A carbon-reduced recycled aggregate based on alkali-activated strengthening and a preparation method thereof
By strengthening waste concrete aggregates with alkali activators and geopolymers to form a three-dimensional network gel, the problems of insufficient strength and carbon emissions of recycled aggregates in asphalt concrete are solved, realizing the preparation and application of efficient and environmentally friendly recycled aggregates.
Patent Information
- Application Number
- CN202410506594.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-25
AI Technical Summary
Existing recycled aggregates have insufficient compressive strength, low elastic modulus, low density, and surface porosity in asphalt concrete, resulting in insufficient strength and increased asphalt usage. Meanwhile, traditional silicate cement strengthening methods generate a large amount of carbon emissions and resource consumption.
Carbon-reducing recycled aggregates are prepared by mixing alkali activators and geopolymers with waste concrete aggregates through specific proportions and processes, including cleaning treatment, drying, geopolymer slurry preparation, asphalt warm mix agent mixing, and vacuum strengthening, forming a three-dimensional network gel to improve strength and density.
It improves the strength and density of recycled aggregates, meets the needs of road engineering, reduces carbon emissions and construction temperature, simplifies the processing procedures, and realizes resource recycling and environmental protection.
Smart Images

Figure CN118420257B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering, and particularly relates to a carbon-reduced recycled aggregate based on alkali-activated strengthening and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization and the continuous strengthening of infrastructure construction, a large amount of construction waste is also generated. These wastes not only occupy a large amount of land resources, but also cause serious pollution to the environment. In addition, the treatment of construction waste will also produce a large amount of carbon emissions. How to use these wastes in an environmentally friendly and efficient manner has become an important issue currently faced. Replacing natural aggregates with construction waste for road construction can achieve the purpose of turning waste into treasure and recycling resources. It can effectively protect natural resources, reduce the consumption of natural aggregates and energy, and effectively alleviate resource and environmental problems. As an environmentally friendly and economical building material, recycled aggregates have broad prospects for application.
[0003] However, after a large number of performance tests on asphalt concrete prepared from recycled aggregate, people found that the main difference between recycled aggregate and natural aggregate is that the former often contains a large amount of additional mortar and cracks caused by mechanical crushing, which leads to the following two major problems in the use of recycled aggregate: 1. The compressive strength of recycled aggregate is only 80-90% of that of ordinary natural aggregate, and the elastic modulus is also low, which will lead to insufficient strength in asphalt concrete; 2. The density of recycled aggregate is lower than that of natural aggregate, and there are a large number of pores on the surface, which will lead to an increase in the amount of asphalt in asphalt concrete; In order to solve the above problems, the existing solution is to use cement-based materials to strengthen construction waste so that its performance meets the requirements of road engineering aggregates.
[0004] However, traditional silicate cement produces a lot of carbon emissions during the production process. It is estimated that producing one ton of silicate cement will emit one ton of CO into the atmosphere. 2 At the same time, it consumes a large amount of non-renewable resources. The use of silicate cement to strengthen recycled aggregate not only has no economic advantage, but also damages the environment. Moreover, at present, waste concrete needs to be transported to professional equipment for crushing, screening, grading and other treatments before it can be used as recycled aggregate. The process is relatively complicated and not very convenient to use, which also limits the widespread application of recycled aggregate.
[0005] Therefore, the development of a green, environmentally friendly, economical and high-performance recycled aggregate and its preparation method has important practical significance for the development of the current construction industry. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a carbon-reduced recycled aggregate based on alkali-activated strengthening and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A carbon-reducing recycled aggregate based on alkali-activated strengthening comprises the following components and their corresponding mass proportions: 70% to 85% of waste concrete aggregate, 5% to 10% of alkali activator, 8% to 15% of geopolymer, and 2% to 5% of asphalt warm mix agent, wherein the proportions of the waste concrete aggregate, alkali activator, geopolymer and asphalt warm mix agent are all calculated by unit volume mass.
[0009] Preferably, the particle size of the waste concrete aggregate is 2 to 25 mm.
[0010] Preferably, the alkaline activator comprises solid water glass with a modulus of 1 to 2.5 and alkaline oxide, wherein the mass ratio of the solid water glass to the alkaline activator is 40% to 80%, and the mass ratio of the alkaline oxide to the alkaline activator is 20% to 60%.
[0011] Preferably, the alkaline oxide comprises any one or more mixtures of sodium hydroxide, potassium hydroxide or sodium carbonate.
[0012] Preferably, the geopolymer comprises any one or more mixtures of metakaolin, fly ash and blast furnace slag.
[0013] Preferably, the asphalt warm mix agent is a synthetic zeolite asphalt warm mix agent.
[0014] A method for preparing carbon-reduced recycled aggregate based on alkali-activated strengthening comprises the following steps:
[0015] S10, cleaning and processing: the waste concrete aggregates with a particle size of 2 to 25 mm after crushing and screening are washed and rinsed with clean water until the water is clear and free of sediment, thereby obtaining pre-treated waste concrete aggregates;
[0016] S20, drying: placing the pretreated waste concrete aggregate in an oven at a temperature of 110±5° C., and performing ventilation drying for 4 to 6 hours to obtain dried waste concrete aggregate;
[0017] S30, geopolymer slurry preparation: according to the preset alkali dosage, the required alkali activator and the mass of geopolymer are accurately calculated, and then the geopolymer raw material is dissolved in the activator solution and stirred to form the geopolymer slurry;
[0018] S40, mixing the asphalt warm mix agent: adding the asphalt warm mix agent to the geopolymer slurry, stirring evenly, so that the asphalt warm mix agent is evenly dispersed in the geopolymer slurry to obtain a mixed slurry;
[0019] S50, strengthening: mixing the mixed slurry prepared in step S40 with the waste concrete aggregate prepared in step S20 under vacuum conditions, so that the geopolymer and the asphalt warm mix agent are evenly coated on the surface of the waste concrete aggregate;
[0020] S60, molding and curing: take out the reinforced mixed waste concrete aggregate, filter out the mixed impurities, and place the mixed waste concrete aggregate in a standard curing room for curing to form carbon-reduced recycled aggregate.
[0021] Preferably, in step S10, the following steps are also included:
[0022] S101, screening aggregates: using a sieve with an aperture of 2 to 25 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing;
[0023] S102, aggregate washing: Pour the waste concrete aggregates with a particle size of 2 to 25 mm separated by the screen into a washing tank or a large container, fully soak them with clean water, and stir them with a stirring tool for 30 to 60 minutes to remove dirt on the surface of the waste concrete aggregates;
[0024] S103, aggregate washing: take out the waste concrete aggregate from the washing tank and wash it with clean water for 2 to 4 times to ensure that the surface of the waste concrete aggregate is clean and free of sand;
[0025] S104, Inspection and Drying: Spread the rinsed waste concrete aggregate in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregate is clean and free of impurities for subsequent steps.
[0026] Preferably, in step S20, the following steps are also included:
[0027] S201, prepare the oven: check the working status of the oven to ensure that it operates normally and the temperature is accurately controlled. Set the oven temperature to 110°C and set the temperature floating range to ±5°C to maintain a constant temperature environment;
[0028] S202, drying aggregate: take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 to 6 hours, turn on the oven ventilation device to ensure air circulation, and accelerate the drying process of the waste concrete aggregate;
[0029] S203, complete drying: during the drying process, regularly check the temperature in the oven and the state of the waste concrete aggregates. After reaching the set drying time, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregates out of the oven, and place them in a clean, dry container for subsequent steps.
[0030] Preferably, in step S30, the following steps are also included:
[0031] S301, alkali activator preparation: according to the preset alkali dosage (Na 2 O accounts for the percentage of the total mass of the cementitious material), and accurately calculate the mass of the required water glass and alkaline oxide; then gradually add the weighed solid water glass into an appropriate amount of water, stirring while adding, to ensure that the solid water glass is uniformly dissolved in the water, after the dissolution is completed, let it cool to room temperature, and perform an aging treatment for 18 to 30 hours; then gradually add the weighed alkaline oxide to the prepared water glass solution, stir until the alkaline oxide is completely dissolved, and ensure that the solution is uniform, after the dissolution is completed, let the activator solution cool to room temperature for use;
[0032] S302, geopolymer preparation: according to the preset alkali dosage (Na 2 O is measured as a percentage of the total mass of the cementitious material, the mass of the required geopolymer is accurately calculated, and one or more mixtures of metakaolin, fly ash, silica fume and blast furnace slag are selected as the geopolymer raw material according to the demand for alkali content;
[0033] S303, preparing geopolymer slurry: adding geopolymer into the alkaline activator solution in small amounts and multiple times. Each time the geopolymer is added, it needs to be fully stirred for 10 to 30 minutes to ensure that the geopolymer is completely dissolved in the alkaline activator to obtain a uniform geopolymer slurry for subsequent steps.
[0034] Preferably, in step S40, the following steps are also included:
[0035] S401, preliminary mixing: taking a certain amount of geopolymer slurry and putting it into a mixing container, and adding the corresponding asphalt warm mix agent into the geopolymer slurry in a ratio of 5:1, and gently stirring with a stirrer during the process of adding the asphalt warm mix agent, so that the asphalt warm mix agent is initially dispersed in the geopolymer slurry to avoid large agglomeration;
[0036] S402, continuous stirring and mixing: start the mixer and set the stirring time to 30 to 60 minutes. During the stirring process, regularly check the uniformity of the mixed slurry to ensure that the asphalt warm mix agent is completely dispersed and fully integrated with the geopolymer slurry;
[0037] S403, sampling inspection: After the mixing is completed, take samples to check the uniformity and consistency of the mixed slurry. If unevenness or caking is found, the mixing time can be appropriately extended or manual mixing can be performed to improve the uniformity, so as to facilitate subsequent mixing with waste concrete aggregates.
[0038] Preferably, in step S50, the following steps are also included:
[0039] S501, vacuuming the mixture: putting the mixed slurry prepared in step S40 and the waste concrete aggregate prepared in step S20 into a vacuum kettle in a ratio of 3:5, then closing the vacuum kettle and starting a vacuum pump to extract the air in the kettle to create a low-pressure environment and reduce the generation of bubbles during the mixing process;
[0040] S502, oscillating and mixing: under vacuum, start the oscillation device in the vacuum kettle, set the oscillation time to 30 to 60 minutes, and ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate;
[0041] S503, static treatment: after stopping the oscillation, let the waste concrete aggregate stand in the vacuum kettle for 1 to 3 hours, so that the mixed slurry can be more stably attached to the surface of the waste concrete aggregate;
[0042] S504, filter impurities: After standing, open the vacuum kettle, take samples to check the mixing effect of the waste concrete aggregate and the mixed slurry, and use a fine sieve or filter to filter the mixed waste concrete aggregate to remove any unattached impurities or small particles to ensure the purity of the mixed waste concrete aggregate.
[0043] Preferably, in step S60, the following steps are also included:
[0044] S601, aggregate curing: spread the filtered mixed waste concrete aggregate on a tray or shelf in a standard curing room, set the temperature of the standard curing room to 25±2℃, and the humidity to 92% to 98% to simulate the curing environment;
[0045] Ensure that there is a certain amount of spacing between mixed waste concrete aggregates to facilitate even distribution of moisture and heat;
[0046] S602, Aggregate curing: The mixed waste concrete aggregate is placed in a standard curing room for 20 to 40 hours to ensure that the mixed slurry is fully cured and forms a solid carbon-reduced recycled aggregate with the waste concrete aggregate;
[0047] S603, Inspection and storage: After the maintenance is completed, the carbon-reduced recycled aggregate is taken out, inspected and evaluated, and the qualified carbon-reduced recycled aggregate is stored in a dry and ventilated place for subsequent use.
[0048] Compared with the prior art, the technical solution of the present application has the following beneficial technical effects: the present invention utilizes waste concrete aggregate to replace traditional natural crushed stone aggregate, thereby not only realizing the effective recycling of resources, but also significantly reducing the over-exploitation of natural resources, alleviating the environmental pressure caused by the disorderly stacking of waste concrete, and not only solving the problems existing in existing recycled aggregates, but also providing sustainable building materials for road engineering construction, reflecting the profound practice of the concept of sustainable development; by using a specific alkali activator to strengthen the aggregate particles, not only the strength and density of the aggregate particles are improved, so that their performance meets the requirements of road engineering aggregates, but also the preparation process is simple and environmentally friendly, without the need to use traditional strengthening materials such as silicate cement, thereby reducing carbon emissions. and damage to the environment; by optimizing the formula of the alkali activator, the strengthening effect of the aggregate particles is further improved. Under the stimulation of the alkaline solution, the geopolymer forms a unique three-dimensional network gel, which has excellent thermal stability, chemical stability and bonding strength, thereby effectively making up for the strength deficiency of the recycled aggregate and greatly improving its overall performance; the present invention utilizes the micropores and cracks on the surface of the recycled aggregate to adsorb the asphalt warm mix agent, which not only significantly reduces the construction temperature of the recycled aggregate asphalt concrete during the mixing process, but also effectively reduces carbon emissions. At the same time, the preparation method of the present invention can also process construction waste on-site, avoiding the problems of long-distance transportation and complex processing, simplifying the construction process, and improving the convenience and economy of recycled aggregate.
[0049] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0051] Figure 1 It is a schematic flow chart of a method for preparing carbon-reduced recycled aggregate based on alkali-activated strengthening according to the present invention;
[0052] Figure 2 It is an elevation diagram of a method for preparing carbon-reduced recycled aggregate based on alkali-activated strengthening according to the present invention. DETAILED DESCRIPTION
[0053] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0054] In order to achieve the above purpose, the present invention provides the following technical solutions:
[0055] A carbon-reducing recycled aggregate based on alkali activation strengthening comprises waste concrete aggregate, alkali activator, geopolymer and asphalt warm mix agent, wherein the mass ratios of the waste concrete aggregate, alkali activator, geopolymer and asphalt warm mix agent per unit volume mass are as follows: 70% to 85% of waste concrete aggregate, 5% to 10% of alkali activator, 8% to 15% of geopolymer and 2% to 5% of asphalt warm mix agent; the carbon-reducing recycled aggregate in the present invention utilizes specific waste concrete aggregate and mixes it with a specific proportion of alkali activator to strengthen aggregate performance, adds geopolymer to improve structural stability, and uses asphalt warm mix agent to optimize construction workability and working performance, thereby achieving the purpose of reducing carbon emissions and improving the use efficiency and environmental protection performance of recycled aggregate.
[0056] Furthermore, the particle size of waste concrete aggregate is 2 to 25 mm. The particle size of aggregate has a crucial impact on its performance in the new concrete mixture. Too large or too small a particle size may lead to uneven mixing or affect the strength of concrete. Therefore, we choose a particle size range of 2 to 25 mm, which is the optimal range that has been carefully calculated and experimentally verified. This specific particle size range is selected to ensure that the aggregate can be evenly distributed in the new concrete mixture while providing sufficient structural stability and bearing capacity. In this way, we not only achieve effective recycling of resources, but also provide new possibilities for building more environmentally friendly and sustainable building materials.
[0057] Furthermore, the alkali activator is mainly composed of solid water glass and alkaline oxides, wherein the ratio of solid water glass to alkaline oxides is carefully formulated to ensure the best activating effect, and is applicable to a variety of concrete materials, and can effectively improve the strength, durability and other key properties of the materials; in the alkali activator, the modulus of solid water glass is controlled at 1 to 2.5, which is to ensure that solid water glass and alkaline oxides can fully react to produce the best activating effect, wherein the selection of the modulus of solid water glass directly affects the final performance and stability of the concrete material; the mass proportion of solid water glass is 40% to 80%, which can effectively promote the hardening and curing of concrete materials; the mass proportion of alkaline oxides in the alkali activator is 20% to 60%, wherein the alkaline oxide can be any one of sodium hydroxide, potassium hydroxide or sodium carbonate, or a mixture of these substances, wherein the selection and proportion of sodium hydroxide, potassium hydroxide or sodium carbonate are based on the activating requirements and performance optimization considerations for different concrete materials.
[0058] Furthermore, geopolymers are mainly composed of industrial by-products or natural minerals such as kaolin, fly ash and blast furnace slag. Under appropriate conditions, these materials can form cementitious materials with high strength and durability. In the preparation of geopolymers, any one of kaolin, fly ash and blast furnace slag can be selected as the main component, or these materials can be mixed in a certain proportion. This flexibility enables geopolymers to be optimized according to different engineering requirements and material costs. Kaolin, fly ash and blast furnace slag are all by-products or wastes of industrial production. Using them to prepare geopolymers not only realizes the recycling of resources, but also effectively reduces the pollution of industrial waste to the environment, which meets the current high requirements for environmental protection and sustainability of building materials. Since the main components of geopolymers have excellent cementitious properties, the prepared geopolymer concrete materials perform well in strength, durability, impermeability and other aspects, making geopolymers have broad application prospects in infrastructure construction such as buildings, roads and bridges.
[0059] Furthermore, the asphalt warm mix agent is a synthetic zeolite asphalt warm mix agent. Synthetic zeolite asphalt warm mix agent, with its unique structure and performance, provides excellent warm mix effect for asphalt concrete. Through its unique zeolite structure, the warm mix agent can effectively reduce the construction temperature during the asphalt mixing process while maintaining the stability and durability of concrete, making important contributions to environmental protection and energy conservation. Lowering the construction temperature means reducing energy consumption and carbon emissions, which meets the current high requirements of the construction industry for green and environmental protection.
[0060] Please refer to Figure 1 , Figure 2 A method for preparing carbon-reduced recycled aggregate based on alkali-activated strengthening comprises the following steps:
[0061] S10, cleaning and treatment: First, the concrete waste is crushed and the waste concrete aggregate with a particle size between 2 and 25 mm is screened out, and then carefully washed and rinsed with clean water until the water is clear and free of sediment. The purpose of this step is to obtain pre-treated waste concrete aggregates, ensure that their surface is clean and free of impurities, and lay a good foundation for subsequent treatment;
[0062] S20, drying: then, the pre-treated waste concrete aggregate is placed in an oven at a temperature of 110±5°C for ventilation drying for 4 to 6 hours. Through this step, completely dried waste concrete aggregate is obtained, which creates favorable conditions for the subsequent uniform coating of geopolymer and asphalt warm mix agent;
[0063] S30, preparation of geopolymer slurry: In this stage, according to the preset alkali dosage, the mass of the required alkali activator and geopolymer is accurately calculated, and then the geopolymer raw material is dissolved in the activator solution, and a uniform and stable geopolymer slurry is prepared by stirring;
[0064] S40, asphalt warm mix agent mixing: Next, the asphalt warm mix agent is added to the geopolymer slurry prepared in step S30, and is fully stirred to ensure that the asphalt warm mix agent can be evenly dispersed in the geopolymer slurry to obtain a mixed slurry with uniform mixing and stable performance;
[0065] S50, strengthening: under vacuum conditions, the mixed slurry prepared in step S40 is mixed with the waste concrete aggregate that has been washed in step S20. Through this step, the geopolymer slurry and the asphalt warm mix agent can be evenly coated on the surface of the waste concrete aggregate, thereby enhancing its overall strength and stability;
[0066] S60, molding and curing: Finally, the waste concrete aggregates strengthened in step S50 are taken out, and the impurities generated in the mixing process are filtered out. Subsequently, the waste concrete aggregates are placed in a standard curing room for curing. After a period of curing, the waste concrete aggregates are transformed into carbon-reduced recycled aggregates with excellent performance and stability.
[0067] Furthermore, in step S10, the following steps are also included:
[0068] S101, Screening Aggregates: Use a screen with an aperture precisely controlled at 2-25mm to screen the waste concrete aggregates after preliminary crushing. The purpose of this step is to ensure that the particle size of the collected waste concrete aggregates is uniform, which facilitates subsequent processing and ensures the quality of the final product;
[0069] S102, Aggregate washing: Pour the screened waste concrete aggregate into a special washing tank or a large-capacity container, fully soak it with clean water, and stir it continuously for 30 to 60 minutes with the help of a stirring tool to ensure that the dirt and residue on the surface of the waste concrete aggregate are completely removed;
[0070] S103, Aggregate Flushing: After soaking and stirring, take the waste concrete aggregate out of the washing tank and rinse it continuously with clean water for 2 to 4 times. This step is very important to ensure that the surface of the waste concrete aggregate is clean and free of sediment, providing high-quality raw materials for subsequent processing;
[0071] S104, Inspection and Drying: The rinsed waste concrete aggregates are spread out in a clean area for visual inspection to confirm whether their surfaces are clean and free of impurities. The waste concrete aggregates are naturally dried at this stage to prepare for the next processing steps. Through strict cleaning and inspection processes, not only the quality of the waste concrete aggregates is improved, but also a solid foundation is laid for subsequent production links.
[0072] Furthermore, in step S20, the following steps are also included:
[0073] S201, prepare the oven: before starting the drying process, conduct a comprehensive inspection of the oven, including confirming whether the oven is in good working condition and whether the temperature control system is accurate. To create a constant thermal environment, the oven temperature is set at 110°C and a temperature floating range of ±5°C is set to ensure temperature stability during the entire drying process;
[0074] S202, drying aggregate: Next, the pre-treated and cleaned waste concrete aggregate is spread on a tray in the oven, and then the heating function of the oven is started, and a drying cycle of 4 to 6 hours is set. At the same time, the ventilation system of the oven is turned on to promote air circulation, thereby more effectively accelerating the drying speed of the aggregate;
[0075] S203, complete drying: During the aggregate drying process, it is necessary to regularly monitor the temperature in the oven and the state of the waste concrete aggregate. Once the preset drying time is reached, the heating device of the oven is immediately turned off and the oven door is opened to dissipate heat. Subsequently, the completely dried waste concrete aggregate is carefully taken out of the oven using special tools and stored in a clean and dry container to prepare for subsequent processing steps.
[0076] Furthermore, in step S30, the following steps are also included:
[0077] S301, preparation of alkali activator: First, according to the preset alkali dosage (in terms of Na 2O is the percentage of the total mass of the cementitious material), and the specific mass of the water glass and alkaline oxide required for the alkaline activator is accurately calculated;
[0078] Then, the precisely weighed solid water glass is gradually added to an appropriate amount of clean water, and stirring is continued during the addition process to ensure that the solid water glass can be evenly and completely dissolved in the water;
[0079] After the solid water glass is dissolved, the water glass solution is cooled naturally to room temperature and aged for 18 to 30 hours to improve its stability and activity;
[0080] Next, the pre-weighed alkaline oxide is gradually added to the prepared water glass solution, while being continuously stirred until the alkaline oxide is completely dissolved and the entire mixed solution is ensured to be uniform, thereby obtaining an alkaline activator solution, and the alkaline activator solution is again allowed to cool naturally to room temperature for subsequent use;
[0081] S302, geopolymer preparation: according to the preset alkali dosage (Na 2 O as a percentage of the total mass of the cementitious material), accurately calculate the mass of the required geopolymer; optimize the preparation of geopolymer according to different engineering requirements and material costs, and select one or more mixtures of metakaolin, fly ash, silica fume and blast furnace slag as the raw materials of geopolymer to ensure its performance and quality;
[0082] S303, prepare geopolymer slurry: add geopolymer into the alkaline activator solution in small amounts and multiple times. Each time the geopolymer is added, it needs to be fully stirred for 10 to 30 minutes to ensure that the geopolymer is completely dissolved in the alkaline activator. Through this step, a uniform and high-quality geopolymer slurry is obtained, which lays a solid foundation for subsequent operation steps.
[0083] Furthermore, in step S40, the following steps are also included:
[0084] S401, preliminary mixing: first, measure a certain amount of geopolymer slurry and place it in a professional mixing container. Then, slowly add the asphalt warm mix agent into the container in a precise ratio (i.e., a ratio of 5:1 between geopolymer slurry and asphalt warm mix agent). During this process, use a special agitator to perform gentle stirring to ensure that the asphalt warm mix agent can be initially and evenly dispersed in the geopolymer slurry, thereby effectively avoiding the occurrence of large block aggregation;
[0085] S402, continuous stirring and mixing: Next, we start the efficient mixer and set an appropriate stirring time, usually between 30 and 60 minutes. During the whole stirring process, the uniformity of the mixed slurry needs to be checked regularly to ensure that the asphalt warm mix agent can be completely and thoroughly dispersed, so that the asphalt warm mix agent and the geopolymer slurry can achieve a perfect fusion state;
[0086] S403, sampling inspection: Once the mixing process is completed, sampling is carried out immediately, and the uniformity and consistency of the mixed slurry are carefully checked. If any unevenness or lumps are found, the mixing time is extended according to the actual situation, or more careful manual mixing is performed to ensure the quality of the slurry; finally, the carefully prepared mixed slurry is mixed with waste concrete aggregate.
[0087] Furthermore, in step S50, the following steps are also included:
[0088] S501, vacuuming the mixture: First, the mixed slurry and waste concrete aggregate are placed in a vacuum kettle at a ratio of 3:5. Then, the vacuum kettle is tightly closed and an efficient vacuum pump is started to quickly extract the air in the kettle. This step is crucial and can create a low-pressure environment in the vacuum kettle, which greatly reduces the generation of bubbles in the subsequent mixing process and ensures the quality of the mixture.
[0089] S502, oscillating and mixing: after ensuring that the vacuum kettle has reached a suitable low-pressure environment, start the oscillation device in the kettle and set a reasonable oscillation time, usually between 30 and 60 minutes, to ensure that the mixed slurry can fully and evenly cover and wrap each waste concrete aggregate;
[0090] S503, static treatment: after the oscillation process is completed, the mixed waste concrete aggregate is allowed to stand in the vacuum kettle for 1 to 3 hours. The purpose of this step is to allow the mixed slurry to adhere more tightly and stably to the surface of the waste concrete aggregate, thereby enhancing its overall stability and durability;
[0091] S504, filter impurities: After the static treatment is completed, open the vacuum kettle and take samples to check the mixing effect to ensure the purity of the mixed waste concrete aggregate; and use a fine sieve or a special filter to filter the mixed waste concrete aggregate to completely remove any unattached impurities or small particles on the mixed waste concrete aggregate. This fine filtering step is designed to ensure that the mixed waste concrete aggregate we finally obtain is of high quality and without any defects.
[0092] Furthermore, in step S60, the following steps are also included:
[0093] S601. Aggregate curing: In a standard curing room, the filtered mixed waste concrete aggregates are carefully spread on special trays or racks. In order to simulate the best curing environment, the temperature of the standard curing room is strictly set to 25±2℃, and the humidity is controlled within the range of 92% to 98%. At the same time, in order to ensure that moisture and heat can be evenly distributed among the aggregates, appropriate spacing is retained between the mixed waste concrete aggregates.
[0094] S602, Aggregate Curing: The mixed waste concrete aggregate is placed in a standard curing room for 20 to 40 hours of static curing. This key step is to ensure that the mixed slurry can be fully solidified and closely combined with the waste concrete aggregate, ultimately forming a strong and durable carbon-reducing recycled aggregate;
[0095] S603, Inspection and storage: After the curing period, the carbon-reduced recycled aggregates are taken out and comprehensively inspected and evaluated. After strict screening, qualified carbon-reduced recycled aggregates are stored in a dry, ventilated dedicated area for use in subsequent construction projects or other related applications.
[0096] Example 1
[0097] A carbon-reducing recycled aggregate based on alkali-activated strengthening is prepared from raw materials containing the following components: 85% of waste concrete aggregate, 5% of alkali activator, 8% of geopolymer, and 2% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 2 mm; in this ratio, a high proportion of waste concrete aggregate helps to maximize resource reuse, reduce the demand for new materials, and thus reduce costs, while a low proportion of alkali activator and geopolymer reduces dependence on chemicals while ensuring performance; and 2% asphalt warm mix agent makes construction smoother and improves work performance; the alkali activator Solid water glass and sodium hydroxide are mixed in a ratio of 6:4. 60% of solid water glass (modulus is 1.5) provides sufficient silicate components to help form a strong gel structure. 40% of sodium hydroxide, as an alkaline oxide, effectively promotes the alkali-induced reaction and improves the early strength of the aggregate. The geopolymer is mixed with kaolin and fly ash in a ratio of 6:4. The mixture of kaolin and fly ash serves as a geopolymer, which combines the high reactivity of kaolin and the particle filling effect of fly ash to improve the density and strength of the aggregate.
[0098] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0099] S10, using a sieve with an aperture of 2 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 2 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 30 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water twice to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to carry out the subsequent steps;
[0100] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 105°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0101] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 1.5 and sodium hydroxide, and mix them in a ratio of 6:4 to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform an aging treatment for 18 hours; then gradually add the weighed sodium hydroxide to the prepared water glass solution, stir until the sodium hydroxide is completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, let the alkali activator solution cool to room temperature for standby use; according to different engineering requirements, weigh metakaolin and fly ash, and mix them in a ratio of 6:4 to prepare a geopolymer; add the geopolymer to the alkali activator solution in small amounts and multiple times, and each time the geopolymer is added, it is necessary to fully stir for 10 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0102] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 30 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0103] S50, putting the mixed slurry and waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 30 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 1 hour, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter;
[0104] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 23°C and the humidity to 92% to simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 20 hours to ensure that the mixed slurry is fully cured and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0105] Example 2
[0106] A carbon-reducing recycled aggregate based on alkali activation strengthening is prepared from raw materials containing the following components: 75% of waste concrete aggregate, 7% of alkali activator, 13% of geopolymer, and 5% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 5 mm; in this embodiment, 7% of the alkali activator can effectively strengthen the performance of the waste concrete aggregate, while 13% of the geopolymer provides good structural stability, and by appropriately increasing the ratio of the alkali activator and the geopolymer, the strength and durability of the recycled aggregate can be enhanced, and 5% of the asphalt warm mix agent helps to improve construction and workability; the alkali activator is prepared by mixing solid water glass and potassium hydroxide in a ratio of 5:5, wherein 50% of the solid water glass (modulus of 2) is combined with 50% of potassium hydroxide to provide balanced alkalinity and silicate components, which helps to form a stable aggregate structure; the geopolymer is prepared from blast furnace slag, wherein the high silicate content in the blast furnace slag helps to improve the durability and chemical corrosion resistance of the aggregate.
[0107] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0108] S10, using a sieve with an aperture of 5 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 5 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 35 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water twice to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to carry out the subsequent steps;
[0109] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 110°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0110] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 2 and potassium hydroxide, and mix them in a ratio of 5:5 to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform an aging treatment for 20 hours; then gradually add the weighed potassium hydroxide to the prepared water glass solution, stir until the potassium hydroxide is completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, let the alkali activator solution cool to room temperature for standby use; according to different engineering requirements, weigh a sufficient amount of blast furnace slag as a geopolymer, and then add the geopolymer to the alkali activator solution in small amounts and multiple times. Each time the geopolymer is added, it is necessary to stir it for 10 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0111] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 35 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0112] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 35 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 1 hour, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, sampling to check the mixing effect, and using a filter to filter the mixed waste concrete aggregate;
[0113] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 25°C and the humidity to 93% to simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 24 hours to ensure that the mixed slurry is fully solidified and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0114] Example 3
[0115] A carbon-reducing recycled aggregate based on alkali activation and strengthening is prepared from raw materials containing the following components: 70% of waste concrete aggregate, 10% of alkali activator, 15% of geopolymer, and 5% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 8 mm; in this ratio, 70% of the waste concrete aggregate ensures the main structure of the aggregate, 10% of the alkali activator moderately strengthens the aggregate, and 15% of the geopolymer provides a stable structural support. A high proportion of alkali activator and geopolymer can significantly improve the mechanical properties and durability of the recycled aggregate, and is suitable for projects with high requirements on material performance, while 5 % asphalt warm mix agent significantly improves the workability of construction; the alkali activator is mixed with solid water glass and sodium carbonate in the ratio of 8:2, among which 80% high proportion of solid water glass (modulus is 1) ensures sufficient supply of silicate, and 20% sodium carbonate as alkaline oxide provides the necessary alkaline environment for alkali activation reaction, enhancing the durability of aggregate; geopolymer is mixed with kaolin, fly ash and blast furnace slag in the ratio of 3:4:3. The three raw materials are mixed and used, combining their respective advantages to improve the comprehensive performance of aggregate, including strength, durability and crack resistance.
[0116] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0117] S10, using a sieve with an aperture of 10 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 10 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 35 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water for 3 times to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to proceed to the subsequent steps;
[0118] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 110°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 5 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0119] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 1 and sodium carbonate, and mix them in a ratio of 8:2 to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform aging treatment for 24 hours; then gradually add the weighed sodium carbonate to the prepared water glass solution, stir until the sodium carbonate is completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, cool to room temperature for standby use; according to different engineering requirements, weigh metakaolin, fly ash and blast furnace slag, mix and prepare a geopolymer in a ratio of 3:4:3, and then add the geopolymer to the alkali activator solution in small amounts and multiple times. Each time the geopolymer is added, it is necessary to fully stir for 15 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0120] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 40 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0121] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 40 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 2 hours, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter;
[0122] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 25°C and the humidity to 95%, simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 24 hours to ensure that the mixed slurry is fully solidified and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0123] Example 4
[0124] A carbon-reducing recycled aggregate based on alkali-activated strengthening is prepared from raw materials containing the following components: 80% of waste concrete aggregate, 6% of alkali activator, 12% of geopolymer, and 2% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 10 mm; in this ratio, 80% of the waste concrete aggregate maximizes the use of waste resources, 6% of the alkali activator reduces the use of chemical reagents while maintaining the strength of the aggregate, 12% of the geopolymer enhances the stability of the structure, and 5% of the asphalt warm mix agent improves the construction performance The alkali activator is prepared by mixing solid water glass, sodium hydroxide and potassium hydroxide in a ratio of 5:3:2, wherein solid water glass (modulus is 1.5) ensures sufficient supply of silicate, and the mixed use of sodium hydroxide and potassium hydroxide provides a diversified alkaline environment, which helps to more comprehensively stimulate the activity of aggregates; the geopolymer is prepared by mixing kaolin and fly ash in a ratio of 8:2. A high proportion of kaolin and a low proportion of fly ash are used as geopolymers, which ensure the rapid response of aggregates and the formation of early strength.
[0125] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0126] S10, using a sieve with an aperture of 15 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 15 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 40 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water for 3 times to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to proceed to the subsequent steps;
[0127] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 115°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0128] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 1.5, sodium hydroxide and potassium hydroxide, and mix them in a ratio of 5:3:2 to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform aging treatment for 24 hours; then gradually add the weighed sodium hydroxide and potassium hydroxide mixture to the prepared water glass solution, stir until the sodium hydroxide and potassium hydroxide are completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, cool to room temperature for standby use; according to different engineering requirements, weigh metakaolin and fly ash, mix and prepare a geopolymer in a ratio of 8:2, and then add the geopolymer to the alkali activator solution in small amounts and multiple times. Each time the geopolymer is added, it is necessary to stir it for 20 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0129] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 45 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0130] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 45 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 1 hour, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, sampling to check the mixing effect, and using a filter to filter the mixed waste concrete aggregate;
[0131] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 27°C and the humidity to 98% to simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 28 hours to ensure that the mixed slurry is fully solidified and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0132] Example 5
[0133] A carbon-reducing recycled aggregate based on alkali activation strengthening is prepared from raw materials comprising the following components: 78% of waste concrete aggregate, 8% of alkali activator, 10% of geopolymer, and 4% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 16 mm; in this ratio, while ensuring the strength of the aggregate, by fine-tuning the ratio of each component, this ratio is intended to provide the best construction performance and durability, reduce costs, and is also environmentally friendly; the alkali activator is prepared by mixing solid water glass and sodium carbonate in a ratio of 7:3, wherein 70% of solid water glass (modulus of 2.5) and 30% of sodium carbonate are combined, which not only ensures the supply of silicate, but also provides a suitable alkaline environment, which is conducive to forming high-strength aggregate; the geopolymer is prepared by mixing metakaolin and blast furnace slag in a ratio of 5:5, and the mixture of metakaolin and blast furnace slag combines the advantages of both and improves the mechanical properties and durability of the aggregate.
[0134] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0135] S10, using a sieve with an aperture of 20 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 20 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 45 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water for 4 times to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to proceed to the subsequent steps;
[0136] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 110°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 5 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0137] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 2.5 and sodium carbonate, and mix them in a ratio of 7:3 to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform aging treatment for 24 hours; then gradually add the weighed sodium carbonate to the prepared water glass solution, stir until the sodium carbonate is completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, cool to room temperature for standby use; according to different engineering requirements, weigh metakaolin and blast furnace slag, mix and prepare a geopolymer in a ratio of 5:5, and then add the geopolymer to the alkali activator solution in small amounts and multiple times. Each time the geopolymer is added, it is necessary to stir it for 25 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0138] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 50 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0139] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 50 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 2 hours, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter;
[0140] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 25°C and the humidity to 98%, simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 30 hours to ensure that the mixed slurry is fully cured and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0141] Example 6
[0142] A carbon-reducing recycled aggregate based on alkali-activated strengthening is prepared from raw materials containing the following components: 82% of waste concrete aggregate, 9% of alkali activator, 14% of geopolymer, and 5% of warm asphalt mix agent, wherein the particle size of the waste concrete aggregate is 20 mm; in this ratio, while maximizing the use of waste concrete aggregate, the strength and stability of the aggregate are ensured by 9% of alkali activator and 14% of geopolymer, and the early strength and durability of the material are improved. It is suitable for engineering projects that need to be put into use quickly, and 5% of warm asphalt mix agent It can effectively improve construction workability; the alkali activator is prepared by mixing solid water glass, sodium hydroxide, potassium hydroxide and sodium carbonate in a ratio of 4:2:2:2, wherein the mixture of 40% solid water glass (modulus is 2) and three alkaline oxides provides a rich alkaline environment, which helps to promote the alkali activation reaction more comprehensively and improve the performance of aggregate; the geopolymer is prepared by mixing fly ash and blast furnace slag in a ratio of 5:5, and the mixture of fly ash and blast furnace slag is used as a geopolymer to improve the stability and impermeability of the aggregate.
[0143] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0144] S10, using a sieve with an aperture of 15 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 15 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 50 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water twice to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to proceed to the subsequent steps;
[0145] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 105°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0146] S30, according to the preset alkali dosage, weigh the solid water glass with a modulus of 2, sodium hydroxide, potassium hydroxide and sodium carbonate, and mix them in a ratio of 4:2:2:2 to prepare an alkali activator; during the configuration process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water, and after the dissolution is completed, let it cool to room temperature and perform aging treatment for 28 hours; then gradually add the weighed sodium hydroxide, potassium hydroxide and sodium carbonate mixture to the prepared water glass solution, stir until the sodium hydroxide, potassium hydroxide and sodium carbonate mixture is completely dissolved, and ensure that the solution is uniform, and cool to room temperature for standby use after the dissolution is completed; according to different engineering requirements, weigh fly ash and blast furnace slag, mix and prepare a geopolymer in a ratio of 5:5, then add the geopolymer to the alkali activator solution in small amounts and multiple times, and each time the geopolymer is added, it is necessary to stir it for 20 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0147] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 30 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0148] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 30 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 3 hours, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter;
[0149] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 25°C and the humidity to 98%, simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 30 hours to ensure that the mixed slurry is fully cured and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0150] Example 7
[0151] A carbon-reducing recycled aggregate based on alkali activation strengthening is prepared from raw materials containing the following components: 72% of waste concrete aggregate, 9% of alkali activator, 14% of geopolymer, and 5% of asphalt warm mix agent, wherein the particle size of the waste concrete aggregate is 25 mm; in this embodiment, the waste concrete aggregate makes full use of waste resources, while 9% of alkali activator and 14% of geopolymer reduce the use of new materials as much as possible while ensuring the performance of the aggregate, and 5% of asphalt warm mix agent makes the construction smoother; the alkali activator is prepared by mixing solid water glass, sodium hydroxide and potassium hydroxide in a ratio of 6:2:2, wherein 70% of solid water glass (modulus of 2.5) is mixed with sodium hydroxide and potassium hydroxide, thereby achieving balanced improvement of aggregate performance, ensuring the strength of the aggregate and improving its durability; the geopolymer is prepared by mixing metakaolin, fly ash and blast furnace slag in a ratio of 5:3:2, and the specific proportions of the three geopolymers are mixed to achieve comprehensive optimization of aggregate performance, including strength, durability and workability.
[0152] The method for preparing carbon-reduced recycled aggregate specifically comprises the following steps:
[0153] S10, using a sieve with an aperture of 25 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 25 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 60 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water for 3 times to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to proceed to the subsequent steps;
[0154] S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 110°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 6 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps;
[0155] S30. According to the preset alkali dosage, weigh solid water glass with a modulus of 2.5, sodium hydroxide and potassium hydroxide, and mix them in a ratio of 6:2:2 to prepare an alkali activator; during the configuration process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform an aging treatment for 30 hours; then gradually add the weighed sodium hydroxide and potassium hydroxide mixture to the prepared water glass solution, stir until the sodium hydroxide and potassium hydroxide mixture is completely dissolved, and ensure that the solution is uniform, and cool to room temperature for standby use after the dissolution is completed; according to different engineering requirements, weigh metakaolin, fly ash and blast furnace slag, mix and prepare a geopolymer in a ratio of 5:3:2, and then add the geopolymer to the alkali activator solution in small amounts and multiple times. Each time the geopolymer is added, it is necessary to fully stir for 30 minutes to ensure that the geopolymer is completely dissolved in the alkali activator to obtain a uniform geopolymer slurry for subsequent steps;
[0156] S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the addition of the asphalt warm mix agent to allow the asphalt warm mix agent to be initially dispersed in the geopolymer slurry; after the addition of the asphalt warm mix agent, turning on the mixer and stirring for 60 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, sampling is taken to check the uniformity and consistency of the mixed slurry, and the prepared mixed slurry is immediately mixed with the waste concrete aggregate;
[0157] S50, putting the mixed slurry and the waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 60 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 2 hours, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter;
[0158] S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room, set the temperature of the standard curing room to 25°C and the humidity to 98%, simulate the curing environment, and allow the mixed waste concrete aggregate to stand in the standard curing room for 40 hours to ensure that the mixed slurry is fully cured and forms a firm carbon-reduced recycled aggregate with the aggregate; after the curing is completed, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
[0159] In summary: the present invention utilizes waste concrete aggregate to replace traditional natural crushed stone aggregate, which not only realizes the effective recycling of resources, but also significantly reduces the over-exploitation of natural resources, alleviates the environmental pressure caused by the disorderly stacking of waste concrete, and can not only solve the problems existing in the existing recycled aggregates, but also provide sustainable building materials for road engineering construction, reflecting the profound practice of the concept of sustainable development; by using a specific alkali activator to strengthen the aggregate particles, not only the strength and density of the aggregate particles are improved, so that their performance meets the requirements of road engineering aggregates, but also the preparation process is simple and environmentally friendly, without the need to use traditional strengthening materials such as silicate cement, thereby reducing carbon emissions and damage to the environment; by optimizing The formula of the alkali activator further improves the strengthening effect of the aggregate particles. Under the stimulation of the alkaline solution, the geopolymer forms a unique three-dimensional network gel, which has excellent thermal stability, chemical stability and bonding strength, thereby effectively making up for the strength deficiency of the recycled aggregate and greatly improving its overall performance. The present invention utilizes the micropores and cracks on the surface of the recycled aggregate to adsorb the asphalt warm mix agent, which not only significantly reduces the construction temperature of the recycled aggregate asphalt concrete during the mixing process, but also effectively reduces carbon emissions. At the same time, the preparation method of the present invention can also process construction waste on-site, avoiding the problems of long-distance transportation and complex processing, simplifying the construction process, and improving the convenience and economy of recycled aggregate.
[0160] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0161] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.
Claims
1. A method for preparing carbon-reduced recycled aggregate based on alkali-activated strengthening, characterized in that: The following steps are involved: S10, using a sieve with an aperture of 2 to 25 mm to screen the preliminarily crushed waste concrete aggregates, collecting the screened waste concrete aggregates, and preparing for the next step of washing; pouring the waste concrete aggregates within the particle size range of 2 to 25 mm separated by the sieve into a large washing tank, fully soaking them with clean water, and stirring them with a stirring tool for 30 to 60 minutes to remove dirt on the surface of the waste concrete aggregates; taking the waste concrete aggregates out of the washing tank, and washing them with clean water for 2 to 4 times to ensure that the surface of the waste concrete aggregates is clean and free of sand; spreading the washed waste concrete aggregates in a clean area for visual inspection and drying to ensure that the surface of the waste concrete aggregates is clean and free of impurities, so as to carry out the subsequent steps; S20, check the working status of the oven to ensure that it operates normally and the temperature control is accurate, set the oven temperature to 110°C, and set the temperature floating range to ±5°C to maintain a constant temperature environment; take the pre-treated clean waste concrete aggregate, evenly spread it on the tray in the oven, start the oven heating function, set the drying time to 4 to 6 hours, turn on the oven ventilation device to accelerate the drying of the waste concrete aggregate; after the set drying time is reached, turn off the oven heating function, open the oven door, use tools to take the dried waste concrete aggregate out of the oven, and place it in a clean and dry container for subsequent steps; S30. According to the preset alkali dosage, weigh solid water glass and alkaline oxide, and mix them in proportion to prepare an alkali activator; during the preparation process, gradually add the weighed solid water glass to an appropriate amount of water, stirring while adding to ensure that the solid water glass is evenly dissolved in the water. After the dissolution is completed, let it cool to room temperature and perform an aging treatment for 18 to 30 hours; then gradually add the weighed alkaline oxide to the prepared water glass solution, stir until the alkaline oxide is completely dissolved, and ensure that the solution is uniform. After the dissolution is completed, let the alkaline activator solution cool to room temperature for standby use; according to different engineering requirements, weigh metakaolin and fly ash, and mix them in a ratio of 6:4 to prepare a geopolymer; add the geopolymer to the alkaline activator solution in small amounts and multiple times, and each time the geopolymer is added, it needs to be fully stirred for 10 to 30 minutes to ensure that the geopolymer is completely dissolved in the alkaline activator to obtain a uniform geopolymer slurry for subsequent steps; S40, placing the geopolymer slurry and the asphalt warm mix agent in a mixing container at a ratio of 5:1, and gently stirring during the process of adding the asphalt warm mix agent to make the asphalt warm mix agent preliminarily dispersed in the geopolymer slurry; after the asphalt warm mix agent is added, start the mixer and stir for 30 to 60 minutes to ensure that the asphalt warm mix agent is completely integrated with the geopolymer slurry; after the stirring is completed, take a sample to check the uniformity and consistency of the mixed slurry, and immediately mix the prepared mixed slurry with the waste concrete aggregate; S50, putting the mixed slurry and waste concrete aggregate into a vacuum kettle in a ratio of 3:5, closing the vacuum kettle, and starting the vacuum pump to extract the air in the kettle; in a vacuum state, starting the oscillation device in the vacuum kettle, setting the oscillation time to 30 to 60 minutes, to ensure that the mixed slurry can fully and evenly wrap each waste concrete aggregate; after stopping the oscillation, allowing the mixed waste concrete aggregate to stand in the vacuum kettle for 1 to 3 hours, so that the mixed slurry is more stably attached to the surface of the waste concrete aggregate; after the standing period is completed, opening the vacuum kettle, taking samples to check the mixing effect, and filtering the mixed waste concrete aggregate using a filter; S60. Spread the filtered mixed waste concrete aggregate on a tray in a standard curing room. Set the temperature of the standard curing room to 25±2℃ and the humidity to 92%~98% to simulate the curing environment. Let the mixed waste concrete aggregate stand in the standard curing room for 20~40 hours to ensure that the mixed slurry is fully solidified and forms a firm carbon-reduced recycled aggregate with the aggregate. After the curing, take out the carbon-reduced recycled aggregate, inspect and evaluate it, and store the qualified carbon-reduced recycled aggregate in a dry and ventilated place for subsequent use.
2. A carbon-reduced recycled aggregate prepared by the preparation method of carbon-reduced recycled aggregate based on alkali-activated strengthening as claimed in claim 1, characterized in that: The invention comprises the following components and their corresponding mass proportions: 72% to 85% of waste concrete aggregate, 5% to 10% of alkali activator, 8% to 9% of geopolymer and 2% to 5% of asphalt warm mix agent, wherein the proportions of the waste concrete aggregate, alkali activator, geopolymer and asphalt warm mix agent are all calculated by unit volume mass; the geopolymer comprises metakaolin and fly ash; the alkali activator comprises solid water glass with a modulus of 1 to 2.5 and alkaline oxide, wherein the mass proportion of solid water glass to the alkali activator is 40% to 80%, and the mass proportion of alkaline oxide to the alkali activator is 20% to 60%; the alkaline oxide comprises any one or more mixtures of sodium hydroxide, potassium hydroxide or sodium carbonate.
Citation Information
Patent Citations
Geopolymeric concrete based on recycled aggregate and preparation method of geopolymeric concrete
CN103601424A