Preformed blood sealing plug and preparation method thereof
By reacting aldehyde-based polyethylene glycol and amino polyethylene glycol to form a Schiff base bond, and combining it with a third component to adjust the degradation cycle, the problem of uncertainty in the safety and degradation cycle of existing blood vessel sealing materials is solved, and a safe The preformed blood sealing plug with high resistance and moderate degradation achieves the effectiveness of blood vessel sealing and rapid degradation effect.
Patent Information
- Application Number
- CN202410889276.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-03
AI Technical Summary
There are uncertainties in the degradation cycle of existing blood vessel sealing materials, which may cause the blood sealing plug to stay in the body for too long or have poor sealing effect, and the harmful by-product N-hydroxysuccinimide is generated, which affects safety. .
The Schiff base bond is formed through the reaction of aldehyde-based polyethylene glycol and amino polyethylene glycol, combined with the third component aldehyde-based polyethylene glycol to adjust the degradation cycle, and cross-linked and freeze-dried under low temperature conditions to prepare a preformed blood seal. Stopper, control the molar ratio of aldehyde group/amino group and solute mass fraction to ensure the safety and moderate degradation cycle of the blood sealing stopper.
A preformed blood-sealing plug with higher safety and moderate degradation cycle has been achieved, which avoids the generation of harmful by-products and ensures the effectiveness and rapid degradation of the blood-sealing plug during the blood vessel blocking process.
Smart Images

Figure CN118420916B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedicine, and in particular relates to a preformed blood sealing plug and a preparation method thereof. Background Art
[0002] Vascular closure devices are used during minimally invasive cardiovascular diagnosis and interventional surgery. The puncture site will produce a cavity, which must be closed after the surgery to prevent blood loss. Vascular closure devices are required for coronary intervention, neurointervention, peripheral artery intervention and tumor intervention.
[0003] In the prior art, there is a method of producing gel by reacting polyethylene glycol succinimidyl ester with polyethylene glycol amino groups, but this method will produce N-hydroxysuccinimide, which is toxic and will affect the blocking performance and cause local tissue inflammation. In order to avoid the generation of harmful byproducts, a gel produced by the reaction of polyethylene glycol aldehyde group and polyethylene glycol amino group can be used. The only byproduct is water, which is safe to use, and the Schiff base formed between the two substances has antibacterial and anti-inflammatory effects.
[0004] Although the use of polyethylene glycol aldehyde and polyethylene glycol amino groups to generate gel can solve the problem of safety in use, the length of the degradation cycle of blood plugs will directly affect whether the blood plugs can become qualified plugging materials. If the degradation cycle of the blood plug is too long, it is easy for the blood plug to stay in the body for too long, resulting in unnecessary side effects; while if the degradation cycle is too short, it is easy to lead to poor plugging effect, and the blood plug will be completely decomposed before the blood vessel is completely closed. Summary of the invention
[0005] The invention provides a preformed blood sealing plug and a preparation method thereof. The blood sealing plug has the characteristics of safe use and moderate degradation period.
[0006] The preformed blood-sealing plug provided by the present invention is mainly obtained by reacting a first component, aldehyde polyethylene glycol, and a second component, amino polyethylene glycol, to form a Schiff base bond, wherein the second component, amino polyethylene glycol, is selected from any one or more of formula I, formula II, and formula III:
[0007]
[0008] The first component aldehyde polyethylene glycol is any one or more selected from the substances consisting of formula V, formula VI and formula VII and group R:
[0009]
[0010] Wherein, the group R is:
[0011] Formula a Or formula b , m=3~8,
[0012] The aldehyde group at the end of the first component aldehyde polyethylene glycol reacts with the amino group at the end of the second component amino polyethylene glycol to form the Schiff base bond. The molecular weights of the first component aldehyde polyethylene glycol and the second component amino polyethylene glycol are both 10k-20k Da.
[0013] Furthermore, the third component is aldehyde-based polyethylene glycol, and the third component aldehyde-based polyethylene glycol is selected from any one or more of formula VIII, formula IX and formula X:
[0014]
[0015] The aldehyde group at the end of the aldehyde polyethylene glycol of the third component reacts with the amino group at the end of the amino polyethylene glycol of the second component to form a Schiff base bond, and the molecular weight of the aldehyde polyethylene glycol of the third component is 10k-20k Da.
[0016] Furthermore, the first component aldehyde polyethylene glycol is selected as formula VI, the group R is selected as formula b, m is selected as 3, and the molecular weight is 10k Da, the second component amino polyethylene glycol is selected as formula III, and the molecular weight is 20k Da, and the third component aldehyde polyethylene glycol is selected as formula IX, and the molecular weight is 10k Da.
[0017] Furthermore, the mass ratio of the first component aldehyde-based polyethylene glycol / the third component aldehyde-based polyethylene glycol / the second component amino polyethylene glycol is 1:1:2.
[0018] Furthermore, the first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as formula b, m is selected as 3, and is selected as formula VI, group R is selected as formula a, the molecular weight of the first component aldehyde polyethylene glycol is 10k Da, the second component amino polyethylene glycol is selected as formula III, with a molecular weight of 20k Da, and the third component aldehyde polyethylene glycol is selected as formula IX, with a molecular weight of 10k Da.
[0019] Furthermore, the mass ratio of the first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as b, m is selected as 3 / the first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as a / the third component aldehyde polyethylene glycol / the second component amino polyethylene glycol is 1:1:1:3.
[0020] The present invention further provides a method for preparing the preformed blood sealing plug, comprising the following steps:
[0021] Fully dissolving the first component aldehyde polyethylene glycol and the second component amino polyethylene glycol in a buffered salt solution to prepare a first solution containing the first component aldehyde polyethylene glycol and a second solution containing the second component amino polyethylene glycol, and mixing the two solutions to form a mixed solution;
[0022] The obtained mixed solution is placed in a sealed tube or applied on release paper, cross-linked at -20°C to 0°C for 12 to 36 hours, and then freeze-dried and demolded.
[0023] Furthermore, the mixed solution also includes a third component, aldehyde polyethylene glycol, which is fully dissolved in the buffered salt solution to form a third solution containing the third component, aldehyde polyethylene glycol, and the third solution containing the third component, aldehyde polyethylene glycol, is mixed with the first solution containing the first component, aldehyde polyethylene glycol, and the second solution containing the second component, amino polyethylene glycol.
[0024] Furthermore, the solute mass fractions of the first solution containing the first component aldehyde polyethylene glycol, the second solution containing the second component amino polyethylene glycol, and the third solution containing the third component aldehyde polyethylene glycol are 5% to 10%.
[0025] Furthermore, in the mixed solution, the molar ratio of aldehyde group / amino group is 1:0.25-4.
[0026] The technical solutions provided by the embodiments of this specification may have the following beneficial effects:
[0027] The present invention uses aldehyde polyethylene glycol and amino polyethylene glycol to form a Schiff base bond, thereby avoiding the generation of harmful byproduct N-hydroxysuccinimide in the prior art, making the use of the preformed blood sealing plug safer;
[0028] In addition, the first component of the present invention, aldehyde-based polyethylene glycol, makes the degradation period of the preformed blood sealing plug moderate by adding specific groups.
[0029] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present specification. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 It is the swelling days-swelling multiples graph of the blood plugs No. 1-8 in the in vitro experiment in Table 2;
[0031] Figure 2 It is the swelling days-swelling multiples diagram of the blood plugs No. 9-16 in the in vitro experiment in Table 2;
[0032] Figure 3 This is an electron microscope scan of the blood sealant No. 1 in Table 5;
[0033] Figure 4 This is an electron microscope scanning image of the blood sealant No. 4 in Table 5. DETAILED DESCRIPTION
[0034] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0035] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0036] The present invention relates to a preformed blood-sealing plug and a preparation method thereof. The blood-sealing plug is mainly obtained by reacting a first component, aldehyde polyethylene glycol, with a second component, amino polyethylene glycol to form a Schiff base bond. The reaction formula is as follows:
[0037]
[0038] The aldehyde group at the end of the first component forms a Schiff base bond with the amino group at the end of the second component.
[0039] The second component aminopolyethylene glycol can be selected from any one or more of formula I, formula II and formula III,
[0040]
[0041] The first component aldehyde polyethylene glycol can be selected from any one or more of the substances consisting of formula V, formula VI and formula VII and group R:
[0042]
[0043] Wherein, the group R is:
[0044] Formula a Or formula b , m=3~8.
[0045] For example, when the first component aldehyde polyethylene glycol is selected as formula VI, R is b, and m is 3, its molecular formula is:
[0046]
[0047] When the first component aldehyde polyethylene glycol is selected as formula VI, and R is a, its molecular formula is:
[0048]
[0049] For blood sealing plugs, at least one substance type of the first component aldehyde polyethylene glycol and the second component amino polyethylene glycol can be selected, or multiple substances can be selected. That is, for the first component aldehyde polyethylene glycol, a single substance can be selected, or multiple substances with different arm numbers and different groups can be selected.
[0050] The reaction components of the blood-sealing plug further include a third component, aldehyde-based polyethylene glycol, which can be selected from any one or more of Formula VIII, Formula IX and Formula X:
[0051]
[0052] Adding the third component, aldehyde-based polyethylene glycol, to the blood-sealing plug mainly plays the role of regulating the degradation cycle. Because under the same experimental conditions, the degradation cycle of the third component, aldehyde-based polyethylene glycol, with the same number of arms is shorter than that of the first component, aldehyde-based polyethylene glycol, in order to reduce the degradation cycle of the blood-sealing plug generated by the first component, aldehyde-based polyethylene glycol, and the second component, amino polyethylene glycol, the third component, aldehyde-based polyethylene glycol, can be added to the reaction components.
[0053] In the present invention, polyethylene glycol is used as a molecular skeleton. Generally, the molecular weight of polyethylene glycol as an in vivo implant is usually above 5k Da, with a maximum value of 40k Da, because polyethylene glycol will be excreted from the body through the kidneys in the form of metabolites or original polymers. Low molecular weight polyethylene glycol is easily converted into toxic substances by alcohol dehydrogenase in the body and has nephrotoxicity; while high molecular weight polyethylene glycol is directly excreted from the body in the form of original polymers, which is basically non-toxic and has high safety. However, as the molecular weight increases, the circulation time of polyethylene glycol in the body becomes longer, and it is not easy to be excreted from the body by the kidneys, so the molecular weight of the preferred reaction component is selected to be 10k-20k Da.
[0054] To prepare the blood-sealing plug involved in the present invention, the selected first component aldehyde polyethylene glycol and the second group amino polyethylene glycol need to be dissolved in a buffer solution respectively to obtain a first solution containing the first component aldehyde polyethylene glycol and a second solution containing the second component amino polyethylene glycol with a certain solute mass fraction. If the reaction components also include a third component aldehyde polyethylene glycol, a third solution containing the third component aldehyde polyethylene glycol needs to be prepared. After the reaction components are fully dissolved in the buffer solution, the reactants are mixed in proportion to control the molar ratio of the aldehyde group and the amino group in the mixed solution.
[0055] The mixed solution is poured into a sealed tube or applied on release paper, and reacted and cross-linked for 12 to 36 hours at -20°C to 0°C, and then freeze-dried and demolded to obtain the blood sealing plug of the present invention.
[0056] In a specific experimental process, the buffer solution can be a neutral buffer, an acidic buffer or an alkaline buffer.
[0057] In this experiment, the cross-linking reaction was carried out at freezing temperature so that the water in the reaction product condensed into ice, which was more conducive to the formation of pores in the cross-linked network.
[0058] Example 1
[0059] Weigh 50 mg of the first component aldehyde polyethylene glycol of different components and fully dissolve it in 950 mg of neutral phosphate buffer as solution A; weigh 50 mg of the second component amino polyethylene glycol and fully dissolve it in 950 mg of neutral phosphate buffer as solution B; mix solutions A and B in proportion so that the molar ratio of aldehyde to amino in the mixed solution is 1:1, pour the mixed solution into a silicone tube, seal it, and perform low-temperature cross-linking at -20°C for 36 hours, and then freeze-dry and remove the membrane.
[0060] Table 1 Effect of different carbon chain lengths on degradation cycle
[0061]
[0062] The experimental results of Example 1 show that: for the first component aldehyde polyethylene glycol using the functional group selection formula b, when m is less than or equal to 2, the degradation period is very short, when m is equal to 3, the degradation period suddenly changes, and when m is 3-8, the degradation period of the blood sealing plug does not change significantly.
[0063] Example 2
[0064] A certain mass of the first aldehyde polyethylene glycol solution was weighed and fully dissolved in a neutral phosphate buffer to form a solution A with a certain mass fraction. A certain mass of the second amino polyethylene glycol was weighed and fully dissolved in a neutral phosphate buffer to form a solution B with a certain mass fraction. Solutions A and B were mixed in proportion so that the molar ratio of aldehyde group / amino group in the mixed solution was 1:1. The mixed solution was applied on release paper, and low-temperature cross-linking was carried out at -20°C for 12 hours, and then freeze-dried and demolded.
[0065] Table 2
[0066]
[0067] The experimental data in Table 2 show that as the mass fraction of the solute increases, the degradation period of the blood-sealing plug gradually increases. The mass fraction of the solute affects the degradation period on the one hand, and the swelling time of the blood-sealing plug on the other hand. As the mass fraction of the solute increases, the cross-linking density of the blood-sealing plug will gradually increase, and the swelling time will also increase. As a qualified blood-sealing plug product, it needs to have the ability to quickly absorb blood, swell and seal the wound, so the swelling time cannot be too long. Figure 1 and Figure 2 They are the swelling rates of blood-sealing plugs No. 1-8 and 9-16 in Table 2 in the in vitro experiment. It can be clearly seen from the figure that in the early stage of swelling, that is, the part with the largest slope in the front section of the figure, as the solute mass fraction increases, the swelling rate of the blood-sealing plug in a short time gradually decreases. In order to make the blood-sealing plug have a faster swelling rate, the preferred solute mass fraction is 5%-10%.
[0068] Comparing the numbers 9 to 12 and 17 to 20 in Table 2, it can be seen that with the increase of the molecular weight of the single arm, the degradation period of the blood sealing plug gradually decreases.
[0069] Example 3
[0070] A certain mass of the first aldehyde polyethylene glycol solution was weighed and fully dissolved in a neutral phosphate buffer to form a 5% mass fraction A solution. A certain mass of the second amino polyethylene glycol was weighed and fully dissolved in a neutral phosphate buffer to form a 5% mass fraction B solution. Solutions A and B were mixed in proportion to form mixed solutions with different aldehyde / amino molar ratios. The mixed solution was poured into a silicone tube and sealed, and low-temperature cross-linked at -20°C for 36 hours, and then freeze-dried and de-membraned.
[0071] Table 3 Effect of aldehyde / amino molar ratio on degradation cycle
[0072]
[0073] According to the experimental data of Example 3, as the aldehyde group / amino group molar ratio increases, the degradation cycle shows a trend of increasing first and then decreasing. When the aldehyde group / amino group ratio is near 1, the degradation cycle is the longest. It can be understood that when the aldehyde group / amino group ratio is 1, all aldehyde groups react with amino groups to form Schiff base bonds, and the cross-linking points are the most; when the aldehyde group / amino group ratio is 4, only 25% of the aldehyde groups react with amino groups. For this example, the first component aldehyde group polyethylene glycol is a four-arm component, that is, only one of the four arms reacts, and the cross-linking points are less than when the aldehyde group / amino group ratio is 1. The number of cross-linking points will directly affect the degradation cycle, and the more cross-linking points, the longer the time required for degradation. But from the overall point of view, with the change of the aldehyde group / amino group molar ratio, the degradation cycle of the blood sealing plug does not change significantly. Because when the molar ratio of the aldehyde group / amino group differs too much, it is easy to cause a waste of raw materials. Therefore, it is preferred that the ratio range of the two is 1:0.25~4.
[0074] Example 4
[0075] A certain mass of a first aldehyde polyethylene glycol solution was weighed and fully dissolved in a neutral phosphate buffer to form a 5% mass fraction A solution. A certain mass of a second amino polyethylene glycol was weighed and fully dissolved in a neutral phosphate buffer to form a 5% mass fraction B solution. Solutions A and B were mixed in proportion to form a mixed solution so that the molar ratio of aldehyde groups to amino groups in the mixed solution was 1:1. The mixed solution was applied on a release paper and subjected to low-temperature crosslinking at -20°C for 36 hours, followed by freeze-drying and film removal.
[0076] Table 4
[0077]
[0078] Example 5
[0079] A certain mass of the first component aldehyde polyethylene glycol or the third component aldehyde polyethylene glycol is fully dissolved in a neutral phosphate buffer to form a 5% mass fraction A solution, a certain mass of the second amino polyethylene glycol is fully dissolved in a neutral phosphate buffer to form a 5% mass fraction B solution, the A and B solutions are mixed in proportion to form a mixed solution so that the molar ratio of the aldehyde group / amino group in the mixed solution is 1:1, the mixed solution is applied on a release paper, and low-temperature cross-linking is carried out at -20°C for 36 hours, and then freeze-dried and demolded.
[0080] Table 5
[0081]
[0082] The experimental data combined with Example 4 and Example 5 show that when the raw material components of the blood-sealing plug are replaced with components with a short degradation period or a long degradation period, the degradation period of the blood-sealing plug will be shortened or lengthened accordingly. As shown in Table 4, the degradation period of Formula IX is the shortest, followed by Formula VI, R=a, and finally Formula VI, R=b, m=3. As shown in No. 1-2 of Table 5, the degradation period of the blood-sealing plug is lengthened by replacing the raw material Formula VI, R=b, m=3 with Formula VI, R=a. The same can be obtained by comparing No. 1 and 3 or 2 and 3. In addition, when the proportion of the blood-sealing plug components changes, the degradation period of the blood-sealing plug will also change. If the components with a long degradation period increase, the corresponding degradation period will also increase, and vice versa.
[0083] In the embodiment of Table 5, the preferred examples are No. 1 and 4. In this case, the degradation period of the blood plug is within 20 to 30 days, which can meet the purpose of blood vessel occlusion and achieve the effect of timely degradation. Figure 3 , Figure 4 As shown, according to the electron microscope scanning images of the two, the pores of these two blood sealing plugs are large and relatively uniform, and the swelling effect is better.
Claims
1. A preformed blood sealing plug, characterized in that: It is mainly obtained by reacting the first component, aldehyde polyethylene glycol, and the second component, amino polyethylene glycol, to form a Schiff base bond, wherein the second component, amino polyethylene glycol, is selected from any one or more of formula I, formula II and formula III: The first component aldehyde polyethylene glycol is any one or more selected from the substances consisting of formula V, formula VI and formula VII and group R: Wherein, the group R is: Formula a Or formula b , m=3~8, The aldehyde group at the end of the first component aldehyde polyethylene glycol reacts with the amino group at the end of the second component amino polyethylene glycol to form the Schiff base bond, and the molecular weights of the first component aldehyde polyethylene glycol and the second component amino polyethylene glycol are both 10k~20k Da; It also includes a third component, aldehyde-based polyethylene glycol, which is selected from any one or more of Formula VIII, Formula IX and Formula X: The aldehyde group at the end of the aldehyde polyethylene glycol of the third component reacts with the amino group at the end of the amino polyethylene glycol of the second component to form a Schiff base bond, and the molecular weight of the aldehyde polyethylene glycol of the third component is 10k-20k Da.
2. The preformed blood sealing plug according to claim 1, characterized in that: The first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as formula b, m is selected as 3, and the molecular weight is 10k Da, the second component amino polyethylene glycol is selected as formula III, and the molecular weight is 20k Da, and the third component aldehyde polyethylene glycol is selected as formula IX, and the molecular weight is 10k Da.
3. The preformed blood sealing plug according to claim 2, characterized in that: The mass ratio of the first component aldehyde polyethylene glycol: the third component aldehyde polyethylene glycol: the second component amino polyethylene glycol is 1:1:
2.
4. The preformed blood sealing plug according to claim 1, characterized in that: The first component aldehyde polyethylene glycol is formula VI in which group R is selected as formula b and m is selected as 3, and formula VI in which group R is selected as formula a. The molecular weight of the first component aldehyde polyethylene glycol is 10k Da, the second component amino polyethylene glycol is selected as formula III, with a molecular weight of 20k Da, and the third component aldehyde polyethylene glycol is selected as formula IX, with a molecular weight of 10k Da.
5. The preformed blood sealing plug according to claim 4, characterized in that: The first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as b, and m is selected as 3: the first component aldehyde polyethylene glycol is selected as formula VI, group R is selected as a: the third component aldehyde polyethylene glycol: the second component amino polyethylene glycol has a mass ratio of 1:1:1:
3.
6. A method for preparing the preformed blood sealing plug according to any one of claims 1 to 5, characterized in that: The following steps are involved: Fully dissolving the first component aldehyde polyethylene glycol and the second component amino polyethylene glycol in a buffered salt solution to prepare a first solution containing the first component aldehyde polyethylene glycol and a second solution containing the second component amino polyethylene glycol, and mixing the two solutions to form a mixed solution; The mixed solution also includes a third component, aldehyde-based polyethylene glycol, which is fully dissolved in the buffered salt solution to form a third solution containing the third component, aldehyde-based polyethylene glycol, and the third solution containing the third component, aldehyde-based polyethylene glycol, is mixed with the first solution containing the first component, aldehyde-based polyethylene glycol, and the second solution containing the second component, amino polyethylene glycol; The obtained mixed solution is placed in a sealed tube or applied on release paper, cross-linked at -20°C to 0°C for 12 to 36 hours, and then freeze-dried and demolded.
7. The method for preparing a preformed blood sealing plug according to claim 6, characterized in that: The solute mass fractions of the first solution containing the first component aldehyde polyethylene glycol, the second solution containing the second component amino polyethylene glycol, and the third solution containing the third component aldehyde polyethylene glycol are 5% to 10%.
8. The method for preparing the preformed blood sealing plug according to claim 7, characterized in that: In the mixed solution, the molar ratio of aldehyde group:amino group is 1:0.25-4.
Citation Information
Patent Citations
Injectable hydrogel and preparation method and application thereof
CN107233629A
Scaffold material as well as preparation method and application thereof
CN111803454A
Degradable medical hydrogel
CN112225912A