COFs material and preparation method thereof, lithium battery positive electrode material and application thereof
By preparing COFs materials with high specific surface area and stable structure, and doping them with carbon black, the problem of insufficient electrochemical performance and cycle performance of lithium battery cathode materials has been solved, and the energy density and cycle life of lithium-ion batteries have been improved.
Patent Information
- Application Number
- CN202410854682.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing COFs materials as cathode materials for lithium batteries do not perform well in terms of electrochemical performance stability and cycle performance. The limitations of chemical bonds lead to low energy density and short cycle life.
A method for preparing COFs materials is adopted, which includes mixing 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridin-2-amine), p-benzene Diformaldehyde is mixed with a catalyst, subjected to ultrasonic, freezing and reaction treatments, and combined with carbon black doping to form a COFs material with a high specific surface area and stable structure, which can be used as anode material for lithium batteries.
It improves the electrochemical performance and cycle stability of lithium-ion batteries, prolongs the battery's service time, and improves the battery's energy density and cycle life.
Smart Images

Figure CN118440273B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of positive electrode materials, and more specifically relates to a COFs material and a preparation method thereof, a lithium battery positive electrode material and an application thereof. Background Art
[0002] Lithium battery is an important energy storage device, and the selection of its cathode material has a significant impact on the performance of the battery. Although traditional lithium battery cathode materials such as lithium cobalt oxide and lithium manganese oxide meet the performance requirements of the battery to a certain extent, they still have problems such as low energy density and short cycle life. In order to solve these problems, researchers began to explore new lithium battery cathode materials, among which covalent organic framework materials (hereinafter referred to as COFs materials) are considered to be a new type of cathode material due to their unique properties, such as stable porous structure and high specific surface area.
[0003] However, there are still some problems with the existing COFs materials as positive electrode materials for lithium batteries. For example, due to the limitation of chemical bonds in COFs materials and the low theoretical specific capacity, COFs materials do not perform well in terms of electrochemical stability and cycle performance. It can be seen that COFs materials used to prepare positive electrode materials for lithium batteries still need to be further optimized to improve their electrochemical stability and cycle performance in positive electrode materials for lithium batteries. Summary of the invention
[0004] In view of the above-mentioned defects and problems of the prior art, the present invention develops a COFs material and a preparation method thereof, a lithium battery positive electrode material and applications thereof.
[0005] The first aspect of the present application provides a method for preparing a COFs material, comprising the following steps:
[0006] Step (1): mixing 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine), terephthalaldehyde and a solvent, and then sonicating for 5-20 minutes to obtain a primary mixed solution;
[0007] Step (2): adding a catalyst to the initial mixed solution, and obtaining a mixed solution after ultrasonic treatment;
[0008] Step (3): freezing the mixed solution at -180-200°C for 2-8 minutes, degassing and sealing;
[0009] Step (4): placing the sealed mixed solution at a temperature of 100-140° C. to react for 4-9 days. After the reaction is completed, the mixture is cooled, washed, subjected to Soxhlet extraction and dried to obtain the COFs material.
[0010] Optionally, in step (1), the molar ratio of the 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) to the terephthalaldehyde is 1:1.5-4.
[0011] Optionally, the solvent in step (1) is o-dichlorobenzene and 1,4-dioxane, and the volume ratio of the o-dichlorobenzene to the 1,4-dioxane is 2-6:1.
[0012] Optionally, in step (2), the catalyst is an aqueous acetic acid solution with a concentration of 5-7 mol / L, and the molar ratio of the aqueous acetic acid solution to the 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) is 1:13-22.
[0013] Optionally, in step (3), freezing the mixed liquid at a temperature of -180-200°C for 2-8 minutes specifically includes: freezing the mixed liquid in a liquid nitrogen environment for 2-8 minutes.
[0014] Optionally, in step (4), acetone, dichloromethane, tetrahydrofuran, water and ethanol are used to wash the solid.
[0015] In a second aspect, the present application further provides a COFs material, which is prepared using any of the preparation methods described in the first aspect above.
[0016] Another aspect of the present invention further provides the above-mentioned lithium battery positive electrode material, comprising carbon black and the COFs material prepared in the above-mentioned second aspect, wherein the mass ratio of the carbon black to the COFs material is 1:8.
[0017] Another aspect of the present invention provides the use of lithium battery positive electrode materials in the preparation of lithium ion button batteries.
[0018] Optionally, after the lithium-ion button battery is cycled 40 times, the average value of the battery charge and discharge specific capacity is 160-175 mAh / g, and the charge and discharge retention rate is 99.0%-99.6%.
[0019] In summary, this application has the following beneficial effects:
[0020] The present application uses a convenient synthesis method to prepare triazine COFs materials with large specific surface area, regular pore structure and high stability. The COFs materials are doped with conductive carbon black to form lithium battery positive electrode materials, which is beneficial to the transmission of ions / electrons and helps to improve the energy density of lithium-ion batteries, thereby improving the cycle stability of the battery and extending the battery life, solving the problem of insufficient electrochemical performance stability and cycle performance of COFs materials as lithium battery positive electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.
[0022] Figure 1 The synthetic route for preparing COFs materials.
[0023] Figure 2 This is the XRD pattern of the COFs material prepared in Example 1.
[0024] Figure 3 This is a test performance effect diagram of a button battery using a lithium battery positive electrode material made from carbon black and the COFs material prepared in Example 1. DETAILED DESCRIPTION
[0025] The present application is further described in detail with reference to the following examples. It should be noted that if no specific conditions are specified in the following examples, the conventional conditions or the conditions recommended by the manufacturer are followed, and the raw materials used in the following examples can be obtained from common commercial sources unless otherwise specified.
[0026] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0027] In this application, "first aspect", "second aspect", "third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0028] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0029] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0030] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0031] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application. The terms used in this application and in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more related listed items. The term "multiple" in this application means at least two, such as two, three, etc., unless otherwise clearly and specifically limited.
[0032] In order to facilitate the description of the technical solution of the present application, the following description is made before starting the experiment of the present application:
[0033] COFs materials are called covalent organic frameworks. They are crystalline materials with ordered porous structures formed by reversible strong covalent bonds (CC, CO, C-Si, BO) connecting light elements of the first and second periods such as light elements C, H, O, N, B, and Si. COFs will become carbon materials after high-temperature carbonization, maintaining the original structure of the material. Triazine COFs materials refer to COFs materials containing C=N(Ar) bonds. This application specifically uses 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridin-2-amine) (its English name is 5,5' 5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridin-2-amine)). The obtained COFs materials have significantly improved conductivity, rate performance and cyclability when used as positive electrode materials for lithium batteries.
[0034] In the present application, the preparation method of COFs material comprises the following steps:
[0035] Step (1): 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine), terephthalaldehyde and a solvent are mixed and ultrasonicated for 5-20 minutes to obtain a primary mixed solution. Specifically, the molar ratio of 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) to terephthalaldehyde is 1:1.5-4. The solvent is o-dichlorobenzene and 1,4-dioxane, and the volume ratio of o-dichlorobenzene to 1,4-dioxane is 2-6:1.
[0036] Step (2): Add a catalyst to the initial mixed solution, and obtain a mixed solution after ultrasonic treatment. Specifically, the catalyst is an aqueous acetic acid solution with a concentration of 5-7 mol / L, and the molar ratio of the aqueous acetic acid solution to 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) is 1:13-22.
[0037] Step (3): Freeze the mixed solution at a temperature of -180-200°C for 2-8 minutes, degas and seal. Specifically, freeze the mixed solution in a liquid nitrogen environment for 2-8 minutes.
[0038] Step (4): The sealed mixed solution is placed in a temperature of 100-140° C. for reaction for 4-9 days. After the reaction is completed, the mixture is cooled, washed, extracted with Soxhlet and dried to obtain a COFs material. Specifically, acetone, dichloromethane, tetrahydrofuran, water and ethanol can be used to wash the solid.
[0039] The synthesis route of COFs materials can be as follows Figure 1 As shown, in the actual preparation process, the preparation can be carried out within the above-mentioned value range, and no specific limitation is made here.
[0040] The obtained COFs material can be used to prepare the positive electrode material of lithium battery, and the positive electrode material of lithium battery can be used to prepare lithium-ion button battery. The lithium-ion button battery mainly includes a positive electrode shell, a negative electrode shell, a (positive / negative) electrode sheet, a diaphragm, a gasket, a spring and an electrolyte. The battery shell in the application example of this application is CR2032, the battery diaphragm is glass fiber (Whatman GF / D), and the electrolyte is 1 mol·L -1 The solution is prepared by lithium hexafluorophosphate (LiPF6) and ethylene carbonate (EC) / diethyl carbonate (DEC) (w / w=1:1). The negative electrode uses lithium sheet, and the preparation of the positive electrode sheet mainly includes two steps: preparation of slurry and coating of the electrode sheet. The raw materials of the slurry mainly include positive electrode material, conductive agent, binder and solvent. The binder uses polyvinylidene fluoride (PVDF) and the conductive agent uses carbon black. The mass ratio of positive electrode material, conductive agent and binder is 8:1:1.
[0041] The coating method of the positive electrode is: use a scraper to apply the slurry on the aluminum foil. During this process, the aluminum foil needs to be flat and wrinkles should be reduced as much as possible; before coating, the aluminum foil and the coating machine platform should be carefully cleaned with alcohol and cotton wool; after cleaning with cotton wool, they should be carefully cleaned with toilet paper.
[0042] After coating, in order to remove a large amount of solvent and moisture in the slurry, the coated positive electrode sheet is dried by air drying and vacuum drying. The temperature of the air drying process is 90 degrees Celsius and the drying time is 5 hours; the temperature of the vacuum drying process is 120 degrees Celsius and the drying time is 10 hours.
[0043] Since the coating of the dried positive electrode sheet is relatively loose, if it is used directly, it is easy to fall off and be damaged after being soaked by the electrolyte. Therefore, a tablet press is required to press the dried positive electrode sheet. The tablet press can use 80-120kg / cm 2 Pressure is used to suppress.
[0044] When assembling button cells in a glove box, the glove box must be vacuum dried for 4-6 hours before assembly. The temperature should not be too high and can be set at 60-80°C. After the raw materials enter the hatch, exhaust-intake operations must be strictly followed in accordance with the operating procedures, at least three times, before assembly can begin.
[0045] Example 1
[0046] The preparation method of COFs material is as follows:
[0047] Step (1): 0.1 mol 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tri(pyridine-2-amine) and 0.15 mol p-terephthalaldehyde are added to a glass tube, 1.4 ml o-dichlorobenzene and 0.6 ml dioxane are added through a pipette, and after mixing, the mixture is placed in an ultrasonic device for 10 minutes to obtain a primary mixed solution.
[0048] Step (2): add 0.2 ml of 6 mol / L acetic acid solution to the initial mixed solution, place it in an ultrasonic device and sonicate for 5 minutes to obtain a mixed solution.
[0049] Step (3): Place the glass tube containing the mixed solution in a liquid nitrogen environment (-196°C) and freeze for 5 minutes. Use a vacuum pump to extract the gas in the glass tube for 5 minutes, then introduce nitrogen gas and heat the glass tube to room temperature through a hair dryer. Repeat the above operation three times. Finally, vacuum extract the gas and seal the glass tube with a flame spray gun.
[0050] Step (4): Place the glass tube in an oven at 120°C for seven days, then cool down, separate the glass tube with a glass knife, filter the solid, and then wash the solid with acetone, dichloromethane, tetrahydrofuran, water and ethanol in sequence, and finally extract it with a Soxhlet extractor, place it in an oven at 120°C for drying, and complete the preparation of the COFs material.
[0051] As an example, the X-ray powder diffraction pattern (PXRD) of the COFs material prepared in Example 1 is as follows: Figure 2 As shown, from Figure 2 It can be seen that the COFs material prepared in Example 1 has good crystallinity.
[0052] Comparative Example 1
[0053] The difference from Example 1 is that terephthalaldehyde is replaced by an equal amount of 2,5-dihydroxy-1,4-benzenedicarboxylic aldehyde. The rest of the preparation method is the same as that of Example 1.
[0054] Comparative Example 2
[0055] The difference from Example 1 is that 5,5',5''-(1,3,5-triazine-2,4,6-trisubstituted)tris(pyridin-2-amine) is replaced by an equal amount of 2,4,6-tris(4-aminophenoxy)-1,3,5-triazine. The rest of the preparation method is the same as that of Example 1.
[0056] Comparative Example 3
[0057] The difference from Example 1 is that step (2) is not performed. In step (1), 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine), terephthalaldehyde, catalyst and solvent are mixed and then ultrasonicated for 5-20 minutes to obtain a mixed solution. The rest of the preparation method is the same as that of Example 1.
[0058] Application examples of COFs materials 1-4
[0059] The preparation method of lithium-ion button cell is as follows:
[0060] 1. Preparation of slurry: First, place COFs and PVDF in a 20ml vial and stir until there is no white substance to obtain the first solution; then slowly add 0.05g of conductive carbon black to the weighing bottle and stir for half an hour, then weigh 0.4g of active substance, add it to the mortar and grind it thoroughly for half an hour. The mass ratio of COFs, carbon black and PVDF is 8:1:1. Add the ground mixture to a vial, add 2mL of the first solution, stir until the slurry is viscous, and obtain a slurry. Among them, the active substance can be lithium cobalt oxide, lithium manganese oxide or lithium iron phosphate.
[0061] 2. Apply the slurry on the electrode sheet to form a positive electrode sheet, and then dry and press the positive electrode sheet in turn to obtain a positive electrode sheet to be used;
[0062] 3. Assemble the positive electrode shell, the negative electrode shell, the standby positive electrode sheet, the negative electrode sheet, the diaphragm, the gasket, the shrapnel and the electrolyte into a lithium-ion button battery.
[0063] Among them, Application Example 1 adopts the COFs material prepared in Example 1; Application Example 2 adopts the COFs material prepared in Comparative Example 1; Application Example 3 adopts the COFs material prepared in Comparative Example 2; Application Example 4 adopts the COFs material prepared in Comparative Example 3.
[0064] Performance test of button cell batteries
[0065] Experimental method: The button-type batteries prepared in Application Examples 1-4 were subjected to cycle performance tests at a current density of 100 mA-1 A. The test results are shown in Table 1. As an example, the performance test effect diagram of the button-type battery prepared in Application Example 1 is shown in Figure 3 .
[0066] Table 1. Cyclic performance test data of button-type batteries prepared in Application Examples 1-3
[0067] project Battery charge and discharge capacity after 40 cycles (mAh / g) Charge and discharge retention rate (%) Application Example 1 164 99.3 Application Example 2 121 65.4 Application Example 3 118 59.2 Application Example 4 134 71.8
[0068] As can be seen from Table 1, the button cell prepared in Application Example 1 has an average charge and discharge capacity of 164 mAh / g after 40 cycles, and a charge and discharge retention rate of 99.3%. It can be seen that the COFs material has a very good effect as a positive electrode for a lithium battery. One reason for this is that the COFs material prepared in Example 1 has an excellent specific surface area, which produces more active sites and promotes the diffusion of lithium ions. Another reason is that the lithium ions undergo a redox reaction with enough triazine groups and -NH- groups in the COFs material, making COFs a high-performance electrode material. In addition, doping the COFs material with conductive carbon black to form a positive electrode material for a lithium battery is beneficial to the transmission of ions / electrons, and helps to improve the energy density of lithium-ion batteries, thereby improving the cycle stability of the battery and extending the battery life.
[0069] However, the cycle performance of the button-type batteries prepared in Application Examples 2 and 3 is not very good, which shows that the selection of raw materials for preparing COFs materials is very important. Only by selecting suitable raw materials (5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) and terephthalaldehyde), the COFs materials prepared for lithium-ion button-type batteries have excellent cycle performance. Similarly, by comparing the data of Application Examples 1 and 4, it can be seen that the steps for preparing COFs materials also need to be strictly controlled. When the catalyst is also added to step (1), the comprehensive performance of the prepared COFs material may not be very good due to the reduced reaction thoroughness, thereby affecting the cycle performance of the lithium-ion button-type battery prepared thereby.
[0070] In summary, the method for synthesizing COFs materials of the present invention is simple and low in cost, which meets the market demand for low-cost and high-efficiency battery materials. The COFs materials prepared by the present invention have a large specific surface area and a uniform pore size distribution, which is conducive to the transmission of ions / electrons, and can improve the cycle stability of the battery. As a positive electrode material for lithium batteries, it has excellent electrochemical properties and good cycle stability, and can effectively improve the energy density and cycle life of lithium batteries, meeting the market demand for high energy density and long cycle life lithium batteries. Therefore, the present invention can be widely used in application fields such as lithium battery manufacturing, energy storage equipment research and development, and environmentally friendly battery material development, and has broad market application prospects and market demand.
[0071] It should be understood that the disclosed invention is not limited only to the specific method, scheme and material of description, because these all can change.It should also be understood that the terminology used herein is only for the purpose of describing specific embodiment scheme, rather than being intended to limit the scope of the present invention, and the scope of the present invention is only limited to the appended claims.
[0072] Those skilled in the art will also recognize, or be able to ascertain using no more than routine experimentation, many equivalents to the specific embodiments of the invention described herein. Such equivalents are also intended to be encompassed by the appended claims.
Claims
1. A method for preparing a COFs material, characterized in that: The steps include: Step (1): mixing 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine), terephthalaldehyde and a solvent, and then sonicating for 5-20 minutes to obtain a primary mixed solution; Step (2): adding a catalyst to the initial mixed solution, and obtaining a mixed solution after ultrasonic treatment; Step (3): freezing the mixed solution at -180-200°C for 2-8 minutes, degassing and sealing; Step (4): placing the sealed mixed solution at a temperature of 100-140° C. for reaction for 4-9 days, and after the reaction is completed, cooling, washing, Soxhlet extraction and drying are performed in sequence to obtain a COFs material; The structure of the prepared COFs material is shown below: 。 2. The method for preparing the COFs material according to claim 1, characterized in that: In the step (1), the molar ratio of the 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) to the terephthalaldehyde is 1:1.5-4.
3. The method for preparing the COFs material according to claim 1, characterized in that: The solvent in the step (1) is o-dichlorobenzene and 1,4-dioxane, and the volume ratio of the o-dichlorobenzene to the 1,4-dioxane is 2-6:
1.
4. The method for preparing the COFs material according to claim 1, characterized in that: In the step (2), the catalyst is an aqueous acetic acid solution with a concentration of 5-7 mol / L, and the molar ratio of the aqueous acetic acid solution to the 5,5',5''-(1,3,5-triazine-2,4,6-triyl)tris(pyridine-2-amine) is 1:13-22.
5. The method for preparing COFs material according to claim 1, characterized in that: In the step (3), the mixed liquid is placed at a temperature of -180-200°C and frozen for 2-8 minutes, which specifically includes: placing the mixed liquid in a liquid nitrogen environment and freezing it for 2-8 minutes.
6. The method for preparing the COFs material according to any one of claims 1 to 5, characterized in that: In the step (4), acetone, dichloromethane, tetrahydrofuran, water and ethanol are used to wash the solid.
7. A COFs material, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 6.
8. A positive electrode material for a lithium battery, characterized in that: It comprises carbon black and the COFs material according to claim 7, wherein the mass ratio of the carbon black to the COFs material is 1:
8.
9. Use of the lithium battery positive electrode material according to claim 8 in the preparation of lithium ion button batteries.
10. Use of the lithium battery positive electrode material according to claim 9 in preparing lithium ion button batteries, characterized in that: After 40 cycles of lithium-ion button cells, the average charge and discharge capacity of the battery is 160-175 mAh / g, and the charge and discharge retention rate is 99.0%-99.6%.