Semiconductor device and method for manufacturing the same
By adopting a multi-layer ion-doped region structure in a single-photon avalanche diode device, the problems of substrate thickness uniformity, contact resistance and dark count uniformity are solved, and the photon detection efficiency and sensitivity are improved.
Patent Information
- Application Number
- CN202410897100.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Single-photon avalanche diode devices have problems such as poor uniformity of substrate thickness, poor uniformity of contact resistance between the back electrode and the substrate, poor uniformity of dark count, and low photon detection efficiency, especially when the device size is shrunk and the thickness of the epitaxial layer is increased.
Using a multi-layer ion doping region structure, the ion doping concentration is reduced layer by layer through the first and second ion doping regions extending from different surfaces of the substrate, forming a concentration gradient junction to isolate metal ion contamination and improve load carrying capacity. Flow diffusion velocity and avalanche occurrence probability.
The photon detection efficiency and dark count uniformity of the device are improved, the energy consumption and time during the diffusion process are reduced, and the sensitivity and performance uniformity of the device are enhanced.
Smart Images

Figure CN118431316B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor integrated circuit manufacturing, and in particular to a semiconductor device and a manufacturing method thereof. Background Art
[0002] Currently, the Single Photon Avalanche Diode (SPAD) device includes a substrate and an epitaxial layer formed on the substrate. The substrate is heavily P-type doped, the epitaxial layer is P-type intrinsically doped, a PN junction consisting of a P-type doped region and an N-type doped region is formed in the epitaxial layer, a front electrode is formed on the side of the epitaxial layer away from the substrate, and a back electrode is formed on the side of the substrate away from the epitaxial layer.
[0003] However, the above-mentioned single photon avalanche diode device has the following problems:
[0004] (1) The substrate is ground and thinned by chemical mechanical polishing, resulting in poor thickness uniformity of the remaining substrate, which in turn affects the uniformity of device performance;
[0005] (2) The ion doping concentration of the incoming substrate is low (e.g. 1E18 cm -3 ), resulting in poor uniformity of the contact resistance between the back electrode and the substrate;
[0006] (3) Due to the contamination of the PN junction by metal ions, the dark count of the device has a tail problem and the uniformity of the dark count is poor;
[0007] (4) In order to improve the photon detection efficiency (PDE), the first method is to increase the area of the multiplication zone. However, as the device size shrinks, this method is obviously no longer applicable. The second method is to increase the thickness of the epitaxial layer for infrared light sources. However, since the thickness of the multiplication zone is relatively small, if the thickness of the epitaxial layer is too thick (for example, 8.5 microns), the carriers need to diffuse through the intrinsic doping region of the epitaxial layer over a long distance between the substrate and the multiplication zone before they can produce an avalanche. In addition, there is energy consumption during the diffusion process, resulting in only a small number of carriers being able to produce an avalanche, thereby reducing the photon detection efficiency. In addition, the long diffusion time also affects the sensitivity of the semiconductor device.
[0008] Therefore, single photon avalanche diode devices need to be optimized to solve the above problems. Summary of the invention
[0009] The object of the present invention is to provide a semiconductor device and a method for manufacturing the same, so as to improve the photon detection efficiency and dark count uniformity of the device.
[0010] To achieve the above object, the present invention provides a semiconductor device, comprising:
[0011] a substrate having a first surface and a second surface opposite to each other;
[0012] A first ion doped region for forming a photodiode, extending from the first surface of the substrate into the substrate;
[0013] The second ion doping region extends from the second surface of the substrate into the substrate, and the second ion doping region includes at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface.
[0014] Optionally, the first ion-doped region includes a first doping layer and a second doping layer of opposite doping types, the first doping layer extends from the first surface of the substrate into the substrate; the second doping layer extends from a side of the first doping layer away from the first surface toward the second surface, or the second doping layer surrounds the first doping layer; the second ion-doped region has the same doping type as the second doping layer.
[0015] Optionally, the semiconductor device further includes:
[0016] A third ion doping region extends from a side of the first doping layer away from the second doping layer into the first doping layer. The third ion doping region has the same doping type as the second doping layer, and the ion doping concentration of the third ion doping region is greater than the ion doping concentration of the second doping layer.
[0017] Optionally, the semiconductor device further includes:
[0018] A fourth ion doping region extends from a side of the first doping layer away from the second doping layer to the first doping layer. The fourth ion doping region has the same doping type as the first doping layer, and the ion doping concentration of the fourth ion doping region is greater than the ion doping concentration of the first doping layer.
[0019] Optionally, the semiconductor device further includes:
[0020] A first electrode formed on the fourth ion-doped region;
[0021] The second electrode is formed on the second ion-doped region.
[0022] Optionally, the ion doping concentration of the ion implantation region in contact with the second electrode is greater than 1E18 cm -3 .
[0023] Optionally, the semiconductor device further includes:
[0024] An isolation structure extends from the first surface to the second surface of the substrate, and the isolation structure is formed at the periphery of the first ion-doped region.
[0025] Optionally, the substrate is an epitaxial layer; or, the substrate includes a base and an epitaxial layer formed on the base, and the first surface is a side of the epitaxial layer away from the base.
[0026] The present invention also provides a method for manufacturing a semiconductor device, comprising:
[0027] Providing a substrate having a first surface and a second surface opposite to each other;
[0028] A first ion-doped region and a second ion-doped region are formed, wherein the first ion-doped region extends from the first surface of the substrate into the substrate, and the first ion-doped region is used to form a photodiode; the second ion-doped region extends from the second surface of the substrate into the substrate, and the second ion-doped region includes at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in a direction from the second surface toward the first surface.
[0029] Optionally, the first ion-doped region includes a first doping layer and a second doping layer of opposite doping types, the first doping layer extends from the first surface of the substrate into the substrate; the second doping layer extends from a side of the first doping layer away from the first surface toward the second surface, or the second doping layer surrounds the first doping layer; the second ion-doped region has the same doping type as the second doping layer.
[0030] Optionally, the method for manufacturing the semiconductor device further includes:
[0031] A third ion doping region is formed, wherein the third ion doping region extends from a side of the first doping layer away from the second doping layer to the first doping layer, the third ion doping region has the same doping type as the second doping layer, and the ion doping concentration of the third ion doping region is greater than the ion doping concentration of the second doping layer.
[0032] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0033] 1. The semiconductor device of the present invention comprises: a first ion-doped region for forming a photodiode, extending from the first surface of the substrate into the substrate; a second ion-doped region, extending from the second surface of the substrate into the substrate, the second ion-doped region comprising at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface, so that the photon detection efficiency of the device and the uniformity of dark counts and other performances can be improved.
[0034] 2. The manufacturing method of the semiconductor device of the present invention forms a first ion-doped region and a second ion-doped region, wherein the first ion-doped region extends from the first surface of the substrate into the substrate, and the first ion-doped region is used to form a photodiode; the second ion-doped region extends from the second surface of the substrate into the substrate, and the second ion-doped region includes at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface, so that the photon detection efficiency of the device and the uniformity of dark counts and other performances can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic diagram of a semiconductor device according to an embodiment of the present invention;
[0036] Figure 2 The flowchart of the method for manufacturing a semiconductor device according to an embodiment of the present invention is shown.
[0037] Among them, Figure 1~Figure 2 The reference numerals are described as follows:
[0038] 11-substrate; 111-intrinsic doping layer; 121-first doping layer; 122-second doping layer; 13-second ion doping region; 131-first ion implantation region; 132-second ion implantation region; 133-third ion implantation region; 14-third ion doping region; 15-fourth ion doping region; 16-first electrode; 17-second electrode; 18-isolation structure. DETAILED DESCRIPTION
[0039] In order to make the purpose, advantages and features of the present invention more clear, the semiconductor device and the manufacturing method thereof proposed by the present invention are further described in detail below. It should be noted that the drawings are all in a very simplified form and are not in precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.
[0040] An embodiment of the present invention provides a semiconductor device, comprising: a substrate having a first surface and a second surface opposite to each other; a first ion-doped region for forming a photodiode, extending from the first surface of the substrate into the substrate; a second ion-doped region, extending from the second surface of the substrate into the substrate, the second ion-doped region comprising at least two layers of ion implantation regions, the ion doping concentration of each layer of the ion implantation region decreasing layer by layer in a direction from the second surface toward the first surface.
[0041] See below Figure 1 The semiconductor device provided by this embodiment is described in detail.
[0042] The substrate 11 has a first surface and a second surface opposite to each other.
[0043] The substrate 11 may be a single-layer structure, or may include a multi-layer structure composed of the same or different materials. The substrate 11 may be made of semiconductor materials such as Si, SiGe, SiGeC, SiC, GaAs, InAs, InP, and other III / V or II / VI compound semiconductors, or may include a layered substrate such as Si / SiGe, Si / SiC, silicon on insulator (SOI), or silicon germanium on insulator, or may include other materials other than semiconductor materials, which is not limited in the present application.
[0044] The substrate 11 is an epitaxial layer; or, the substrate 11 includes a base and an epitaxial layer formed on the base, the first surface is a side of the epitaxial layer away from the base, and the second surface is a side of the base away from the epitaxial layer.
[0045] The ion doping concentration of the epitaxial layer is very low (e.g., less than 5E14 cm -3 ),like Figure 1 As shown, the epitaxial layer may include an intrinsically doped layer 111, which may serve as a neutral region. As an example, the epitaxial layer may be unintentionally doped, ie, have P-type or N-type doping caused only by accidental contamination of impurities during its manufacture.
[0046] The ion doping concentration of the substrate is much greater than the ion doping concentration of the epitaxial layer. The substrate can be heavily doped (for example, 1E18 cm -3 ).
[0047] The doping types of the substrate and the epitaxial layer may be the same or opposite, for example, the doping type of the substrate is P-type, and the doping type of the epitaxial layer may be N-type or P-type; the doping type of the substrate is N-type, and the doping type of the epitaxial layer may be N-type or P-type. Preferably, the substrate is P+ type, and the epitaxial layer is P- type.
[0048] Preferably, the substrate 11 is an epitaxial layer, and a part of the thickness of the substrate is first removed by a chemical mechanical polishing process, and then the remaining thickness of the substrate is removed by a wet etching process, so that only the epitaxial layer is retained in the substrate 11; because the wet etching process has a higher precision in removing the substrate than the chemical mechanical polishing process, the flatness of the epitaxial layer surface after the substrate is removed is improved, that is, the thickness uniformity of the epitaxial layer after the substrate is removed is improved, thereby improving the uniformity of device performance.
[0049] The first ion doped region for forming a photodiode extends from the first surface of the substrate 11 into the substrate 11. The photodiode may be an avalanche photodiode or a single photon avalanche diode.
[0050] The first ion doping region includes a first doping layer 121 and a second doping layer 122 of opposite doping types, wherein the first doping layer 121 extends from the first surface of the substrate 11 into the substrate 11; the second doping layer 122 extends from a side of the first doping layer 121 away from the first surface toward the second surface (e.g., Figure 1 As shown), alternatively, the second doping layer 122 surrounds the first doping layer 121.
[0051] When the second doping layer 122 extends from a side of the first doping layer 121 away from the first surface toward the second surface, the width of the second doping layer 122 in a direction parallel to the first surface may be less than, equal to or greater than the width of the first doping layer 121 in a direction parallel to the first surface.
[0052] A multiplication region is formed between the first doping layer 121 and the second doping layer 122 .
[0053] The second ion doping region 13 extends from the second surface of the substrate 11 into the substrate 11, and the second ion doping region 13 includes at least two layers of ion implantation regions, each layer of the ion implantation regions is stacked layer by layer, and the ion doping concentration of each layer of the ion implantation regions decreases layer by layer in the direction from the second surface toward the first surface.
[0054] exist Figure 1 In the illustrated embodiment, the second ion doping region 13 comprises three layers of ion implantation regions stacked in a direction from the second surface toward the first surface, namely, a first ion implantation region 131, a second ion implantation region 132, and a third ion implantation region 133 stacked in layers, and the ion doping concentrations from the first ion implantation region 131 to the third ion implantation region 133 gradually decrease. The number of ion implantation region layers in the second ion doping region 13 is not specifically limited and can be set as required.
[0055] Preferably, the width of the ion implantation region of each layer in the direction parallel to the first surface is greater than the width of the first doping layer 121 in the direction parallel to the first surface. In other embodiments, the width of the ion implantation region of each layer in the direction parallel to the first surface may be equal to or less than the width of the first doping layer 121 in the direction parallel to the first surface.
[0056] The second ion doping region 13 and the second doping layer 122 have the same doping type.
[0057] Since the ion doping concentration of each layer of the ion implantation area decreases layer by layer in the direction from the second surface toward the first surface, a concentration gradient junction is formed between two adjacent ion implantation areas. The concentration gradient junction can isolate external metal ions and prevent external metal ions from approaching the PN junction formed between the first doping layer 121 and the second doping layer 122 to affect the electric field distribution, that is, it prevents external metal ions from contaminating the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby avoiding the tail problem of the dark count of the device, thereby improving the uniformity of the dark count of the device.
[0058] Furthermore, since the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface, a concentration gradient junction is formed between two adjacent ion implantation regions, thereby forming an electric field between two adjacent ion implantation regions, and the direction of the electric field is the same as the direction of the electric field generated by applying a reverse bias voltage to the photodiode in the working state, thereby increasing the diffusion speed of carriers to the multiplication region. Even if the thickness of the epitaxial layer is very thick and the carriers need to diffuse through a long distance of the intrinsic doping region of the epitaxial layer before reaching the multiplication region to produce an avalanche, the time required for diffusion is greatly reduced, thereby reducing the carrier loss in the diffusion process, and the energy consumption in the diffusion process is also reduced. More carriers can diffuse into the multiplication region, which increases the probability of avalanche, thereby improving the photon detection efficiency and sensitivity of the semiconductor device.
[0059] Preferably, the semiconductor device also includes: a third ion doping region 14, extending from a side of the first doping layer 121 away from the second doping layer 122 to the first doping layer 121, the third ion doping region 14 has the same doping type as the second doping layer 122, and the ion doping concentration of the third ion doping region 14 is greater than the ion doping concentration of the second doping layer 122.
[0060] Since the doping types of the third ion doping region 14 and the first doping layer 121 are opposite, a junction is formed between the third ion doping region 14 and the first doping layer 121. The junction formed between the third ion doping region 14 and the first doping layer 121 can isolate external metal ions, and prevent external metal ions from approaching the PN junction formed between the first doping layer 121 and the second doping layer 122 to affect the electric field distribution, that is, prevent external metal ions from contaminating the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby avoiding the tail problem of the dark count of the device, thereby improving the uniformity of the dark count of the device.
[0061] Preferably, the semiconductor device also includes: a fourth ion doping region 15, extending from a side of the first doping layer 121 away from the second doping layer 122 to the first doping layer 121, the fourth ion doping region 15 has the same doping type as the first doping layer 121, and the ion doping concentration of the fourth ion doping region 15 is greater than the ion doping concentration of the first doping layer 121.
[0062] Preferably, the doping type of the first doping layer 121 and the fourth ion doping region 15 is N type, and the doping type of the second doping layer 122, the second ion doping region 13 and the third ion doping region 14 is P type. For example, the first doping layer 121 is N type, the fourth ion doping region 15 is N+ type, the second doping layer 122 is P type, the first ion implantation region 131 is P+ type, the second ion implantation region 132 is P type, the third ion implantation region 133 is P- type, and the third ion doping region 14 is P+ type.
[0063] In other embodiments, the doping type of the first doping layer 121 and the fourth ion doping region 15 may be P type, and the doping type of the second doping layer 122 , the second ion doping region 13 , and the third ion doping region 14 may be N type.
[0064] The semiconductor device further comprises:
[0065] A first electrode 16 is formed on a surface of the fourth ion-doped region 15 away from the second surface;
[0066] The second electrode 17 is formed on a surface of the second ion-doped region 13 away from the first surface.
[0067] A reverse bias voltage is applied to the photodiode through the first electrode 16 and the second electrode 17 .
[0068] The fourth ion doping region 15 is used to connect the first doping layer 121 , so that when a voltage is applied to the first doping layer 121 through the first electrode 16 , the contact resistance is reduced.
[0069] Preferably, the fourth ion doping region 15 is an annular structure to reduce the area of the fourth ion doping region 15 in contact with the first electrode 16 to avoid damage to the substrate 11 due to a large heavily doped area. In other embodiments, the fourth ion doping region 15 may be a non-annular structure.
[0070] When the fourth ion doping region 15 is a ring structure, the third ion doping region 14 may be located in a region surrounded by the fourth ion doping region 15 and / or in a peripheral region of the fourth ion doping region 15. The third ion doping region 14 may be in contact with the fourth ion doping region 15 or not.
[0071] If the photodiode is an avalanche photodiode or a single-photon avalanche diode, in the working state, a reverse bias voltage is applied to the photodiode through the first electrode 16 and the second electrode 17, so that the working voltage is higher than the breakdown voltage of the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby forming a voltage difference; under this voltage difference, a depletion layer is generated at the PN junction, and a strong electric field exists in the depletion layer. This electric field can ensure that the carriers in this area can obtain sufficient energy to generate an avalanche through the collision ionization effect, thereby generating a large avalanche current.
[0072] Preferably, the ion doping concentration of the ion implantation region in contact with the second electrode 17 is greater than 1E18 cm -3 , that is, the ion doping concentration of the ion implantation region in contact with the second electrode 17 is greater than the ion doping concentration of the incoming substrate itself, so that the contact resistance between the second electrode 17 and the substrate 11 can be reduced and the uniformity of the contact resistance can be improved. Among them, the greater the ion doping concentration of the ion implantation region in contact with the second electrode 17, the smaller the probability that the contact resistance between the second electrode 17 and the substrate 11 is affected by external factors (such as material type) and fluctuates, so that the uniformity of the contact resistance between the second electrode 17 and the substrate 11 is better.
[0073] The semiconductor device further includes an isolation structure 18 extending from the first surface to the second surface of the substrate 11, wherein the isolation structure 18 is formed at the periphery of the first ion-doped region. Preferably, the isolation structure 18 surrounds the first ion-doped region.
[0074] The isolation structure 18 is used to achieve isolation between adjacent photodiodes to avoid crosstalk.
[0075] The isolation structure 18 is formed in a trench (not shown) in the substrate 11 . The isolation structure 18 includes an insulating material layer (not shown) covering the inner surface of the trench and a conductive layer (not shown) filling the trench.
[0076] Among them, since in this embodiment, there is no need to increase the width of the multiplication zone (to increase the area of the multiplication zone) to improve the photon detection efficiency of the device, it is possible to avoid the multiplication zone being too wide, which would cause defects and damages generated by etching the grooves when forming the isolation structure 18 to directly contact the multiplication zone, thereby avoiding causing an increase in dark counts and reducing device performance.
[0077] In summary, the semiconductor device provided by the present invention comprises: a substrate having a first surface and a second surface opposite to each other; a first ion doping region for forming a photodiode, extending from the first surface of the substrate into the substrate; a second ion doping region, extending from the second surface of the substrate into the substrate, the second ion doping region comprising at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface. The semiconductor device of the present invention can improve the photon detection efficiency of the device and the uniformity of dark counts and other performances.
[0078] An embodiment of the present invention provides a method for manufacturing a semiconductor device. Figure 2 , Figure 2 1 is a flow chart of a method for manufacturing a semiconductor device according to an embodiment of the present invention, wherein the method for manufacturing a semiconductor device comprises:
[0079] Step S1, providing a substrate, wherein the substrate has a first surface and a second surface opposite to each other;
[0080] Step S2, forming a first ion-doped region and a second ion-doped region, wherein the first ion-doped region extends from the first surface of the substrate into the substrate, and the first ion-doped region is used to form a photodiode; the second ion-doped region extends from the second surface of the substrate into the substrate, and the second ion-doped region includes at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface.
[0081] See below Figure 1 The manufacturing method of the semiconductor device provided in this embodiment is introduced in more detail.
[0082] According to step S1 , a substrate 11 is provided. The substrate 11 has a first surface and a second surface opposite to each other.
[0083] The substrate 11 may be a single-layer structure, or may include a multi-layer structure composed of the same or different materials. The substrate 11 may be made of semiconductor materials such as Si, SiGe, SiGeC, SiC, GaAs, InAs, InP, and other III / V or II / VI compound semiconductors, or may include a layered substrate such as Si / SiGe, Si / SiC, silicon on insulator (SOI), or silicon germanium on insulator, or may include other materials other than semiconductor materials, which is not limited in the present application.
[0084] The substrate 11 is an epitaxial layer; or, the substrate 11 includes a base and an epitaxial layer formed on the base, the first surface is a side of the epitaxial layer away from the base, and the second surface is a side of the base away from the epitaxial layer.
[0085] The ion doping concentration of the epitaxial layer is very low (e.g., less than 5E14 cm -3 ),like Figure 1 As shown, the epitaxial layer may include an intrinsically doped layer 111, which may serve as a neutral region. As an example, the epitaxial layer may be unintentionally doped, ie, have P-type or N-type doping caused only by accidental contamination of impurities during its manufacture.
[0086] The ion doping concentration of the substrate is much greater than the ion doping concentration of the epitaxial layer. The substrate can be heavily doped (for example, 1E18 cm -3 ).
[0087] The doping types of the substrate and the epitaxial layer may be the same or opposite, for example, the doping type of the substrate is P-type, and the doping type of the epitaxial layer may be N-type or P-type; the doping type of the substrate is N-type, and the doping type of the epitaxial layer may be N-type or P-type. Preferably, the substrate is P+ type, and the epitaxial layer is P- type.
[0088] Preferably, the substrate 11 is an epitaxial layer, and a part of the thickness of the substrate is first removed by a chemical mechanical polishing process, and then the remaining thickness of the substrate is removed by a wet etching process, so that only the epitaxial layer is retained in the substrate 11; because the wet etching process has a higher precision in removing the substrate than the chemical mechanical polishing process, the flatness of the epitaxial layer surface after the substrate is removed is improved, that is, the thickness uniformity of the epitaxial layer after the substrate is removed is improved, thereby improving the uniformity of device performance.
[0089] According to step S2, a first ion-doped region and a second ion-doped region 13 are formed, wherein the first ion-doped region extends from the first surface of the substrate 11 into the substrate 11, and the first ion-doped region is used to form a photodiode; the second ion-doped region 13 extends from the second surface of the substrate 11 into the substrate 11, and the second ion-doped region 13 includes at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface.
[0090] The photodiode may be an avalanche photodiode or a single photon avalanche diode, etc.
[0091] The first ion doping region may be formed first and then the second ion doping region 13 , or the second ion doping region 13 may be formed first and then the first ion doping region.
[0092] The first ion doping region includes a first doping layer 121 and a second doping layer 122 of opposite doping types, wherein the first doping layer 121 extends from the first surface of the substrate 11 into the substrate 11; the second doping layer 122 extends from a side of the first doping layer 121 away from the first surface toward the second surface (e.g., Figure 1 As shown), alternatively, the second doping layer 122 surrounds the first doping layer 121.
[0093] When the second doping layer 122 extends from a side of the first doping layer 121 away from the first surface toward the second surface, the width of the second doping layer 122 in a direction parallel to the first surface may be less than, equal to or greater than the width of the first doping layer 121 in a direction parallel to the first surface.
[0094] A multiplication region is formed between the first doping layer 121 and the second doping layer 122 .
[0095] Among them, the first doping layer 121 and the second doping layer 122 can be formed respectively by sequentially forming a patterned mask layer for limiting the ion implantation range on the first surface of the substrate 11, an ion implantation process and an annealing process. The order in which the first doping layer 121 and the second doping layer 122 are formed is not limited.
[0096] The second ion doping region 13 may be formed by first using an ion implantation process and then an annealing process. The number of ion implantation processes may be one or more, which is selected according to the concentration difference between the ion implantation regions of each layer; the annealing process preferably uses a laser annealing process to avoid high temperature affecting device performance.
[0097] exist Figure 1In the illustrated embodiment, the second ion doping region 13 comprises three layers of ion implantation regions stacked in a direction from the second surface toward the first surface, namely, a first ion implantation region 131, a second ion implantation region 132, and a third ion implantation region 133 stacked in layers, and the ion doping concentrations from the first ion implantation region 131 to the third ion implantation region 133 gradually decrease. The number of ion implantation region layers in the second ion doping region 13 is not specifically limited and can be set as required.
[0098] Preferably, the width of each layer of the ion implantation region in a direction parallel to the first surface is greater than the width of the first doping layer 121 in a direction parallel to the first surface. Further preferably, each layer of the ion implantation region extends from the entire second surface of the substrate 11 into the substrate 11, so that there is no need to form a patterned mask layer on the second surface of the substrate 11 to limit the formation range of the ion implantation region, but ions can be directly implanted into the entire second surface of the substrate 11, thereby simplifying the process steps.
[0099] In other embodiments, the width of the ion implantation region of each layer in the direction parallel to the first surface may be equal to or smaller than the width of the first doping layer 121 in the direction parallel to the first surface.
[0100] The second ion doping region 13 and the second doping layer 122 have the same doping type.
[0101] Since the ion doping concentration of each layer of the ion implantation area decreases layer by layer in the direction from the second surface toward the first surface, a concentration gradient junction is formed between two adjacent ion implantation areas. The concentration gradient junction can isolate external metal ions and prevent external metal ions from approaching the PN junction formed between the first doping layer 121 and the second doping layer 122 to affect the electric field distribution, that is, it prevents external metal ions from contaminating the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby avoiding the tail problem of the dark count of the device, thereby improving the uniformity of the dark count of the device.
[0102] Furthermore, since the ion doping concentration of each layer of the ion implantation region decreases layer by layer in the direction from the second surface toward the first surface, a concentration gradient junction is formed between two adjacent ion implantation regions, thereby forming an electric field between two adjacent ion implantation regions, and the direction of the electric field is the same as the direction of the electric field generated by applying a reverse bias voltage to the photodiode in the working state, thereby increasing the diffusion speed of carriers to the multiplication region. Even if the thickness of the epitaxial layer is very thick and the carriers need to diffuse through a long distance of the intrinsic doping region of the epitaxial layer before reaching the multiplication region to produce an avalanche, the time required for diffusion is greatly reduced, thereby reducing the carrier loss in the diffusion process, and the energy consumption in the diffusion process is also reduced. More carriers can diffuse into the multiplication region, which increases the probability of avalanche, thereby improving the photon detection efficiency and sensitivity of the semiconductor device.
[0103] Preferably, the manufacturing method of the semiconductor device also includes: forming a third ion doping region 14, wherein the third ion doping region 14 extends from a side of the first doping layer 121 away from the second doping layer 122 to the first doping layer 121, the third ion doping region 14 has the same doping type as the second doping layer 122, and the ion doping concentration of the third ion doping region 14 is greater than the ion doping concentration of the second doping layer 122.
[0104] Since the doping types of the third ion doping region 14 and the first doping layer 121 are opposite, a junction is formed between the third ion doping region 14 and the first doping layer 121. The junction formed between the third ion doping region 14 and the first doping layer 121 can isolate external metal ions, and prevent external metal ions from approaching the PN junction formed between the first doping layer 121 and the second doping layer 122 to affect the electric field distribution, that is, prevent external metal ions from contaminating the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby avoiding the tail problem of the dark count of the device, thereby improving the uniformity of the dark count of the device.
[0105] Preferably, the manufacturing method of the semiconductor device also includes: forming a fourth ion doping region 15, wherein the fourth ion doping region 15 extends from a side of the first doping layer 121 away from the second doping layer 122 to the first doping layer 121, the fourth ion doping region 15 has the same doping type as the first doping layer 121, and the ion doping concentration of the fourth ion doping region 15 is greater than the ion doping concentration of the first doping layer 121.
[0106] Preferably, the doping type of the first doping layer 121 and the fourth ion doping region 15 is N type, and the doping type of the second doping layer 122, the second ion doping region 13 and the third ion doping region 14 is P type. For example, the first doping layer 121 is N type, the fourth ion doping region 15 is N+ type, the second doping layer 122 is P type, the first ion implantation region 131 is P+ type, the second ion implantation region 132 is P type, the third ion implantation region 133 is P- type, and the third ion doping region 14 is P+ type.
[0107] In other embodiments, the doping type of the first doping layer 121 and the fourth ion doping region 15 may be P type, and the doping type of the second doping layer 122 , the second ion doping region 13 , and the third ion doping region 14 may be N type.
[0108] The method for manufacturing the semiconductor device further includes:
[0109] forming a first electrode 16 on a surface of the fourth ion-doped region 15 away from the second surface;
[0110] A second electrode 17 is formed on a surface of the second ion-doped region 13 away from the first surface.
[0111] A reverse bias voltage is applied to the photodiode through the first electrode 16 and the second electrode 17 .
[0112] The fourth ion doping region 15 is used to connect the first doping layer 121 , so that when a voltage is applied to the first doping layer 121 through the first electrode 16 , the contact resistance is reduced.
[0113] Preferably, the fourth ion doping region 15 is an annular structure to reduce the area of the fourth ion doping region 15 in contact with the first electrode 16 to avoid damage to the substrate 11 due to a large heavily doped area. In other embodiments, the fourth ion doping region 15 may be a non-annular structure.
[0114] When the fourth ion doping region 15 is a ring structure, the third ion doping region 14 may be located in a region surrounded by the fourth ion doping region 15 and / or in a peripheral region of the fourth ion doping region 15. The third ion doping region 14 may be in contact with the fourth ion doping region 15 or not.
[0115] If the photodiode is an avalanche photodiode or a single-photon avalanche diode, in the working state, a reverse bias voltage is applied to the photodiode through the first electrode 16 and the second electrode 17, so that the working voltage is higher than the breakdown voltage of the PN junction formed between the first doping layer 121 and the second doping layer 122, thereby forming a voltage difference; under this voltage difference, a depletion layer is generated at the PN junction, and a strong electric field exists in the depletion layer. This electric field can ensure that the carriers in this area can obtain sufficient energy to generate an avalanche through the collision ionization effect, thereby generating a large avalanche current.
[0116] Preferably, the ion doping concentration of the ion implantation region in contact with the second electrode 17 is greater than 1E18 cm -3 , that is, the ion doping concentration of the ion implantation region in contact with the second electrode 17 is greater than the ion doping concentration of the incoming substrate itself, so that the contact resistance between the second electrode 17 and the substrate 11 can be reduced and the uniformity of the contact resistance can be improved. Among them, the greater the ion doping concentration of the ion implantation region in contact with the second electrode 17, the smaller the probability that the contact resistance between the second electrode 17 and the substrate 11 is affected by external factors (such as material type) and fluctuates, so that the uniformity of the contact resistance between the second electrode 17 and the substrate 11 is better.
[0117] The method for manufacturing the semiconductor device further includes: forming an isolation structure 18, wherein the isolation structure 18 extends from the first surface to the second surface of the substrate 11, and the isolation structure 18 is formed at the periphery of the first ion doping region. Preferably, the isolation structure 18 surrounds the first ion doping region.
[0118] The isolation structure 18 is used to isolate adjacent photodiodes and avoid crosstalk.
[0119] The isolation structure 18 is formed in a trench (not shown) in the substrate 11 . The isolation structure 18 includes an insulating material layer (not shown) covering the inner surface of the trench and a conductive layer (not shown) filling the trench.
[0120] Among them, since in this embodiment, there is no need to increase the width of the multiplication zone (to increase the area of the multiplication zone) to improve the photon detection efficiency of the device, it is possible to avoid the multiplication zone being too wide, which would cause defects and damages generated by etching the grooves when forming the isolation structure 18 to directly contact the multiplication zone, thereby avoiding causing an increase in dark counts and reducing device performance.
[0121] In summary, the manufacturing method of the semiconductor device provided by the present invention includes: providing a substrate, the substrate having a first surface and a second surface opposite to each other; forming a first ion doping region and a second ion doping region, the first ion doping region extending from the first surface of the substrate into the substrate, the first ion doping region being used to form a photodiode; the second ion doping region extending from the second surface of the substrate into the substrate, the second ion doping region comprising at least two layers of ion implantation regions, the ion doping concentration of each layer of the ion implantation region decreasing layer by layer in the direction from the second surface toward the first surface. The manufacturing method of the semiconductor device of the present invention can improve the photon detection efficiency of the device and the uniformity of dark counts and other performances.
[0122] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.
Claims
1. A semiconductor device, characterized in that: include: a substrate having a first surface and a second surface opposite to each other; A first ion doping region for forming a photodiode, extending from the first surface of the substrate into the substrate, the first ion doping region comprising a first doping layer and a second doping layer of opposite doping types, the first doping layer extending from the first surface of the substrate into the substrate; The second doped layer extends from a side of the first doped layer away from the first surface toward the second surface, or the second doped layer surrounds the first doped layer; A second ion doping region extending from the second surface of the substrate into the substrate, the second ion doping region comprising at least two layers of ion implantation regions, wherein the ion doping concentration of each layer of the ion implantation regions decreases layer by layer in a direction from the second surface toward the first surface; a third ion-doped region extending from a side of the first doped layer away from the second doped layer into the first doped layer, the third ion-doped region, the second ion-doped region and the second doped layer have the same doping type of P-type doping, and a junction formed between the third ion-doped region and the first doped layer is used to isolate external metal ions; a fourth ion-doped region extending from a side of the first doped layer away from the second doped layer into the first doped layer; A first electrode formed on the fourth ion-doped region; The second electrode is formed on the second ion-doped region.
2. The semiconductor device according to claim 1, wherein The ion doping concentration of the third ion doping region is greater than the ion doping concentration of the second doping layer.
3. The semiconductor device according to claim 1, wherein The fourth ion doping region has the same doping type as the first doping layer, and the ion doping concentration of the fourth ion doping region is greater than the ion doping concentration of the first doping layer.
4. The semiconductor device according to claim 3, characterized in that The ion doping concentration of the ion implantation region in contact with the second electrode is greater than 1E18 cm -3 .
5. The semiconductor device according to claim 1, wherein: The semiconductor device further comprises: An isolation structure extends from the first surface to the second surface of the substrate, and the isolation structure is formed at the periphery of the first ion-doped region.
6. The semiconductor device according to any one of claims 1 to 5, characterized in that The substrate is an epitaxial layer; or, the substrate includes a base and an epitaxial layer formed on the base, and the first surface is a side of the epitaxial layer away from the base.
7. A method for manufacturing a semiconductor device, characterized in that: include: Providing a substrate having a first surface and a second surface opposite to each other; forming a first ion-doped region and a second ion-doped region, wherein the first ion-doped region extends from the first surface of the substrate into the substrate, and the first ion-doped region is used to form a photodiode; the first ion-doped region comprises a first doping layer and a second doping layer of opposite doping types, and the first doping layer extends from the first surface of the substrate into the substrate; The second doped layer extends from a side of the first doped layer away from the first surface toward the second surface, or the second doped layer surrounds the first doped layer; The second ion doping region extends from the second surface of the substrate into the substrate, the second ion doping region comprises at least two layers of ion implantation regions, and the ion doping concentration of each layer of the ion implantation region decreases layer by layer in a direction from the second surface toward the first surface; forming a third ion-doped region, the third ion-doped region extending from a side of the first doped layer away from the second doped layer into the first doped layer, the third ion-doped region, the second ion-doped region and the second doped layer having the same doping type of P-type doping, and a junction formed between the third ion-doped region and the first doped layer for isolating external metal ions; forming a fourth ion-doped region, wherein the fourth ion-doped region extends from a side of the first doped layer away from the second doped layer to the first doped layer; forming a first electrode on the fourth ion-doped region; A second electrode is formed on the second ion-doped region.
8. The method for manufacturing a semiconductor device according to claim 7, wherein: The ion doping concentration of the third ion doping region is greater than the ion doping concentration of the second doping layer.
Citation Information
Patent Citations
Annular-gate single-photon avalanche diode capable of preventing edge breakdown and preparation method of annular-gate single-photon avalanche diode capable of preventing edge breakdown
CN106449770A
Stacked backside illuminated SPAD array
CN109716525A
Semiconductor device and manufacturing method thereof
CN115621352A