A high temperature resistant optical film material for polarizer and preparation method thereof
By modifying polyethylene terephthalate and introducing urea group side chains to form a hydrogen bonding network, the problem of poor stability of polarizers under high temperature conditions is solved, and high transmittance, low haze and Optical film material with high temperature resistance, suitable for applications in hot environments.
Patent Information
- Application Number
- CN202410888218.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-04
AI Technical Summary
Existing polarizers may soften, deform or degrade under high temperature conditions, making it difficult to maintain a stable polarization effect in situations such as hot light sources.
By modifying polyethylene terephthalate, flexible urea group side chains are introduced to form a hydrogen bond network, increase the glass transition temperature, and prepare high-temperature resistant optical film materials.
It improves the high temperature resistance of the material, meets high light transmittance and low haze, and has excellent chemical stability and flexibility, making it suitable for manufacturing high temperature resistant polarizers.
Smart Images

Figure SMS_2 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of materials, and in particular relates to a high temperature resistant optical film material for polarizers and a preparation method thereof. Background Art
[0002] Polarizer is the full name of polarizing film, which can control the polarization direction of a specific light beam. When natural light passes through the polarizer, the light whose vibration direction is perpendicular to the transmission axis of the polarizer will be absorbed, and only the polarized light whose vibration direction is parallel to the transmission axis of the polarizer will be left. Polarizer is mainly made of PVA (polyvinyl alcohol) film, TAC (triacetyl cellulose) film, protective film, release film and pressure-sensitive adhesive.
[0003] With the continuous development of electronic and display technology towards high integration, high density and ultra-thinness, polarizing films with high temperature resistance are increasingly used in high temperature industrial environments, hot light sources and other occasions, which can maintain stable polarization effects in high temperature environments. Polyethylene terephthalate polymer is made into polyethylene terephthalate PET film by biaxial stretching. Because of its excellent mechanical properties, chemical stability, weather resistance, and optical properties of high transmittance, low haze and high brightness, it is often used in combination with PVA and TAC to form a multilayer optical film structure for polarization applications. PET film has good stability within a certain temperature range, but it may soften, deform or degrade under high temperature conditions. Therefore, it is of great significance to prepare a high temperature resistant optical film material by modifying it to adapt to more application scenarios. Summary of the invention
[0004] In order to solve the above problems, an object of the present invention is to provide a high temperature resistant optical film material for polarizer and a preparation method thereof.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] A high temperature resistant optical film material for polarizer, the structural formula of which is as follows:
[0007] .
[0008] The method for preparing the high temperature resistant optical film material for polarizer comprises the following steps:
[0009] 1) dissolving dimethyl 2-hydroxyterephthalate and 2-hydroxyethylamine in an organic solvent 1, then adding triphenylphosphine and diisopropyl azodicarboxylate, reacting at 25-50° C. for 12-24 hours. After the reaction is completed, removing the solvent by distillation under reduced pressure, washing the obtained residue with deionized water for 2-3 times, and drying to obtain an amino-terminated dimethyl terephthalate derivative;
[0010] 2) adding the terminal amino dimethyl terephthalate derivative and propyl isocyanate prepared in step 1) to organic solvent 2, stirring and dissolving, then adding dibutyltin dilaurate, stirring and reacting at 25-40° C. for 8-12 hours, after the reaction is completed, removing the solvent by distillation under reduced pressure, washing the obtained residue with deionized water 2-3 times, adding it to an alcohol organic solvent, dissolving it, then adding a base thereto, reacting at 30-80° C. for 12-24 hours, after the reaction is completed, removing the solvent by distillation under reduced pressure, washing the residue with deionized water 2-3 times, and drying to obtain a terephthalic acid derivative;
[0011] 3) Add the terephthalic acid derivative and ethylene glycol prepared in step 2) to the organic solvent 3, then add 4-dimethylaminopyridine and 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and react at 25-40° C. for 12-24 hours. After the reaction is completed, filter and wash the filter cake with deionized water for 2-3 times, and dry to obtain a high temperature resistant optical film material for polarizers.
[0012] In step 1), the organic solvent 1 is tetrahydrofuran, acetonitrile or acetone.
[0013] The mass ratio of dimethyl 2-hydroxyterephthalate, 2-hydroxyethylamine, organic solvent 1, triphenylphosphine and diisopropyl azodicarboxylate in step 1) is 1:0.3-0.5:5-10:1.2-1.8:1-1.5.
[0014] The organic solvent 2 in step 2) is dichloromethane, chloroform, acetone, tetrahydrofuran or ether.
[0015] The alcohol organic solvent in step 2) is methanol, ethanol or isopropanol.
[0016] The base in step 2) is potassium hydroxide or sodium hydroxide.
[0017] The mass ratio of the terminal amino dimethyl terephthalate derivative, propyl isocyanate, organic solvent 2, dibutyltin dilaurate, alcohol organic solvent and base in step 2) is 1:0.35~0.5:5~10:0.02~0.1:5~10:0.3~0.8.
[0018] The organic solvent 3 in step 3) is acetone, acetonitrile, tetrahydrofuran, benzene or toluene.
[0019] The mass ratio of the terephthalic acid derivative, ethylene glycol, organic solvent 3, 4-dimethylaminopyridine and 1-ethyl-(3-dimethylaminopropyl)carbodiimide in step 3) is 1:0.2~0.3:5~10:0.04~0.4:0.5~1.5.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] The high temperature resistant optical film material for polarizer of the present invention is prepared by modifying polyethylene terephthalate and introducing flexible urea group side chains into its side chains as strong hydrogen bond donor and acceptor molecular fragments; in the modified polyethylene terephthalate, the flexible urea group side chains of different molecular main chains can attract each other to form a hydrogen bond network, and the existence of such strong non-covalent interaction effectively increases the glass transition temperature of the polymer and enhances the high temperature resistance of the material.
[0022] The high temperature resistant optical film material for polarizer of the present invention can meet the requirements of high light transmittance and low haze, and at the same time has strong flexibility, excellent chemical stability and high temperature resistance, and can be used as an optical film material for manufacturing polarizer. DETAILED DESCRIPTION
[0023] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.
[0024] Example 1 Preparation of high temperature resistant optical film material for polarizer:
[0025] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.03 kg of 2-hydroxyethylamine were dissolved in 0.5 kg of tetrahydrofuran, and then 0.12 kg of triphenylphosphine and 0.1 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 25° C. for 12 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative; 1 H NMR (300 MHz, 298 K, DMSO-d6): δ 8.08 (d, 1H), 7.55 (s, 1H), 7.46(d, 1H), 4.15 (t, 2H), 3.85 (s, 3H), 3.80 (s, 3H), 3.35 (t, 2H), 1.7 (s, 2H).
[0026] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.035 kg of propyl isocyanate were added to 0.5 kg of dichloromethane, stirred to dissolve, and then 0.002 kg of dibutyltin dilaurate was added, and the mixture was stirred and reacted at 25°C for 12 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed with deionized water twice, added to 0.5 kg of methanol, dissolved, and then 0.03 kg of sodium hydroxide was added thereto, and the mixture was reacted at 30°C for 24 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed with deionized water 3 times and dried to obtain a terephthalic acid derivative; 1 H NMR (300 MHz, 298 K, DMSO-d6): δ 12.72(s, 1H), 12.05 (s, 1H), 8.31 (d, 1H), 7.85 (s, 1H), 7.76 (d, 1H), 6.05 (s,2H), 4.15 (t, 2H), 3.44 (t, 2H), 3.35 (t, 2H), 1.57 (m, 2H), 0.85 (t, 3H).
[0027] 0.1 kg of terephthalic acid derivative and 0.02 kg of ethylene glycol were added to 0.5 kg of acetone, and then 0.004 kg of 4-dimethylaminopyridine and 0.05 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the mixture was reacted at 25° C. for 24 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed twice with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0028] Example 2 Preparation of high temperature resistant optical film material for polarizer:
[0029] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.032 kg of 2-hydroxyethylamine were dissolved in 0.6 kg of tetrahydrofuran, and then 0.13 kg of triphenylphosphine and 0.11 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 30° C. for 20 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative;
[0030] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.038 kg of propyl isocyanate were added to 0.6 kg of chloroform, stirred and dissolved, and then 0.004 kg of dibutyltin dilaurate was added, and stirred and reacted at 28°C for 11 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed twice with deionized water, added to 0.6 kg of ethanol, dissolved, and then 0.04 kg of sodium hydroxide was added thereto, and reacted at 40°C for 22 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed 3 times with deionized water and dried to obtain a terephthalic acid derivative;
[0031] 0.1 kg of terephthalic acid derivative and 0.022 kg of ethylene glycol were added to 0.6 kg of acetonitrile, and then 0.009 kg of 4-dimethylaminopyridine and 0.08 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the reaction was carried out at 28°C for 22 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed twice with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0032] Example 3 Preparation of high temperature resistant optical film material for polarizer:
[0033] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.038 kg of 2-hydroxyethylamine were dissolved in 0.7 kg of tetrahydrofuran, and then 0.15 kg of triphenylphosphine and 0.13 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 35° C. for 18 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed 3 times with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative;
[0034] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.04 kg of propyl isocyanate were added to 0.7 kg of tetrahydrofuran, stirred to dissolve, and then 0.006 kg of dibutyltin dilaurate was added, and the mixture was stirred and reacted at 30°C for 10 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed with deionized water for 3 times, and then added to 0.7 kg of methanol. After dissolution, 0.05 kg of sodium hydroxide was added thereto, and the mixture was reacted at 50°C for 18 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed with deionized water for 3 times and dried to obtain a terephthalic acid derivative;
[0035] 0.1 kg of terephthalic acid derivative and 0.025 kg of ethylene glycol were added to 0.7 kg of tetrahydrofuran, and then 0.02 kg of 4-dimethylaminopyridine and 0.1 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the mixture was reacted at 30° C. for 18 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0036] Example 4 Preparation of high temperature resistant optical film material for polarizer:
[0037] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.042 kg of 2-hydroxyethylamine were dissolved in 0.8 kg of acetone, and then 0.16 kg of triphenylphosphine and 0.14 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 40° C. for 15 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative;
[0038] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.045 kg of propyl isocyanate were added to 0.8 kg of acetone, stirred and dissolved, and then 0.008 kg of dibutyltin dilaurate was added, and stirred and reacted at 35°C for 9 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed twice with deionized water, added to 0.8 kg of isopropanol, dissolved, and then 0.065 kg of potassium hydroxide was added thereto, and reacted at 60°C for 15 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain a terephthalic acid derivative;
[0039] 0.1 kg of terephthalic acid derivative and 0.028 kg of ethylene glycol were added to 0.9 kg of toluene, and then 0.03 kg of 4-dimethylaminopyridine and 0.13 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the mixture was reacted at 35°C for 15 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed twice with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0040] Example 5 Preparation of high temperature resistant optical film material for polarizer:
[0041] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.05 kg of 2-hydroxyethylamine were dissolved in 1 kg of acetonitrile, and then 0.18 kg of triphenylphosphine and 0.15 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 50° C. for 12 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed 3 times with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative;
[0042] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.05 kg of propyl isocyanate were added to 1 kg of ether, stirred to dissolve, and then 0.01 kg of dibutyltin dilaurate was added, and stirred to react at 40°C for 8 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed with deionized water for 3 times, and then added to 1 kg of isopropanol. After dissolution, 0.08 kg of potassium hydroxide was added thereto, and the reaction was carried out at 80°C for 12 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed with deionized water for 3 times and dried to obtain a terephthalic acid derivative;
[0043] 0.1 kg of terephthalic acid derivative and 0.03 kg of ethylene glycol were added to 1 kg of benzene, and then 0.04 kg of 4-dimethylaminopyridine and 0.15 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the mixture was reacted at 40°C for 12 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0044] Example 6 Preparation of high temperature resistant optical film material for polarizer:
[0045] 0.1 kg of dimethyl 2-hydroxyterephthalate and 0.045 kg of 2-hydroxyethylamine were dissolved in 0.9 kg of tetrahydrofuran, and then 0.18 kg of triphenylphosphine and 0.1 kg of diisopropyl azodicarboxylate were added, and the mixture was reacted at 25° C. for 12 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain an amino-terminated dimethyl terephthalate derivative;
[0046] 0.1 kg of terminal amino dimethyl terephthalate derivative and 0.045 kg of propyl isocyanate were added to 1 kg of acetone, stirred and dissolved, and then 0.008 kg of dibutyltin dilaurate was added, and stirred and reacted at 40°C for 12 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the obtained residue was washed twice with deionized water, added to 0.9 kg of methanol, dissolved, and then 0.07 kg of sodium hydroxide was added thereto, and reacted at 30°C for 12 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and the residue was washed twice with deionized water and dried to obtain a terephthalic acid derivative;
[0047] 0.1 kg of terephthalic acid derivative and 0.029 kg of ethylene glycol were added to 0.8 kg of tetrahydrofuran, and then 0.04 kg of 4-dimethylaminopyridine and 0.05 kg of 1-ethyl-(3-dimethylaminopropyl)carbodiimide were added, and the reaction was carried out at 25°C for 12 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with deionized water and dried to obtain a high temperature resistant optical film material for polarizers.
[0048] The high temperature resistant optical film material for polarizer prepared in Examples 1 to 6 was melt extruded and biaxially stretched to form a film, and the performance thereof was tested, and a commercially available optical PET film was used as a comparative example. The tensile performance was tested according to the method in GB / T 25255-2010, the haze and transmittance were tested according to the method in GB / T 2410-2008, the thickness was tested according to the method in GB / T 33399-2016, and the birefringence was tested according to the method in GB / T 28609-2012.
[0049] Table 1 Performance parameter results of optical thin film materials
[0050]
[0051] It can be seen from the results in Table 1 that the high temperature resistant optical film material for polarizer prepared by the present invention has a higher glass transition temperature and higher high temperature resistance than that of the comparative example. It also has high light transmittance and low haze, and is highly flexible. It has broad application prospects as an optical film material for manufacturing polarizers.
[0052] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.
Claims
1. A high temperature resistant optical film material for polarizer, characterized in that: Its structural formula is as follows: 。 2. The method for preparing the high temperature resistant optical film material for polarizer according to claim 1, characterized in that: The following steps are involved: 1) dissolving dimethyl 2-hydroxyterephthalate and 2-hydroxyethylamine in an organic solvent 1, then adding triphenylphosphine and diisopropyl azodicarboxylate, reacting at 25-50° C. for 12-24 hours. After the reaction is completed, removing the solvent by distillation under reduced pressure, washing the obtained residue with deionized water for 2-3 times, and drying to obtain an amino-terminated dimethyl terephthalate derivative; 2) adding the terminal amino dimethyl terephthalate derivative and propyl isocyanate prepared in step 1) to organic solvent 2, stirring to dissolve, then adding dibutyltin dilaurate, stirring to react at 25-40° C. for 8-12 hours, after the reaction is completed, removing the solvent by distillation under reduced pressure, washing the obtained residue with deionized water 2-3 times, adding it to an alcohol organic solvent, dissolving it, then adding a base thereto, reacting at 30-80° C. for 12-24 hours, after the reaction is completed, removing the solvent by distillation under reduced pressure, washing the residue with deionized water 2-3 times, and drying to obtain a terephthalic acid derivative; 3) Add the terephthalic acid derivative and ethylene glycol prepared in step 2) to the organic solvent 3, then add 4-dimethylaminopyridine and 1-ethyl-(3-dimethylaminopropyl)carbodiimide, and react at 25-40° C. for 12-24 hours. After the reaction is completed, filter and wash the filter cake with deionized water for 2-3 times, and dry to obtain a high temperature resistant optical film material for polarizers.
3. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: In step 1), the organic solvent 1 is tetrahydrofuran, acetonitrile or acetone.
4. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The mass ratio of dimethyl 2-hydroxyterephthalate, 2-hydroxyethylamine, organic solvent 1, triphenylphosphine and diisopropyl azodicarboxylate in step 1) is 1:0.3-0.5:5-10:1.2-1.8:1-1.
5.
5. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The organic solvent 2 in step 2) is dichloromethane, chloroform, acetone, tetrahydrofuran or ether.
6. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The alcohol organic solvent in step 2) is methanol, ethanol or isopropanol.
7. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The base in step 2) is potassium hydroxide or sodium hydroxide.
8. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The mass ratio of the terminal amino dimethyl terephthalate derivative, propyl isocyanate, organic solvent 2, dibutyltin dilaurate, alcohol organic solvent and base in step 2) is 1:0.35~0.5:5~10:0.02~0.1:5~10:0.3~0.
8.
9. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The organic solvent 3 in step 3) is acetone, acetonitrile, tetrahydrofuran, benzene or toluene.
10. The method for preparing a high temperature resistant optical film material for a polarizer according to claim 2, characterized in that: The mass ratio of the terephthalic acid derivative, ethylene glycol, organic solvent 3, 4-dimethylaminopyridine and 1-ethyl-(3-dimethylaminopropyl)carbodiimide in step 3) is 1:0.2~0.3:5~10:0.04~0.4:0.5~1.5.
Citation Information
Patent Citations
Self-healing liquid crystalline elastomer based on chitin-type liquid crystal and preparation method of self-healing liquid crystalline elastomer
CN104530315A
Optical polyester film and preparation method thereof
CN114103364A