensional porous carbon-based network structure extends the effective transmission path of electromagnetic waves and expands the multiple scattering space while endowing the material with sufficient dielectric loss capability. The loading of magnetic cobalt nanoparticles endows the composite aerogel with effective magnetic loss behavior and good impedance matching characteristics. The construction of the heterogeneous structure greatly enriches the polarization loss capability, thereby effectively improving its radar stealth performance. Meanwhile, the high porosity structure ensures extremely low thermal conductivity of the sample, effectively improving thermal insulation performance and thus reducing heat radiation, which helps to achieve infrared stealth.
Claims
1. The application of a composite aerogel in the preparation of radar / infrared compatible stealth materials, characterized in that: The composite aerogel uses a three-dimensional porous chitosan aerogel as a carbon-based framework, on which cobalt salt-derived cobalt nanoparticles are loaded. The size of the loaded cobalt nanoparticles is 400-500 nm. The loading amount of cobalt nanoparticles is 10-15% of the mass of the composite aerogel. The porosity of the three-dimensional porous carbon network structure is 85%-86%, the total pore volume is 5.8-8.5 mL / g, and the average pore size is 41-62 μm. The preparation method of the above-mentioned composite aerogel includes the following steps: (1) Mix chitosan with cobalt acetate tetrahydrate, add it to deionized water and stir to obtain a mixed solution; the mass ratio of chitosan to cobalt acetate tetrahydrate is 1:1~1.5; the mass-volume ratio of solid to deionized water is 1~1.25g / 15mL; (2) Add glacial acetic acid to the mixed solution in step (1) and stir to obtain a high-viscosity, transparent, and clear solution; (3) The high-viscosity transparent clear solution was placed on a semiconductor cooling chip and directionally frozen, and then freeze-dried in a freeze dryer to obtain a cobalt-containing chitosan aerogel; the temperature of the semiconductor cooling chip was -50~-60℃, and the directional freezing time was 3~3.5h; (4) The cobalt-containing chitosan aerogel was placed in a high-temperature tube furnace, and an inert gas was introduced. After calcination, a radar / infrared compatible stealth composite aerogel was obtained.
2. The application of the composite aerogel according to claim 1 in the preparation of radar / infrared compatible stealth materials, characterized in that: In step (1), the stirring time is 1~1.5h and the stirring rate is 800~850r / min.
3. The application of the composite aerogel according to claim 1 in the preparation of radar / infrared compatible stealth materials, characterized in that: In step (2), the volume ratio of the mixed solution to glacial acetic acid is 51~52:1; the stirring time is 3~4h and the stirring rate is 800~850r / min.
4. The application of the composite aerogel according to claim 1 in the preparation of radar / infrared compatible stealth materials, characterized in that: In step (3), the sample is placed in a freeze dryer and the freeze-drying time is 24~26h.
5. The application of the composite aerogel according to claim 1 in the preparation of radar / infrared compatible stealth materials, characterized in that: In step (4), the inert gas is argon, the heating rate is 2~2.5℃ / min, the high-temperature annealing temperature is 750~800℃, and the carbonization time is 2~2.5h.
Citation Information
Patent Citations
Composite aerogel material as well as preparation method and application thereof
CN116726816A