Photoelectric composite cable for underwater buoy and preparation process thereof
By using the outer sheath of polyurethane, self-healing polyurethane prepolymer and nano-zinc oxide, combined with water-blocking sealant and aluminum-plastic composite cable technology, the problems of underwater wear and conductor leakage of optoelectronic composite cables are solved, achieving high Water resistance and wear resistance improve signal transmission capability and safety.
Patent Information
- Application Number
- CN202410512725.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Existing optoelectronic composite cables are prone to leakage of conductors due to wear or aging when used underwater, causing serious safety hazards, and lack sufficient waterproofing and wear resistance.
Polyurethane, self-healing polyurethane prepolymer and composite nano-zinc oxide are used as the base material of the outer sheath. The outer sheath is prepared by mixing and extruding with a twin-screw extruder, and the water-blocking sealant is filled between the cable core structures. The surface is wrapped with a braided layer, tensile reinforcement layer and braided fastening layer, combined with aluminum-plastic composite cable and silver-plated copper wire stranding technology to improve the cable's water resistance, wear resistance and signal transmission capabilities.
Significantly improve the mechanical strength, mechanical damage resistance and water resistance of the optoelectronic composite cable, so that it has good signal transmission capabilities underwater, and has the transmission functions of a variety of communication signal lines and high-voltage power supplies, enhancing safety and reliability.
Smart Images

Figure CN118430880B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite cables, in particular to an optoelectronic composite cable for underwater buoys and a preparation process thereof. Background Art
[0002] Optical-electric composite cable is a cable that integrates optical fiber and transmission line. It has the characteristics of optical-electric transmission and is used to solve the problems of broadband access, equipment power consumption and signal transmission. It is widely used in the power supply of long-distance communication power supply system and short-distance communication system. With the progress of society, the application places of optical-electric composite cable are also constantly expanding, such as laying under the sea and in water. As a result, the performance requirements of optical-electric composite cable are becoming more and more stringent.
[0003] During the use of optoelectronic composite cables, if the optoelectronic composite cables are worn or aged, the conductors will leak out. If they are soaked in water, serious safety hazards will occur. Therefore, it is of practical significance to improve the waterproof and wear resistance of optoelectronic composite cables. Summary of the invention
[0004] The purpose of the present invention is to provide a high-strength wear-resistant polyurethane composite plate and a processing technology thereof to solve the problems in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A photoelectric composite cable for an underwater buoy comprises a cable core, wherein the structure of the cable core comprises an optical cable element, a water ingress detection line, a 48V power line, an RS422 data line, a 220V power line, and a drainage line, and water-blocking sealant is filled between the various structures of the cable core; the outer surface of the cable core is wrapped with a braided layer, a tensile reinforcement layer, a braided fastening layer, and an outer sheath in sequence.
[0007] Furthermore, the outer surfaces of the optical cable components, water ingress detection lines, 48V power lines, RS422 data lines, and 220V power lines are coated with aluminum-plastic composite cables.
[0008] Furthermore, the optical cable element is composed of an optical fiber and an armor layer on the surface of the optical fiber. The armor layer on the surface of the optical fiber is a seamless stainless steel tube with a diameter of 1.3 mm; the braided layer and the tensile reinforcement layer are both aramid fiber layers; and the braided fastening layer is a twisted water-blocking aramid layer.
[0009] Furthermore, the aramid fiber layer is woven from aramid fibers.
[0010] Furthermore, the twisted water-blocking aramid layer is formed by twisting the aramid fibers in the Z direction at 90 degrees to form a twisted rope armor.
[0011] Furthermore, the 48V power cord is made of 17-21 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the water inlet detection line and RS422 data line are made of 6-8 0.25mm silver-plated copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with ethylene tetrafluoroethylene copolymer; the 220V power cord is made of 17-21 0.31mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the drainage line is made of 17-21 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant.
[0012] Furthermore, the water-blocking sealant is a silicone-based sealant or a chlorobutyl-based sealant.
[0013] Furthermore, a process for preparing an optoelectronic composite cable for an underwater buoy comprises the following steps:
[0014] S1: Mix polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide, put them into a twin-screw extruder for mixing and extrusion, pelletize and dry to obtain an outer sheath base material, and extrude the outer sheath base material in a semi-extrusion manner to obtain an outer sheath;
[0015] S2: Assemble the structure of the cable core, fill water-blocking sealant between the various structures of the cable core, and then wrap the braided layer, the tensile reinforcement layer, the braided fastening layer, and the outer sheath in sequence on the outer surface to obtain an optoelectronic composite cable for underwater buoys.
[0016] Furthermore, in parts by weight, the outer sheath base material comprises 32-36 parts of polyurethane, 15-27 parts of self-repairing polyurethane prepolymer, and 1-5 parts of composite nano zinc oxide.
[0017] Furthermore, the preparation of the self-repairing polyurethane prepolymer comprises the following steps:
[0018] 1) Mix trioxymethylene, salicylaldehyde and glacial acetic acid, heat to 88-92°C, add concentrated sulfuric acid, keep warm for 22-24 hours, cool, pour into ice-water mixture and let stand overnight, wash, filter, wash with ether 2-3 times, recrystallize the precipitate with acetone 3-5 times to obtain 5,5'-methylenebissalicylaldehyde;
[0019] 2) Under nitrogen protection, the modified polysiloxane, anhydrous tetrahydrofuran and dichloromethane are mixed, the temperature is reduced to 0°C, isophorone diisocyanate is added, and the mixture is stirred for 5-6 hours. The temperature is increased to 18-25°C, 5,5'-methylenebissalicylaldehyde is added, and stirring is continued for 5-6 hours. Anhydrous sodium sulfate is added and filtered, and the mixture is distilled under reduced pressure. The mixture is dissolved in anhydrous tetrahydrofuran, triethylenediamine and diphenylmethane diisocyanate are added, and the mixture is stirred for 15-20 minutes under nitrogen protection, rotary evaporated, transferred to a tetrafluoroethylene mold, and dried to obtain a self-healing polyurethane prepolymer.
[0020] Further, the preparation of the modified polysiloxane comprises the following steps:
[0021] (1) Under a nitrogen atmosphere, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethyltetraenylcyclotetrasiloxane are mixed, the temperature is raised to 88-92°C and kept for 20-30 minutes, the temperature is raised to 108-112°C, tetramethylammonium hydroxide is added, the temperature is kept for 4-6 hours, the temperature is raised to 130°C and kept for 25-30 minutes, and the pressure is reduced for 2-3 hours to obtain amino-terminated vinyl polysiloxane;
[0022] (2) Under a nitrogen atmosphere, 4-vinylbenzene boronic acid, anhydrous sodium sulfate and tetrahydrofuran are mixed, kept at 48-52° C. for 23-24 hours, rotary evaporated and dried to obtain tri(vinylbenzene)boroxane;
[0023] (3) Mix the amino-terminated vinyl polysiloxane with octadecyl methacrylate and tetrahydrofuran, add tri(vinylbenzene)boroxane, benzoyl peroxide and 2,2-azobisisobutyronitrile, stir at 18-25°C for 11-12h, rotary evaporate, hot press at 160°C for 3min, dissolve in toluene, precipitate with petroleum ether, repeat the precipitation 3-5 times, and dry to obtain modified polysiloxane.
[0024] Furthermore, the preparation of composite nano zinc oxide includes the following steps: mixing nano zinc oxide and toluene, stirring at 78-82°C for 8-10 minutes, adding dodecyl trimethoxy silane, continuing to keep warm for 8-9 hours, adding 3-glycidyloxypropyl trimethoxy silane, continuing to keep warm for 7-8 hours, centrifuging, ultrasonically cleaning with ethanol, centrifuging, drying, and grinding to obtain composite nano zinc oxide.
[0025] Beneficial effects of the present invention:
[0026] The present invention provides an optoelectronic composite cable for underwater buoys and a preparation process thereof. The prepared optoelectronic composite cable has good mechanical strength, mechanical damage resistance, wear resistance and water resistance, so that it has good large-capacity optical signal transmission capacity and data signal transmission capacity under the premise of meeting watertight performance, and at the same time has various communication signal lines such as telephone transmission lines and water ingress detection lines, as well as various comprehensive signals and electric energy such as 220V high-voltage boat power and 48V lithium battery power supply.
[0027] In order to make the optoelectronic composite cable soft and reliable during use, the conductor of the optoelectronic composite cable in the present invention adopts a multi-strand twisted structure, so as to improve the vibration and impact resistance and the continuity of repeated bending; in order to improve its longitudinal watertightness, a silicone-based or chlorobutyl-based water-blocking sealant is filled in the twisting process; in order to give the water inlet detection line and RS422 data line the characteristics of weldability and signal transmission, a process of twisting silver-plated copper wire and filling water-blocking sealant is adopted; the aramid fiber is twisted and then armored, which effectively reduces the outer diameter of the product and makes its appearance round; the electric core component in the present invention adopts a combination of a wrapped aluminum-plastic composite cable and a drainage wire as a shielding form of the optoelectronic composite cable, which effectively reduces the outer diameter of the optoelectronic composite cable and reduces the weight.
[0028] In order to give the optoelectronic composite cable excellent water resistance, wear resistance and mechanical damage resistance, the present invention selects polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide as the outer sheath base material to prepare the outer sheath of the optoelectronic composite cable;
[0029] In order to improve the wear resistance and water resistance of the outer sheath, modified polysiloxane was introduced into the self-healing polyurethane prepolymer. First, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethyltetraenylcyclotetrasiloxane were used under the action of tetramethylammonium hydroxide as a catalyst to prepare amino-terminated vinyl polysiloxane. The monomer formed by dehydration of 4-vinylbenzeneboronic acid and amino-terminated vinyl polysiloxane were copolymerized with hydrophobic octadecyl methacrylate through free radical polymerization to prepare modified polysiloxane having a BO six-membered ring dynamic cross-linking network and long-chain alkane groups and amino groups. The modified polysiloxane was used as a raw material to prepare a self-healing polyurethane prepolymer, which can be quickly self-healed at room temperature, water environment and low temperature, thereby greatly improving the water resistance and wear resistance of the protective sheath.
[0030] In the preparation of the self-healing polyurethane prepolymer, bio-based salicylaldehyde is used as a raw material to prepare 5,5'-methylene disalicylicaldehyde with trioxymethylene, and 5,5'-methylene disalicylicaldehyde and isophorone diisocyanate are gradually polymerized with modified polysiloxane, and then 5,5'-methylene disalicylicaldehyde is cross-linked with diphenylmethane diisocyanate to form a phenyl carbamate dynamic bond and a BO six-membered ring dynamic cross-linking network to form a dynamic self-healing silicone elastomer with high mechanical strength, good hydrophobicity, multiple active sites, high compatibility, and high wear resistance. When mixed with other raw materials, it is easy to improve the compatibility; and the introduction of silicon and the complexity of the Si-O-Si cross-linking structure help to improve the flame retardancy of the protective cover;
[0031] Nano zinc oxide is introduced as a filler in the preparation of the protective cover to further improve the water resistance and wear resistance of the protective cover. In order to improve the uniformity of the dispersion of nano zinc oxide in polyurethane, the nano zinc oxide is modified. Super hydrophobic nano zinc oxide with good thermal stability and high dispersibility is prepared in a toluene system by dual modification with dodecyltrimethoxysilane and 3-glycidyloxypropyltrimethoxysilane. A protective cover with a super hydrophobic surface is prepared. At the same time, there is a metal-coordination bond between the composite nano zinc oxide and the self-healing polyurethane prepolymer, which is beneficial to further improve its self-healing rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0033] Figure 1 It is a schematic structural diagram of the optoelectronic composite cable of the present invention;
[0034] 1-optical cable element, 2-water inlet detection line, 3-48V power line, 4-RS422 data line, 5-220V power line, 6-drainage line, 7-telephone line, 8-braided layer, 9-tensile reinforcement layer, 10-braided fastening layer, 11-outer sheath. DETAILED DESCRIPTION
[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that if the embodiments of the present invention involve directional indications such as up, down, left, right, front, and back, the directional indication is only used to explain a specific posture such as the relative position relationship between the components, the movement status, etc. If the specific posture changes, the directional indication will also change accordingly. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.
[0037] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0038] Embodiment 1: A process for preparing an optoelectronic composite cable for an underwater buoy, comprising the following steps:
[0039] S1: polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide are mixed, put into a twin-screw extruder for mixing and extrusion, pelletized and dried to obtain an outer sheath base material, and the outer sheath base material is extruded in a semi-extrusion manner to obtain an outer sheath 11;
[0040] In terms of weight, the outer sheath base material is composed of 32 parts of polyurethane, 15 parts of self-repairing polyurethane prepolymer, and 1 part of composite nano zinc oxide;
[0041] The preparation of the self-repairing polyurethane prepolymer comprises the following steps:
[0042] 1) Mix 0.1mmol trioxymethylene, 0.4mmol salicylaldehyde and 25mL glacial acetic acid, heat to 88℃, add 0.25mL concentrated sulfuric acid, keep warm for 22h, cool, pour into ice-water mixture and let stand overnight, wash, filter, wash twice with ether, recrystallize the precipitate with acetone three times to obtain 5,5'-methylenebissalicylaldehyde;
[0043] 2) Under nitrogen protection, 0.5 g of modified polysiloxane, 5 mL of anhydrous tetrahydrofuran, and 5 mL of dichloromethane were mixed, cooled to 0 ° C, 0.3 mmol of isophorone diisocyanate was added, and stirred for 5 h. The temperature was raised to 18 ° C, 0.2 mmol of 5,5'-methylenebissalicylaldehyde was added, and stirring was continued for 5 h. Anhydrous sodium sulfate was added and filtered, and vacuum distillation was performed. The mixture was dissolved in 30 mL of anhydrous tetrahydrofuran, and 2 mg of triethylenediamine and 0.2 mmol of diphenylmethane diisocyanate were added. Under nitrogen protection, the mixture was stirred for 15 min, and the mixture was rotary evaporated, transferred to a tetrafluoroethylene mold, and dried to obtain a self-healing polyurethane prepolymer;
[0044] The preparation of the modified polysiloxane comprises the following steps:
[0045] (1) Under nitrogen atmosphere, 37.4 g of octamethylcyclotetrasiloxane, 19.4 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 34.2 g of tetramethyltetraenylcyclotetrasiloxane were mixed, heated to 88°C and kept warm for 30 min, heated to 108°C, 6.2 mg of tetramethylammonium hydroxide was added, and kept warm for 4 h, heated to 130°C and kept warm for 25 min, and reduced pressure was applied for 2 h to obtain amino-terminated vinyl polysiloxane;
[0046] (2) Under nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, kept at 48°C for 24 h, rotary evaporated, and dried to obtain tri(vinylbenzene)boroxane;
[0047] (3) 18 g of amino-terminated vinyl polysiloxane, 2 g of octadecyl methacrylate, and 30 mL of tetrahydrofuran were mixed, and 0.21 g of tri(vinylbenzene)boroxane, 52.5 mg of benzoyl peroxide, and 52.5 mg of 2,2-azobisisobutyronitrile were added. The mixture was stirred at 18°C for 12 h, rotary evaporated, hot-pressed at 160°C for 3 min, dissolved in toluene, precipitated with petroleum ether, and precipitated repeatedly for 3 times. The mixture was dried to obtain a modified polysiloxane.
[0048] The preparation of the composite nano zinc oxide comprises the following steps: mixing 2.5 g of nano zinc oxide and 100 mL of toluene, stirring at 78° C. for 10 min, adding 1 mL of dodecyl trimethoxy silane, continuing to keep warm for 8 h, adding 0.25 mL of 3-glycidyloxypropyl trimethoxy silane, continuing to keep warm for 7 h, centrifuging, ultrasonically cleaning with ethanol, centrifuging, drying, and grinding to obtain the composite nano zinc oxide;
[0049] S3: Assembling the structure of the cable core, filling water-blocking sealant between the various structures of the cable core, and then sequentially wrapping the braided layer 8, the tensile reinforcement layer 9, the braided fastening layer 10, and the outer sheath 11 on the outer surface to obtain an optoelectronic composite cable for underwater buoys;
[0050] The cable core structure consists of an optical cable element 1, a water inlet detection line 2, a 48V power line 3, an RS422 data line 4, a 220V power line 5, and a drainage line 6;
[0051] The outer surfaces of the optical cable element 1, the water inlet detection line 2, the 48V power line 3, the RS422 data line 4, and the 220V power line 5 are coated with an aluminum-plastic composite cable;
[0052] The optical cable element 1 is composed of an optical fiber and an armor layer on the surface of the optical fiber, and the armor layer on the surface of the optical fiber is a seamless stainless steel tube with a diameter of 1.3 mm;
[0053] The braided layer 8 and the tensile reinforcement layer 9 are both aramid fiber layers; the braided fastening layer 10 is a twisted water-blocking aramid fiber layer;
[0054] The aramid fiber layer is woven from aramid fibers; the twisted water-blocking aramid layer is formed by twisting the aramid fibers in the Z direction at 90 degrees to form a twisted rope armor;
[0055] The 48V power cord 3 is made of 17 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the water inlet detection line 2 and RS422 data line 4 are made of 6 0.25mm silver-plated copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with ethylene tetrafluoroethylene copolymer; the 220V power cord 5 is made of 17 0.31mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the drainage line 6 is made of 17 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant.
[0056] Embodiment 2: A process for preparing an optoelectronic composite cable for an underwater buoy, comprising the following steps:
[0057] S1: polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide are mixed, put into a twin-screw extruder for mixing and extrusion, pelletized and dried to obtain an outer sheath base material, and the outer sheath base material is extruded in a semi-extrusion manner to obtain an outer sheath 11;
[0058] In terms of weight, the outer sheath base material is composed of 34 parts of polyurethane, 17 parts of self-repairing polyurethane prepolymer, and 3 parts of composite nano zinc oxide;
[0059] The preparation of the self-repairing polyurethane prepolymer comprises the following steps:
[0060] 1) Mix 0.1mmol trioxymethylene, 0.4mmol salicylaldehyde and 25mL glacial acetic acid, heat to 90℃, add 0.25mL concentrated sulfuric acid, keep warm for 23h, cool, pour into ice-water mixture and let stand overnight, wash, filter, wash twice with ether, recrystallize the precipitate with acetone four times to obtain 5,5'-methylenebissalicylaldehyde;
[0061] 2) Under nitrogen protection, 0.5 g of modified polysiloxane, 5 mL of anhydrous tetrahydrofuran, and 5 mL of dichloromethane were mixed, cooled to 0 ° C, 0.3 mmol of isophorone diisocyanate was added, and stirred for 5.5 h. The temperature was raised to 20 ° C, 0.2 mmol of 5,5'-methylenebissalicylaldehyde was added, and stirring was continued for 5.5 h. Anhydrous sodium sulfate was added and filtered, and vacuum distillation was performed, and the mixture was dissolved in 30 mL of anhydrous tetrahydrofuran. 2 mg of triethylenediamine and 0.2 mmol of diphenylmethane diisocyanate were added, and the mixture was stirred for 18 min under nitrogen protection, and rotary evaporated, and the mixture was transferred to a tetrafluoroethylene mold and dried to obtain a self-healing polyurethane prepolymer;
[0062] The preparation of the modified polysiloxane comprises the following steps:
[0063] (1) Under nitrogen atmosphere, 37.4 g of octamethylcyclotetrasiloxane, 19.4 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 34.2 g of tetramethyltetraenylcyclotetrasiloxane were mixed, heated to 90°C and kept warm for 25 min, heated to 110°C, 6.2 mg of tetramethylammonium hydroxide was added, and kept warm for 5 h, heated to 130°C and kept warm for 28 min, and reduced pressure was applied for 2.5 h to obtain amino-terminated vinyl polysiloxane;
[0064] (2) Under nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, heated at 50°C for 23.5 h, rotary evaporated, and dried to obtain tri(vinylbenzene)boroxane;
[0065] (3) 18 g of amino-terminated vinyl polysiloxane, 2 g of octadecyl methacrylate, and 30 mL of tetrahydrofuran were mixed, and 0.21 g of tri(vinylbenzene)boroxane, 52.5 mg of benzoyl peroxide, and 52.5 mg of 2,2-azobisisobutyronitrile were added. The mixture was stirred at 20 °C for 11.5 h, rotary evaporated, hot-pressed at 160 °C for 3 min, dissolved in toluene, precipitated with petroleum ether, and precipitated repeatedly for 4 times. The mixture was dried to obtain a modified polysiloxane.
[0066] The preparation of the composite nano zinc oxide comprises the following steps: mixing 2.5 g of nano zinc oxide and 100 mL of toluene, stirring at 80° C. for 9 min, adding 1 mL of dodecyl trimethoxy silane, continuing to keep warm for 8.5 h, adding 0.25 mL of 3-glycidyloxypropyl trimethoxy silane, continuing to keep warm for 7.5 h, centrifuging, ultrasonically cleaning with ethanol, centrifuging, drying, and grinding to obtain the composite nano zinc oxide;
[0067] S3: Assembling the structure of the cable core, filling water-blocking sealant between the various structures of the cable core, and then sequentially wrapping the braided layer 8, the tensile reinforcement layer 9, the braided fastening layer 10, and the outer sheath 11 on the outer surface to obtain an optoelectronic composite cable for underwater buoys;
[0068] The cable core structure consists of an optical cable element 1, a water inlet detection line 2, a 48V power line 3, an RS422 data line 4, a 220V power line 5, and a drainage line 6;
[0069] The outer surfaces of the optical cable element 1, the water inlet detection line 2, the 48V power line 3, the RS422 data line 4, and the 220V power line 5 are coated with an aluminum-plastic composite cable;
[0070] The optical cable element 1 is composed of an optical fiber and an armor layer on the surface of the optical fiber, and the armor layer on the surface of the optical fiber is a seamless stainless steel tube with a diameter of 1.3 mm;
[0071] The braided layer 8 and the tensile reinforcement layer 9 are both aramid fiber layers; the braided fastening layer 10 is a twisted water-blocking aramid fiber layer;
[0072] The aramid fiber layer is woven from aramid fibers; the twisted water-blocking aramid layer is formed by twisting the aramid fibers in the Z direction at 90 degrees to form a twisted rope armor;
[0073] The 48V power cord 3 is made of 19 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the water inlet detection line 2 and RS422 data line 4 are made of 7 0.25mm silver-plated copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with ethylene tetrafluoroethylene copolymer; the 220V power cord 5 is made of 19 0.31mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the drainage line 6 is made of 19 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant.
[0074] Embodiment 3: A process for preparing an optoelectronic composite cable for an underwater buoy, comprising the following steps:
[0075] S1: polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide are mixed, put into a twin-screw extruder for mixing and extrusion, pelletized and dried to obtain an outer sheath base material, and the outer sheath base material is extruded in a semi-extrusion manner to obtain an outer sheath 11;
[0076] In terms of weight, the outer sheath base material is composed of 36 parts of polyurethane, 27 parts of self-repairing polyurethane prepolymer, and 5 parts of composite nano zinc oxide;
[0077] The preparation of the self-repairing polyurethane prepolymer comprises the following steps:
[0078] 1) Mix 0.1mmol trioxymethylene, 0.4mmol salicylaldehyde and 25mL glacial acetic acid, heat to 92℃, add 0.25mL concentrated sulfuric acid, keep warm for 24h, cool, pour into ice-water mixture and let stand overnight, wash, filter, wash with ether 3 times, recrystallize the precipitate with acetone 5 times to obtain 5,5'-methylenebissalicylaldehyde;
[0079] 2) Under nitrogen protection, 0.5 g of modified polysiloxane, 5 mL of anhydrous tetrahydrofuran, and 5 mL of dichloromethane were mixed, cooled to 0 ° C, 0.3 mmol of isophorone diisocyanate was added, and stirred for 6 h. The temperature was raised to 25 ° C, 0.2 mmol of 5,5'-methylenebissalicylaldehyde was added, and stirring was continued for 6 h. Anhydrous sodium sulfate was added and filtered, and vacuum distillation was performed, and the mixture was dissolved in 30 mL of anhydrous tetrahydrofuran. 2 mg of triethylenediamine and 0.2 mmol of diphenylmethane diisocyanate were added, and the mixture was stirred for 20 min under nitrogen protection, and rotary evaporated, and the mixture was transferred to a tetrafluoroethylene mold and dried to obtain a self-healing polyurethane prepolymer;
[0080] The preparation of the modified polysiloxane comprises the following steps:
[0081] (1) Under a nitrogen atmosphere, 37.4 g of octamethylcyclotetrasiloxane, 19.4 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 34.2 g of tetramethyltetraenylcyclotetrasiloxane were mixed, the temperature was raised to 92°C and kept for 20 min, the temperature was raised to 112°C, 6.2 mg of tetramethylammonium hydroxide was added, the temperature was kept for 6 h, the temperature was raised to 130°C and kept for 30 min, and the pressure was reduced for 3 h to obtain amino-terminated vinyl polysiloxane;
[0082] (2) Under nitrogen atmosphere, 13.5 mmol 4-vinylbenzene boronic acid, 42.2 mmol anhydrous sodium sulfate, and 20 mL tetrahydrofuran were mixed, kept at 52°C for 23 h, rotary evaporated, and dried to obtain tri(vinylbenzene)boroxane;
[0083] (3) 18 g of amino-terminated vinyl polysiloxane, 2 g of octadecyl methacrylate, and 30 mL of tetrahydrofuran were mixed, and 0.21 g of tri(vinylbenzene)boroxane, 52.5 mg of benzoyl peroxide, and 52.5 mg of 2,2-azobisisobutyronitrile were added. The mixture was stirred at 25 °C for 11 h, rotary evaporated, hot-pressed at 160 °C for 3 min, dissolved in toluene, precipitated with petroleum ether, and precipitated repeatedly for 5 times. The mixture was dried to obtain a modified polysiloxane.
[0084] The preparation of the composite nano zinc oxide comprises the following steps: mixing 2.5 g of nano zinc oxide and 100 mL of toluene, stirring at 82° C. for 8 min, adding 1 mL of dodecyl trimethoxy silane, continuing to keep warm for 9 h, adding 0.25 mL of 3-glycidyloxypropyl trimethoxy silane, continuing to keep warm for 8 h, centrifuging, ultrasonically cleaning with ethanol, centrifuging, drying, and grinding to obtain composite nano zinc oxide;
[0085] S3: Assembling the structure of the cable core, filling water-blocking sealant between the various structures of the cable core, and then sequentially wrapping the braided layer 8, the tensile reinforcement layer 9, the braided fastening layer 10, and the outer sheath 11 on the outer surface to obtain an optoelectronic composite cable for underwater buoys;
[0086] The cable core structure consists of an optical cable element 1, a water inlet detection line 2, a 48V power line 3, an RS422 data line 4, a 220V power line 5, and a drainage line 6;
[0087] The outer surfaces of the optical cable element 1, the water inlet detection line 2, the 48V power line 3, the RS422 data line 4, and the 220V power line 5 are coated with an aluminum-plastic composite cable;
[0088] The optical cable element 1 is composed of an optical fiber and an armor layer on the surface of the optical fiber, and the armor layer on the surface of the optical fiber is a seamless stainless steel tube with a diameter of 1.3 mm;
[0089] The braided layer 8 and the tensile reinforcement layer 9 are both aramid fiber layers; the braided fastening layer 10 is a twisted water-blocking aramid fiber layer;
[0090] The aramid fiber layer is woven from aramid fibers; the twisted water-blocking aramid layer is formed by twisting the aramid fibers in the Z direction at 90 degrees to form a twisted rope armor;
[0091] The 48V power cord 3 is made of 21 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the water inlet detection line 2 and RS422 data line 4 are made of 8 0.25mm silver-plated copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with ethylene tetrafluoroethylene copolymer; the 220V power cord 5 is made of 21 0.31mm tinned copper wires twisted together, coated and filled with water-blocking sealant, and then surface-coated with polyethylene; the drainage line 6 is made of 21 0.26mm tinned copper wires twisted together, coated and filled with water-blocking sealant.
[0092] Comparative Example 1: Example 3 was used as a control group, tri(vinylbenzene)boroxane was not prepared, and other processes were normal.
[0093] Comparative Example 2: Example 3 was used as the control group, octadecyl methacrylate was not added, and other processes were normal.
[0094] Comparative Example 3: Taking Example 3 as the control group, the modified siloxane was replaced by 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, and the other processes were normal.
[0095] Comparative Example 4: Example 3 was used as the control group, 5,5'-methylenebissalicylaldehyde was not added, and other processes were normal.
[0096] Comparative Example 5: Taking Example 3 as the control group, nano zinc oxide was used to replace the composite zinc oxide, and the other processes were normal.
[0097] The thickness of the protective sleeve in the embodiment and the comparative example is 1 mm.
[0098] Source of raw materials (for demonstration only):
[0099] Polyurethane TPU 9395AU: Bayer, Covestro; Water-blocking sealant is silicone-based sealant: Nanjing University Chemical 87 glue; Polyethylene 1C7A: Sinopec; Aluminum-plastic composite cable (specification 10mm*0.025mm): Yangzhou Tengfei; Seamless stainless steel pipe (1mm): Zhongtian Electric Power Cable Co., Ltd.; Aramid fiber (Kevlar fiber K49, specification 1580dtex): DuPont; Ethylene tetrafluoroethylene copolymer AP-230: Dongguan Suguang Plastic Raw Materials Co., Ltd.; Trioxane R155: Wuhan Jixin Yibang Biotechnology Co., Ltd.; Salicylaldehyde 90-02-8: Hubei Keward Chemical Co., Ltd.; Diphenylmethane diisocyanate 101-68-8: Shandong Jiaying Chemical Technology Co., Ltd.; 1,3-Bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane S70680: Shanghai Yuanye Biotechnology Co., Ltd. Company; Tetramethyltetraenylcyclotetrasiloxane 396281: Sigma-Aldrich (Shanghai) Trading Co., Ltd.; Tetrahydrofuran T431413, Isophorone diisocyanate I109582, Triethylenediamine T431497, Octamethylcyclotetrasiloxane O160041, Tetramethylammonium hydroxide T100882, 4-vinylphenylboronic acid V102338, Octadecanyl methacrylate S1075 62. Benzoyl peroxide B104630, 2,2-azobisisobutyronitrile A104255, nano zinc oxide Z112847, dodecyltrimethoxysilane D155296, 3-glycidyloxypropyltrimethoxysilane G107576: Aladdin reagent; ethanol, glacial acetic acid, sulfuric acid, ether, acetone, dichloromethane, anhydrous sodium sulfate, toluene, petroleum ether, analytical grade: Sinopharm Group reagent.
[0100] Performance test: The protective sleeves prepared in the embodiments and comparative examples were subjected to performance tests; hydrophobicity: characterized by water contact angle, tested with a 2µL deionized water droplet; self-healing property: a scratch of 800µm in length, 4µm in width and 800µm in depth was drawn on the surface of the sample, and the initial scratch length L0 was recorded. The sample was kept at 30°C for 12h, and the scratch length L1 after the insulation was observed with an electron microscope. The self-healing rate was (L0-L1) / L0×100%; wear resistance: the sample was placed on 1000-mesh sandpaper, with a load of 60g and a pulling speed of 2cm / s. Each movement of 8cm was recorded as a cycle, and the water contact angle of the protective layer was measured after 5 cycles; salt resistance: the sample was immersed in a 12g / L sodium chloride aqueous solution, kept at 80°C for 72h, and the surface of the sample was observed for blistering, damage, etc. The surface was qualified if there was no change; the measurement results are shown in Table 1 below; the specific data are shown in Table 1;
[0101] Table 1
[0102]
[0103] The present invention provides an optoelectronic composite cable for an underwater buoy and a preparation process thereof. The prepared optoelectronic composite cable has good mechanical strength, mechanical damage resistance, wear resistance and water resistance, so that the cable has good large-capacity optical signal transmission capacity and data signal transmission capacity under the premise of meeting watertight performance, and also has various communication signal lines such as telephone transmission lines and water ingress detection lines, as well as various comprehensive signals and electric energy such as 220V high-voltage boat power and 48V lithium battery power supply. In Table 1, / indicates that the item has not been tested.
[0104] By comparing Example 3 with Comparative Example 1, Comparative Example 2 and Comparative Example 3, it can be seen that in order to improve the wear resistance and water resistance of the outer sheath, modified siloxane is introduced into the self-healing polyurethane prepolymer, and octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethyltetraenylcyclotetrasiloxane are first used under the action of tetramethylammonium hydroxide as a catalyst to prepare amino-terminated vinyl polysiloxane, and the monomer formed by dehydration of 4-vinylbenzeneboronic acid and amino-terminated vinyl polysiloxane are copolymerized with hydrophobic octadecyl methacrylate by free radical polymerization to prepare a modified polysiloxane having a BO six-membered ring dynamic cross-linking network and long-chain alkane groups and amino groups; the self-healing polyurethane prepolymer is prepared as a raw material, and the self-healing polyurethane prepolymer is endowed with rapid self-repairability at room temperature, water environment and low temperature, thereby greatly improving the water resistance and wear resistance of the protective cover.
[0105] By comparing Example 3 with Comparative Example 4, it can be seen that in the preparation of the self-healing polyurethane prepolymer, bio-based salicylaldehyde is used as a raw material to prepare 5,5'-methylene disalicylicaldehyde with tripolyformaldehyde, and 5,5'-methylene disalicylicaldehyde and isophorone diisocyanate are gradually polymerized with modified polysiloxane, and then 5,5'-methylene disalicylicaldehyde is cross-linked with diphenylmethane diisocyanate to form a synergistic effect of the dynamic bonds of phenyl carbamate and the dynamic cross-linking network of BO hexacyclic rings, so as to obtain a dynamic self-healing silicone elastomer with high mechanical strength, good hydrophobicity, multiple active sites, high compatibility and high wear resistance, which is easy to improve the compatibility when mixed with other raw materials; and the introduction of silicon and the complexity of the Si-O-Si cross-linking structure help to improve the flame retardancy of the protective cover.
[0106] By comparing Example 3 with Comparative Example 5, it can be seen that nano zinc oxide is introduced as a filler in the preparation of the protective sleeve to further improve the water resistance and wear resistance of the protective sleeve. In order to improve the uniformity of the dispersion of nano zinc oxide in polyurethane, the nano zinc oxide is modified and double-modified with dodecyl trimethoxy silane and 3-glycidyloxypropyl trimethoxy silane to prepare super hydrophobic nano zinc oxide with good thermal stability and high dispersibility in a toluene system to prepare a protective sleeve with a super hydrophobic surface. At the same time, there is a metal-coordination bond between the composite nano zinc oxide and the self-healing polyurethane prepolymer, which is beneficial to further improve its self-healing rate.
[0107] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the present invention specification under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. An optoelectronic composite cable for underwater buoy, characterized in that: The cable core comprises a cable element, wherein the structure of the cable core comprises an optical cable element (1), a water ingress detection line (2), a 48V power line (3), an RS422 data line (4), a 220V power line (5), and a drainage line (6); a water-blocking sealant is filled between the various structures of the cable core; and the outer surface of the cable core is sequentially wrapped with a braided layer (8), a tensile reinforcement layer (9), a braided fastening layer (10), and an outer sheath (11); A process for preparing an optical-electric composite cable for an underwater buoy comprises the following steps: S1: polyurethane, self-repairing polyurethane prepolymer and composite nano zinc oxide are mixed, put into a twin-screw extruder for mixing and extrusion, pelletized and dried to obtain an outer sheath base material, and the outer sheath base material is extruded by semi-extrusion to obtain an outer sheath (11); S2: assembling the cable core structure, filling water-blocking sealant between the various structures of the cable core, and then sequentially wrapping the outer surface with a braided layer (8), a tensile reinforcement layer (9), a braided fastening layer (10), and an outer sheath (11), to obtain an optoelectronic composite cable for an underwater buoy; The preparation of the self-repairing polyurethane prepolymer comprises the following steps: 1) Mix trioxymethylene, salicylaldehyde and glacial acetic acid, heat to 88-92°C, add concentrated sulfuric acid, keep warm for 22-24 hours, cool, pour into ice-water mixture and let stand overnight, wash, filter, wash with ether 2-3 times, recrystallize the precipitate with acetone 3-5 times to obtain 5,5'-methylenebissalicylaldehyde; 2) Under nitrogen protection, the modified polysiloxane, anhydrous tetrahydrofuran and dichloromethane are mixed, the temperature is lowered to 0°C, isophorone diisocyanate is added, and the mixture is stirred for 5-6 hours. The temperature is raised to 18-25°C, 5,5'-methylenebissalicylaldehyde is added, and stirring is continued for 5-6 hours. Anhydrous sodium sulfate is added, filtered, and vacuum distilled. The mixture is dissolved in anhydrous tetrahydrofuran, triethylenediamine and diphenylmethane diisocyanate are added, and the mixture is stirred for 15-20 minutes under nitrogen protection, rotary evaporated, transferred to a mold, and dried to obtain a self-healing polyurethane prepolymer; The preparation of the modified polysiloxane comprises the following steps: (1) Under a nitrogen atmosphere, octamethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethyltetraenylcyclotetrasiloxane are mixed, the temperature is raised to 88-92°C and kept for 20-30 minutes, the temperature is raised to 108-112°C, tetramethylammonium hydroxide is added, the temperature is kept for 4-6 hours, the temperature is raised to 130°C and kept for 25-30 minutes, and the pressure is reduced for 2-3 hours to obtain amino-terminated vinyl polysiloxane; (2) Under a nitrogen atmosphere, 4-vinylbenzene boronic acid, anhydrous sodium sulfate and tetrahydrofuran are mixed, kept at 48-52° C. for 23-24 hours, rotary evaporated and dried to obtain tri(vinylbenzene)boroxane; (3) Mixing amino-terminated vinyl polysiloxane with octadecyl methacrylate and tetrahydrofuran, adding tri(vinylbenzene)boroxane, benzoyl peroxide and 2,2-azobisisobutyronitrile, stirring at 18-25°C for 11-12h, rotary evaporation, hot pressing at 160°C for 3min, dissolving in toluene, precipitating with petroleum ether, repeating the precipitation 3-5 times, and drying to obtain modified polysiloxane; The preparation of the composite nano zinc oxide comprises the following steps: mixing nano zinc oxide and toluene, stirring at 78-82° C. for 8-10 minutes, adding dodecyl trimethoxy silane, continuing to keep warm for 8-9 hours, adding 3-glycidyloxypropyl trimethoxy silane, continuing to keep warm for 7-8 hours, centrifuging, ultrasonically cleaning with ethanol, centrifuging, drying, and grinding to obtain the composite nano zinc oxide.
2. The optical-electric composite cable for underwater buoy according to claim 1, characterized in that: The optical cable element (1), the water ingress detection line (2), the 48V power line (3), the RS422 data line (4), and the 220V power line (5) are coated with an aluminum-plastic composite cable.
3. The optical-electric composite cable for underwater buoy according to claim 1, characterized in that: The optical cable element (1) is composed of an optical fiber and an armor layer on the surface of the optical fiber, wherein the armor layer on the surface of the optical fiber is a seamless stainless steel tube with a diameter of 1.3 mm; the braided layer (8) and the tensile reinforcement layer (9) are both aramid fiber layers; and the braided fastening layer (10) is a twisted water-blocking aramid layer.
4. The optical-electric composite cable for underwater buoy according to claim 1, characterized in that: The 48V power line (3) is prepared by twisting 17-21 0.26mm tinned copper wires, coating and filling water-blocking sealant, and then coating the surface with polyethylene; the water inlet detection line (2) and RS422 data line (4) are prepared by twisting 6-8 0.25mm silver-plated copper wires, coating and filling water-blocking sealant, and then coating the surface with ethylene tetrafluoroethylene copolymer; the 220V power line (5) is prepared by twisting 17-21 0.31mm tinned copper wires, coating and filling water-blocking sealant, and then coating the surface with polyethylene; the drainage line (6) is prepared by twisting 17-21 0.26mm tinned copper wires, coating and filling water-blocking sealant.
5. The optical-electric composite cable for underwater buoy according to claim 1, characterized in that: The water-blocking sealant is a silicone-based sealant or a chlorobutyl-based sealant.
6. The photoelectric composite cable for underwater buoy according to claim 1, characterized in that: Calculated by weight, the outer sheath base material comprises: 32-36 parts of polyurethane, 15-27 parts of self-repairing polyurethane prepolymer, and 1-5 parts of composite nano zinc oxide.
Citation Information
Patent Citations
Preparation method of novel dispiropyran chromophore
CN108864155A
A preparing method of a flame retardant optical cable filler
CN108912434A