Functional coating binder and preparation method thereof and electrode sheet

By using functional coating binders in the dry electrode process and utilizing a combination of water-based modified acrylic polymers and amidated acrylic monomers, the problem of weak adhesion between active materials and current collectors in dry electrodes is solved. It improves the interface adhesion and electrode performance, and reduces the problems of powder and material falling out during production.

CN118440630BActive Publication Date: 2024-10-11SUZHOU DERBY ELECTRONIC MATERIAL TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410897529.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-11
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

In the dry electrode process, the bonding force between the active material and the current collector is weak, resulting in low interface adhesion, serious powder and material falling off, and the electrode performance potential cannot be realized.

Method used

A functional coating adhesive is used. Its main component is a water-based modified acrylic polymer, including amidated acrylic monomers. The interfacial adhesion is improved through functionalized carbon coating, and it is combined with active materials under hot pressing conditions. The material and current collector are tightly integrated.

Benefits of technology

It significantly improves the interface adhesion, reduces the risk of powder and material loss, improves production yield, reduces interface resistance, and improves electrode performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440630B_ABST
    Figure CN118440630B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of battery materials, and in particular to a functional coating binder and a preparation method thereof and an electrode sheet. The raw materials of the functional coating binder include the following components by weight: 1-80 parts of an olefinic functional monomer; 1-80 parts of an ethylenically unsaturated substance; 1-80 parts of an unsaturated water-soluble monomer; 1-80 parts of an unsaturated oil-soluble monomer; 0.1-20 parts of an initiator; 1-60 parts of a pH regulator; and the olefinic functional monomer is an amidated acrylic acid monomer. The functional coating binder provided by the present invention has excellent hot pressing bonding force. When a dry electrode is applied, it can significantly improve the interface performance, effectively improve the interface bonding force, firmly combine the active material layer with the functional coating current collector, reduce the risk of powder and material loss in subsequent processes, and effectively improve the production yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a functional coating binder and a preparation method thereof and an electrode sheet. Background Art

[0002] With the rapid development of energy technology, energy storage devices represented by batteries (especially lithium batteries) play an extremely important role in current production and life; at the same time, the explosive growth of electric vehicles and household energy storage has further promoted the innovation and iteration of the battery industry.

[0003] Under the huge volume demand, higher energy density, lower manufacturing cost and better safety have become the goals that people are eager to pursue. As the core component of the battery, the electrode sheet has a decisive influence on the performance of the battery.

[0004] The production of pole pieces is the primary link in battery manufacturing. The traditional wet process is to disperse the active material, conductive agent, binder and solvent together to make a slurry, and then apply, dry and roll-press it. Although the wet electrode can better exert the basic properties of the material, the use of the positive electrode NMP solvent makes the material cost and energy consumption cost of battery manufacturing high. In contrast, the dry electrode process that abandons the solvent is more competitive in the market.

[0005] The dry process is to dry-mix the active material powder and the conductive agent, then add the powder binder, fibrillate the binder to form a self-supporting material, and finally hot-press and compound it onto the surface of the current collector. The dry process has three significant advantages over the traditional wet process: (1) the dry process is cheaper, reducing the manufacturing cost by 18%; (2) the dry process increases the compaction density of the active material, increasing the energy density by 20%; (3) the electrical performance of dry batteries is better.

[0006] However, there is a serious problem that needs to be solved urgently in dry electrodes: due to the huge difference in interface performance, the metal current collector (including composite current collector) and its carbon-coated functionalized current collector used in the wet process are no longer suitable for the dry process. The adhesion of their interface is far lower than the requirements of the dry electrode process. The electrodes prepared by the dry process currently have serious powder and material loss phenomena, and the interface resistance between the active material and the current collector is very large, which makes it impossible for the electrodes prepared by the dry process to perform at the expected performance level. Summary of the invention

[0007] In order to solve the problem of weak adhesion between active materials and current collectors in the dry electrode process in the prior art, the present invention provides a functional coating binder, the main component of which is a water-based modified acrylic polymer. For the current dry electrode system, the cathode and anode can be functionalized and carbon-coated at the same time, so that the active material can be firmly combined with the current collector after being processed by the dry electrode process, while improving the interface adhesion and effectively reducing the interface resistance, thereby solving the problem of weak adhesion between active materials and current collectors in the dry electrode process in the prior art.

[0008] The technical solution adopted by the present invention to solve its technical problem is:

[0009] A functional coating binder, wherein the raw materials include the following components in parts by weight:

[0010] 1-80 parts of alkenyl-containing functional monomers;

[0011] 1-80 parts of ethylenically unsaturated substances;

[0012] 1-80 parts of unsaturated water-soluble monomer;

[0013] 1-80 parts of unsaturated oil-soluble monomer;

[0014] Initiator 0.1-20 parts;

[0015] 1-60 parts of pH regulator;

[0016] The alkenyl-containing functional monomer is an amidated acrylic acid monomer.

[0017] Optionally, the alkenyl-containing functional monomer is prepared according to the following method:

[0018] S01: firstly adding a carboxyl-containing acrylic acid monomer to a halogen element to obtain an addition product;

[0019] S02: chlorinating the addition product with thionyl chloride to obtain an acyl chloride monomer;

[0020] S03: subjecting the aminoalkane to an amidation reaction with the acyl chloride monomer to eliminate the halogen-reduced double bond and obtain an olefin-containing functional monomer.

[0021] Optionally, the carboxyl-containing acrylic monomer is selected from at least one of acrylic acid, methacrylic acid, itaconic acid, β-carboxyethyl acrylate, fumaric acid, and maleic acid.

[0022] Optionally, the mass ratio of the carboxyl-containing acrylic monomer to the halogen element is in the range of 1:(1-6); the mass ratio of the dichlorothionyl to the addition product is in the range of (0.2-1):1; the mass ratio of the aminoalkane to the acyl chloride monomer is in the range of (0.2-1.5):1.

[0023] Optionally, the ethylenically unsaturated substance is selected from at least one of acrylic acid, methacrylic acid, itaconic acid, β-carboxyethyl acrylate, fumaric acid, maleic acid, acrylic anhydride, methacrylic anhydride, itaconic anhydride, fumaric anhydride, and maleic anhydride.

[0024] Optionally, the unsaturated water-soluble monomer is selected from at least one of acrylamide, methacrylamide, N-hydroxyethyl acrylamide, 2-acrylamido-2-methylpropane sulfonic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, ethylene glycol methyl ether acrylate, polyethylene glycol methyl ether acrylate, sodium vinyl sulfonate, and sodium p-styrene sulfonate.

[0025] Optionally, the unsaturated oil-soluble monomer is selected from at least one of acrylonitrile, methacrylonitrile, styrene, vinyl acetate, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, isooctyl acrylate, octyl methacrylate, isodecyl acrylate, isodecyl methacrylate, and phenyl acrylate.

[0026] Optionally, by weight, it also includes:

[0027] Reaction aid 0.5-40 parts;

[0028] The reaction aid is selected from at least one of a thiol aid, a chain transfer agent, and an emulsifier.

[0029] Another object of the present invention is to provide a method for preparing the functional coating binder as described above, comprising the following steps:

[0030] S1: mixing the alkenyl-containing functional monomer, the ethylenically unsaturated substance, the unsaturated water-soluble monomer, the unsaturated oil-soluble monomer and pure water according to the formula amount to obtain a mixed solution;

[0031] S2: In an inert gas atmosphere, heating a portion of the mixed solution to 40-100° C. to obtain a reaction mixed solution;

[0032] S3: mixing an initiator with water to prepare an initiator solution;

[0033] S4: adding the initiator solution and another part of the mixed solution into the reaction mixed solution, keeping the temperature, to obtain an aqueous acrylic copolymer glue solution;

[0034] S5: adding a pH adjuster to the aqueous acrylic copolymer glue to obtain a functional coating binder.

[0035] Another object of the present invention is to provide an electrode sheet comprising the functional coating adhesive as described above.

[0036] The beneficial effects of the present invention are:

[0037] The functional coating binder provided by the present invention has excellent hot-pressing bonding strength. When used in dry-process electrodes, it can significantly improve the interface performance and effectively enhance the interface bonding strength, so that the active material layer and the functional coating current collector are firmly combined together, reducing the risk of powder and material loss in subsequent processes, and effectively improving the production yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The present invention is further described below in conjunction with the accompanying drawings and embodiments.

[0039] Figure 1 Schematic diagram of the synthesis process of the alkenyl-containing functional monomer in Example 1 of the present invention;

[0040] Figure 2 is a photograph of the functional carbon-coated aluminum foil for dry electrode prepared in Example 1 of the present invention;

[0041] Figure 3 is a photograph of the functional carbon-coated copper foil for dry electrode prepared in Example 2 of the present invention;

[0042] Figure 4 This is a comparison chart of the positive electrode peeling force on the dry-process functional carbon-coated aluminum foil prepared in Example 3 of the present invention and a conventional binder. DETAILED DESCRIPTION

[0043] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.

[0044] In order to solve the problem of weak bonding between active materials and current collectors in the dry electrode process in the prior art, the present invention provides a functional coating binder, wherein the raw materials include the following components in parts by weight:

[0045] 1-80 parts of alkenyl-containing functional monomers;

[0046] 1-80 parts of ethylenically unsaturated substances;

[0047] 1-80 parts of unsaturated water-soluble monomer;

[0048] 1-80 parts of unsaturated oil-soluble monomer;

[0049] Initiator 0.1-20 parts;

[0050] 1-60 parts of pH regulator;

[0051] The alkenyl-containing functional monomer is an amidated acrylic monomer.

[0052] The functional coating binder is a polymer formed by the above-mentioned monomers, and its main component is a water-based modified acrylic polymer; the functional coating binder is aimed at the current dry electrode system and can simultaneously perform functional carbon coating treatment on the cathode and anode. After the functional coating binder provided by the present invention is used to perform functional carbon coating treatment on the surface of the metal current collector (including the composite current collector), the active material can be firmly combined with the current collector after being processed by the dry electrode process, thereby improving the interface adhesion and effectively reducing the interface resistance.

[0053] In order to exert better interfacial adhesion and interfacial resistance, the preferred addition amount of the alkenyl-containing functional monomer in the present invention is 15-45 parts.

[0054] The functional coating binder provided by the present invention has excellent hot-pressing bonding strength. When used in dry-process electrodes, it can significantly improve the interface performance and effectively enhance the interface bonding strength, so that the active material layer and the functional coating current collector are firmly combined together, reducing the risk of powder and material loss in subsequent processes, and effectively improving the production yield.

[0055] In order to ensure the interfacial adhesion, the present invention preferably prepares the alkenyl-containing functional monomer according to the following method:

[0056] S01: firstly adding a carboxyl-containing acrylic acid monomer to a halogen element to obtain an addition product;

[0057] S02: Chlorinating the addition product with thionyl chloride to obtain an acyl chloride monomer;

[0058] S03: subjecting the aminoalkane to an amidation reaction with an acyl chloride monomer to eliminate the halogen-reduced double bond, thereby obtaining an amidated acrylic acid monomer, i.e., an olefin-containing functional monomer.

[0059] The specific process conditions of each step in the above preparation process can be selected from the corresponding existing technology according to the reaction type. It is preferred that the alkenyl-containing functional monomer is purified before preparing the functional coating binder.

[0060] The essence of the excellent performance of the functional coating binder provided by the present invention is that the functional monomer containing alkenyl groups exhibits excellent intermolecular interactions (including van der Waals forces and other electrostatic binding forces) after being matched with other monomers; on the one hand, a strong charge force can be formed between the matched functional groups and the aluminum and copper foils of the cathode and anode, so that the functional coating is firmly anchored on the aluminum and copper foil current collectors; on the other hand, after the hot pressing process, the softened functional coating binder can fit well with the positive electrode layer to form an effective van der Waals force, and at the same time, the alkenyl functional monomer and its matched functional groups can form a strong electrostatic binding force with the binder and active material of the dry electrode, so that the interface peeling force is significantly improved.

[0061] Specifically, the present invention preferably has a carboxyl-containing acrylic acid monomer selected from at least one of acrylic acid, methacrylic acid, itaconic acid, β-carboxyethyl acrylate, fumaric acid, and maleic acid; preferably, the aminoalkane is a primary amine or secondary amine with 2 or more carbon atoms, and further preferably, the aminoalkane is selected from at least one of di-n-propylamine and diethylamine.

[0062] In order to take into account both interfacial adhesion and economy, the present invention preferably has a mass ratio range of 1: (1-6) of carboxyl-containing acrylic acid monomer to halogen monomer; a mass ratio range of (0.2-1): 1 of thionyl chloride to addition product; and a mass ratio range of (0.2-1.5): 1 of aminoalkane to acyl chloride monomer.

[0063] The preferred ethylenically unsaturated substance of the present invention is an ethylenically unsaturated carboxylic acid or an ethylenically unsaturated anhydride; specifically, the preferred ethylenically unsaturated substance is at least one selected from acrylic acid, methacrylic acid, itaconic acid, β-carboxyethyl acrylate, fumaric acid, maleic acid, acrylic anhydride, methacrylic anhydride, itaconic anhydride, fumaric anhydride, and maleic anhydride.

[0064] The unsaturated water-soluble monomer of the present invention is preferably selected from at least one of acrylamide, methacrylamide, N-hydroxyethyl acrylamide, 2-acrylamido-2-methylpropane sulfonic acid, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, ethylene glycol methyl ether acrylate, polyethylene glycol methyl ether acrylate, sodium vinyl sulfonate, and sodium p-styrene sulfonate.

[0065] The unsaturated oil-soluble monomer of the present invention is preferably selected from at least one of acrylonitrile, methacrylonitrile, styrene, vinyl acetate, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, isooctyl acrylate, octyl methacrylate, isodecyl acrylate, isodecyl methacrylate and phenyl acrylate.

[0066] To ensure the smooth progress of the polymerization reaction, the initiator of the present invention is preferably selected from one or more of persulfate initiators, hydroperoxide initiators, organic peroxide initiators, diacyl peroxide initiators, azo initiators and oxidation-reduction initiators.

[0067] The pH regulator in the present invention can be an inorganic base or an organic base; the inorganic base can be selected from at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, calcium hydroxide and ammonia water; the organic base can be selected from at least one of ethanolamine, diethanolamine and triethanolamine.

[0068] Further, according to product requirements, the functional coating binder in the present invention, in parts by weight, includes the following raw materials:

[0069] Reaction aid 0.5-40 parts;

[0070] The reaction aid is selected from at least one of a mercaptan aid, a chain transfer agent, and an emulsifier.

[0071] Among them, the mercaptan auxiliary agent is selected from at least one of benzyl mercaptan, p-tert-butyl benzyl mercaptan, dodecyl mercaptan, octadecyl mercaptan, and 2-ethylhexyl mercaptan; the chain transfer agent is a low molecular alcohol or an ether; wherein the low molecular alcohol is selected from at least one of ethanol, isopropanol, 1-4 butanediol, and isohexanediol; the emulsifier is selected from at least one of sodium dodecyl sulfate, sodium dodecyl sulfonate, sodium stearate, potassium stearate, Tween-20, Tween-80, OP-10, OP-20, SE-10, polyethylene glycol, and polyvinyl alcohol.

[0072] The design mechanism of the present invention is: at a temperature of 60-120°C, the binder of the functional coating will partially soften. When external pressure is applied, the polymer chains can fit or even intersperse with the dry active material layer at the interface, and the contact between the conductive carbon materials will also be better, which is manifested macroscopically as very high peeling force and low interface resistance.

[0073] The composition of the present invention is ultimately intended to enhance the bonding strength between the metal foil and the dry active material layer. One side is a metal material and the other side is an inorganic material (containing a polymer binder). The physical and chemical properties of the two sides are very different, so it is necessary to combine a water-soluble monomer and an oily monomer to form a good bond between the two. The ethylenically unsaturated substance selected is a carboxylic acid and an anhydride material. After forming a salt with a pH adjuster, it can exert a good dispersion ability on the carbon material and give the binder a wider processing window. The role of the olefinic functional monomer is that it can soften and fit the active material layer under hot pressing conditions, and the presence of heteroatoms can greatly shorten the jumping distance of electrons at the interface. The macroscopic performance is a reduction in resistance, that is, the improvement of the peeling force and the reduction of resistance are simultaneously manifested.

[0074] Although conventional acrylate monomers can also be hot-pressed, the interface resistance is very large and the rate performance of the battery is obviously inferior; the functional coating adhesive provided by the present invention can reduce the interface resistance while improving the peeling force.

[0075] The functional coating binder provided by the present invention is a water-based product, which is green, environmentally friendly and economical. It has excellent dispersing ability for carbon materials, and no additional dispersing aid is required when preparing the functional coating slurry. The carbon slurry that meets the requirements can be prepared through existing homogenization equipment and processes. At the same time, the functional coating binder has excellent electrochemical stability and excellent conductivity. When applied to electrochemical energy storage devices, it can show excellent service life and give the energy storage device a lower internal resistance. The functional coating binder also has excellent compatibility and universality, and can be applied to the cathode and anode of the device at the same time, and can show excellent comprehensive performance, including high peel strength, low resistance, etc.

[0076] Another object of the present invention is to provide a method for preparing the functional coating binder as described above, the preparation method comprising the following steps:

[0077] S1: According to the formula, the olefinic functional monomer, the ethylenically unsaturated substance, the unsaturated water-soluble monomer, the unsaturated oil-soluble monomer (if the reaction aid is included, the reaction aid is also included) and pure water are mixed, and the mixture is mixed into a uniform liquid component by a stirrer or a homogenizer to obtain a mixed liquid; preferably, a part of the mixed liquid is added to the reactor, and the other part of the mixed liquid is added to the premixing kettle;

[0078] S2: In an inert gas atmosphere, heating a portion of the mixed solution to 40-100° C. to obtain a reaction mixture; preferably, this step is performed as follows: nitrogen is introduced into the reaction kettle to deoxygenate, stirring is started, and the mixed solution in the reaction kettle is slowly heated to 40-100° C. to obtain a reaction mixture;

[0079] S3: Mixing the initiator with water to prepare an initiator solution; preferably, the concentration of the initiator solution is 0.1wt.%-20.0wt.%;

[0080] S4: adding the initiator solution and another part of the mixed solution to the reaction mixture, keeping the mixture warm, and obtaining an aqueous acrylic copolymer glue solution; preferably, this step is performed as follows: slowly adding the initiator solution and the mixed solution in the premixing kettle to the reactor while reacting, keeping the reaction temperature within a preset range, and after all components are added to the reactor, keeping the mixture warm for 30 to 600 minutes to obtain an aqueous acrylic copolymer glue solution;

[0081] S5: Adding a pH adjuster to the aqueous acrylic copolymer adhesive to adjust the pH to 3 to 9, thereby obtaining a functional coating binder having a solid content of 5 to 40.0 wt.%.

[0082] In the preferred step S1 of the present invention, the mass ratio of the mixed liquid in the reaction kettle to the mixed liquid in the premixing kettle is (1-4): (6-9).

[0083] The preparation method of the functional coating binder provided by the present invention has a simple process and is easy to operate; the prepared functional coating binder has excellent hot pressing bonding strength, and when used in dry electrode, it can significantly improve the interface performance, effectively enhance the interface bonding strength, and firmly combine the active material layer with the functional coating current collector, thereby reducing the risk of powder and material loss in subsequent processes, and effectively improving the production yield.

[0084] Another object of the present invention is to provide an electrode sheet, which includes the functional coating binder as described above.

[0085] The functional coating binder provided by the present invention can be used for cathode and anode carbon-coated aluminum and copper foil applications, and is suitable for energy storage devices such as lithium batteries and supercapacitors.

[0086] The electrode sheet provided by the present invention adopts the functional coating adhesive as described above, which can significantly improve the interface performance, effectively enhance the interface adhesion, firmly combine the active material layer with the functional coating current collector, reduce the risk of powder and material loss in subsequent processes, and effectively improve the production yield.

[0087] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0088] Example 1

[0089] This embodiment provides a method for preparing a functional coating binder. Figure 1 As shown, the alkenyl-containing functional monomer is prepared according to the following method:

[0090] S01: adding β-carboxyethyl acrylate and halogen in a mass ratio of 1:3 to obtain an addition product; wherein the halogen is chlorine; the reaction conditions are room temperature, light exposure, and a reaction time of 2 hours;

[0091] S02: The addition product is subjected to acyl chloride by thionyl chloride, the mass ratio of thionyl chloride to the addition product is 0.6:1, and an acyl chloride monomer is obtained; DMF is used as a reaction catalyst, the reaction temperature is 40°C, and the reaction time is 3 hours;

[0092] S03: di-n-propylamine and acyl chloride monomer are subjected to an amidation reaction, the mass ratio of di-n-propylamine to acyl chloride monomer is 0.8:1, the halogen reduction double bond is eliminated, and an amidated acrylic acid monomer, i.e., an olefin-containing functional monomer, is obtained; the acid-binding agent for the amidation reaction is sodium carbonate, the reaction conditions are room temperature, the reaction time is 4 hours, and the reaction is fully stirred; the solvent for the elimination reaction is tetrahydrofuran, the reaction temperature is 45°C, and the reaction time is 3 hours.

[0093] The preparation method of the functional coating binder is as follows:

[0094] S1: According to the weight percentage, 80.0 parts of alkenyl functional monomer, 10.0 parts of itaconic acid, 1.0 parts of sodium p-styrene sulfonate, 9.0 parts of acrylonitrile, 1.0 parts of dodecyl mercaptan, and 2.0 parts of sodium dodecyl sulfate are mixed with 400 parts of pure water, and the raw materials and water are dispersed in a stirrer to mix into a uniform liquid component to obtain a mixed solution; according to the weight, 40% of the mixed solution is added to a reactor, and 60% is added to a premixing kettle;

[0095] S2: After nitrogen is introduced to remove oxygen in the reactor, stirring is started, and the liquid components in the reactor are slowly heated to 70° C. to obtain a reaction mixture;

[0096] S3: dissolving 2.0 parts of initiator ammonium persulfate into pure water to prepare a 2.0 wt.% initiator solution;

[0097] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 70° C., and after all the components are added into the reactor, heat preservation for 60 minutes to obtain a water-based acrylic copolymer glue solution;

[0098] S5: 8.0 parts of sodium hydroxide was added to the aqueous acrylic copolymer glue solution, and the pH was adjusted to 5.1 to obtain a functional coating binder with a solid content of 20.0 wt.%.

[0099] The above 30.0 parts of functional coating binder (6.0 parts by dry weight) and 2.0 parts of conductive carbon black and 6.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 1.0 micron. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained. The slurry was coated on a smooth battery-grade aluminum foil. After drying at 65°C, a functional carbon-coated aluminum foil for dry electrodes with a dense appearance, good consistency and a coating thickness of 1.2 microns was obtained. Figure 2 As shown, the carbon coating layer has excellent bonding strength with the aluminum foil. The carbon coating layer cannot be peeled off from the aluminum foil using 3M test tape, and the actual peel strength is significantly greater than 1000N / m.

[0100] Example 2

[0101] This embodiment provides a method for preparing a functional coating binder, wherein the method for preparing the alkenyl-containing functional monomer is the same as that in Embodiment 1.

[0102] The preparation method of the functional coating binder is as follows:

[0103] S1: According to the weight ratio, 1.0 part of alkenyl-containing functional monomer, 15.0 parts of β-carboxyethyl acrylate, 80.0 parts of ethylene glycol methyl ether acrylate, 4.0 parts of isooctyl acrylate, and 15.0 parts of isopropanol are mixed with 400 parts of pure water, and the raw materials and water are dispersed in a stirrer to mix into a uniform liquid component to obtain a mixed solution; according to the weight, 20% of the mixed solution is added to a reactor, and 80% is added to a premixing kettle;

[0104] S2: After adding 300 parts of pure water and 20% of the mixed liquid into the reactor, nitrogen was introduced to remove the oxygen in the reactor, stirring was started, and the liquid components in the reactor were slowly heated to 70° C. to obtain a reaction mixture;

[0105] S3: dissolving 8.0 parts of initiator potassium persulfate into pure water to prepare a 4.0 wt.% initiator solution;

[0106] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 70° C., and after all the components are added into the reactor, heat preservation treatment is performed for 300 minutes to obtain a water-based acrylic copolymer glue solution;

[0107] S5: Add 6.0 parts of sodium hydroxide to the aqueous acrylic copolymer glue solution, adjust the pH to 3.9, and obtain a functional coating binder with a solid content of 10.0 wt.%.

[0108] The above 80.0 parts of functional coating binder (8.0 parts by dry weight) and 7.0 parts of conductive carbon black and 1.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 1.0 micron. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained. The slurry was coated on a smooth battery-grade copper foil. After drying at 95°C, a functional carbon-coated copper foil for dry electrodes with a dense appearance, good consistency and a coating thickness of 1.1 microns was obtained. Figure 3 As shown, the carbon coating layer has excellent bonding strength with the copper foil. The carbon coating layer cannot be peeled off from the copper foil using 3M test tape. The actual peel strength is much greater than 1200N / m.

[0109] Example 3

[0110] This embodiment provides a method for preparing a functional coating binder, wherein the method for preparing an olefinic functional monomer is compared with that in Example 1, except that the di-n-propylamine in step S03 is replaced by diethylamine; the acid binding agent in the amidation reaction is changed to sodium bicarbonate, the reaction conditions are room temperature, the reaction time is 3 hours, and sufficient stirring is performed.

[0111] The preparation method of the functional coating binder is as follows:

[0112] S1: According to weight parts, 12.0 parts of alkenyl-containing functional monomers, 27.0 parts of acrylic acid, 40.0 parts of hydroxyethyl methacrylate, 20.0 parts of acrylamide, 1.0 parts of vinyl acetate, and 10.0 parts of ethanol are mixed with 500 parts of pure water, and the raw materials and water are dispersed in a stirrer to mix into a uniform liquid component to obtain a mixed liquid; according to weight, 30% of the mixed liquid is added to a reactor, and 70% is added to a premixing kettle;

[0113] S2: After adding 100 parts of pure water and 30% of the mixed liquid into the reactor, nitrogen was introduced to remove the oxygen in the reactor, stirring was started, and the liquid components in the reactor were slowly heated to 65° C. to obtain a reaction mixture;

[0114] S3: Dissolve 5.0 parts of initiator ammonium persulfate and sodium bisulfite in pure water to prepare a 4.0 wt.% initiator solution;

[0115] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 65° C., and after all the components are added into the reactor, heat preservation treatment is performed for 180 minutes to obtain a water-based acrylic copolymer glue solution;

[0116] S5: 18.0 parts of sodium hydroxide was added to the aqueous acrylic copolymer glue solution, and the pH was adjusted to 6.6 to obtain a functional coating binder with a solid content of 12.0 wt.%.

[0117] The above 80.0 parts of functional coating binder (9.6 parts by dry weight) and 7.0 parts of conductive carbon black and 3.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 1.0 micron. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained, which was coated on a smooth battery-grade aluminum foil. After drying at 75°C, a functional carbon-coated aluminum foil for dry electrodes with a dense appearance, good consistency and a coating thickness of 1.0 micron was obtained; then, a dry positive electrode sheet was prepared on the dry electrode-specific carbon-coated aluminum foil using a dry electrode process, and its 180° peel strength reached 120N / m, which was much higher than 8N / m of the conventional carbon-coated aluminum foil (Comparative Example 1), achieving an increase of more than 10 times in peel strength, such as Figure 4 shown.

[0118] Example 4

[0119] This embodiment provides a method for preparing a functional coating binder, wherein the method for preparing the alkenyl-containing functional monomer is the same as that in Embodiment 3.

[0120] The preparation method of the functional coating binder is as follows:

[0121] S1: According to the weight ratio, 30.0 parts of alkenyl-containing functional monomers, 5.0 parts of methacrylic acid, 45.0 parts of hydroxyethyl methacrylate, 15.0 parts of 2-acrylamido-2-methylpropanesulfonic acid, 5.0 parts of methyl acrylate, 3.0 parts of sodium stearate, and 1.0 part of benzyl mercaptan are mixed with 300 parts of pure water, and the raw materials and water are dispersed in a stirrer to mix into a uniform liquid component to obtain a mixed solution; according to the weight, 20% of the mixture is added to the reactor, and 80% is added to the premixing kettle;

[0122] S2: After adding 60 parts of pure water and 20% of the mixed liquid into the reactor, nitrogen was introduced to remove the oxygen in the reactor, stirring was started, and the liquid components in the reactor were slowly heated to 75° C. to obtain a reaction mixture;

[0123] S3: dissolving 3.0 parts of initiator potassium persulfate into pure water to prepare a 3.0 wt.% initiator solution;

[0124] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 75° C., and after all the components are added into the reactor, heat preservation treatment is performed for 120 minutes to obtain a water-based acrylic copolymer glue solution;

[0125] S5: 9.0 parts of sodium hydroxide was added to the aqueous acrylic copolymer glue solution, and the pH was adjusted to 5.7 to obtain a functional coating binder with a solid content of 22.0 wt.%.

[0126] The above 35.0 parts of functional coating binder (7.7 parts by dry weight) and 8.0 parts of conductive carbon black and 2.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 0.9 microns. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained, which was coated on a smooth battery-grade copper foil. After drying at 70°C, a functional carbon-coated copper foil for dry electrodes with a dense appearance, good consistency and a coating thickness of 1.1 microns was obtained; a dry negative electrode sheet was prepared on this dry electrode-specific carbon-coated copper foil using a dry electrode process, and its 180° peel strength was 37N / m, which was higher than 5N / m of a conventional carbon-coated copper foil (Comparative Example 6). The resistivity of its dry negative electrode sheet was 0.31Ω·cm, which was significantly better than 1.9Ω·cm of a conventional carbon-coated copper foil (Comparative Example 6).

[0127] Example 5

[0128] This embodiment provides a method for preparing a functional coating binder, wherein the method for preparing the alkenyl-containing functional monomer is the same as that in Embodiment 3.

[0129] The preparation method of the functional coating binder is as follows:

[0130] S1: According to the weight percentage, 5.0 parts of alkenyl functional monomer, 80.0 parts of maleic acid, 10.0 parts of hydroxypropyl methacrylate, 5.0 parts of ethyl methacrylate, and 0.5 parts of octadecyl mercaptan are mixed with 200 parts of pure water, and the raw materials and water are dispersed in a blender to mix into a uniform liquid component to obtain a mixed solution; according to the weight, 10% of the mixed solution is added to a reactor, and 90% is added to a premixing kettle;

[0131] S2: After adding 100 parts of pure water and 10% of the mixed liquid into the reactor, nitrogen was introduced to remove the oxygen in the reactor, stirring was started, and the liquid components in the reactor were slowly heated to 80° C. to obtain a reaction mixture;

[0132] S3: dissolving 4.0 parts of initiator ammonium persulfate into pure water to prepare a 2.0 wt.% initiator solution;

[0133] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 80° C., and after all the components are added into the reactor, heat preservation treatment is performed for 90 minutes to obtain a water-based acrylic copolymer glue solution;

[0134] S5: Add 40.0 parts of sodium hydroxide to the aqueous acrylic copolymer glue solution, adjust the pH to 4.2, and obtain a functional coating binder with a solid content of 25.0 wt.%.

[0135] The above 40.0 parts of functional coating binder (10.0 parts by dry weight) and 9.0 parts of conductive carbon black and 1.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 0.9 microns. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained, which was coated on a smooth battery-grade aluminum foil. After drying at 90°C, a functional carbon-coated aluminum foil for dry electrodes with a dense appearance, good consistency and a coating thickness of 0.9 microns was obtained; then, a dry positive electrode sheet was prepared on this dry electrode-specific carbon-coated aluminum foil using a dry electrode process, and its 180° peel strength was 52N / m, which was much higher than that of conventional carbon-coated aluminum foil (Comparative Example 7). The resistivity of its dry positive electrode sheet was 18.2Ω·cm, which was significantly better than 76.1Ω·cm of conventional carbon-coated aluminum foil (Comparative Example 7).

[0136] Example 6

[0137] This embodiment provides a method for preparing a functional coating binder, wherein the method for preparing an olefinic functional monomer is different from that in Embodiment 1, except that the β-carboxyethyl acrylate in step S01 is replaced by acrylic acid.

[0138] The preparation method of the functional coating binder is as follows:

[0139] S1: According to the weight percentage, 19.0 parts of olefinic functional monomer, 1.0 part of fumaric acid, 20.0 parts of sodium vinyl sulfonate, 20.0 parts of butyl acrylate, 40.0 parts of ethyl acrylate, 2.0 parts of OP-10, 5.0 parts of sodium dodecyl sulfonate, all are mixed with 300 parts of pure water, and the raw materials and water are dispersed in a stirrer to mix into a uniform liquid component to obtain a mixed solution; according to the weight, 30% of it is added to the reactor, and 70% is added to the premixing kettle;

[0140] S2: After adding 200 parts of pure water and 30% of the mixed liquid into the reactor, nitrogen was introduced to remove the oxygen in the reactor, stirring was started, and the liquid components in the reactor were slowly heated to 58° C. to obtain a reaction mixture;

[0141] S3: dissolving 6.0 parts of initiator sodium persulfate into pure water to prepare a 3.0 wt.% initiator solution;

[0142] S4: slowly adding the initiator solution and the liquid components in the premixed kettle into the reactor while reacting, maintaining the reaction temperature at 58° C., and after all the components are added into the reactor, heat preservation treatment is performed for 300 minutes to obtain a water-based acrylic copolymer glue solution;

[0143] S5: Add 2.5 parts of sodium hydroxide to the aqueous acrylic copolymer glue solution, adjust the pH to 7.3, and obtain a functional coating binder with a solid content of 18.0 wt.%.

[0144] The above 50.0 parts of functional coating binder (9.0 parts by dry weight) and 6.0 parts of conductive carbon black and 2.0 parts of graphite were fully dispersed and ground to obtain a uniform carbon slurry with a D50 particle size of less than 1.0 micron. After adjusting the solid content, a functional coating slurry for dry electrodes was obtained, which was coated on a smooth battery-grade aluminum foil. After drying at 90°C, a functional carbon-coated aluminum foil with a dense appearance, good consistency and a coating thickness of 1.0 micron was obtained for dry electrodes. Then, a dry positive electrode sheet was prepared on this dry electrode-specific carbon-coated aluminum foil using a dry electrode process, and its 180° peel strength was 56N / m, which was much higher than that of conventional carbon-coated aluminum foil. The resistivity of its dry positive electrode sheet is 21.7Ω·cm, which is significantly better than that of conventional carbon-coated aluminum foil. The dry positive electrode sheet was assembled into a soft-pack battery, and its impedance was reduced by 10.4% compared with conventional carbon-coated aluminum foil, and the 3C rate discharge capacity of the soft-pack battery was increased by 17.7%.

[0145] Example 7

[0146] The difference between this embodiment and embodiment 4 is that the amount of the functional monomer containing alkenyl groups is adjusted from 30.0 parts to 1.0 parts. The results show that the dispersion performance and the conductivity are normal. The carbon-coated aluminum foil can be prepared by the same process. The 180° peel strength of the dry-process positive electrode layer is 10N / m, which is higher than the 5N / m of the conventional carbon-coated copper foil (Comparative Example 6). The resistivity of the dry-process negative electrode sheet is 0.87Ω·cm, which is better than the 1.9Ω·cm of the conventional carbon-coated copper foil (Comparative Example 6).

[0147] Example 8

[0148] The difference between this comparative example and Example 4 is that the amount of the functional monomer containing alkenyl groups is adjusted from 30.0 parts to 80.0 parts. The results show that the dispersion performance and the conductivity are normal. The carbon-coated aluminum foil can be prepared by the same process. The 180° peel strength of the dry-process negative electrode layer is 16N / m, which is higher than the 5N / m of the conventional carbon-coated copper foil (Comparative Example 6). The resistivity of the dry-process negative electrode sheet is 0.75Ω·cm, which is better than the 1.9Ω·cm of the conventional carbon-coated copper foil (Comparative Example 6).

[0149] Example 9

[0150] The difference between this comparative example and Example 4 is that the amount of the functional monomer containing alkenyl groups is adjusted from 30.0 parts to 15.0 parts. The results show that the dispersion performance and the conductivity are normal. The carbon-coated aluminum foil can be prepared by the same process. The 180° peel strength of the dry-process negative electrode layer is 23N / m, which is higher than the 5N / m of the conventional carbon-coated copper foil (Comparative Example 6). The resistivity of the dry-process negative electrode sheet is 0.55Ω·cm, which is better than the 1.9Ω·cm of the conventional carbon-coated copper foil (Comparative Example 6).

[0151] Example 10

[0152] The difference between this comparative example and Example 4 is that the amount of the functional monomer containing alkenyl groups is adjusted from 30.0 parts to 45.0 parts. The results show that the dispersion performance and the conductivity are normal. The carbon-coated aluminum foil can be prepared by the same process. The 180° peel strength of the dry-process negative electrode layer is 28N / m, which is higher than the 5N / m of the conventional carbon-coated copper foil (Comparative Example 6). The resistivity of the dry-process negative electrode sheet is 0.43Ω·cm, which is better than the 1.9Ω·cm of the conventional carbon-coated copper foil (Comparative Example 6).

[0153] Comparative Example 1

[0154] This comparative example uses a mature functional carbon-coated binder (Derby DC-611) on the market for evaluation. The results show that its dispersion performance and conductive performance are normal. The same process as Example 3 can be used to prepare a conventional carbon-coated aluminum foil, but its peeling force with the dry positive electrode layer is very small, and the 180° peeling strength is only 8N / m, which is much lower than the 120N / m that can be achieved in Example 3.

[0155] Comparative Example 2

[0156] The difference between this comparative example and Example 3 is that the alkenyl-containing functional monomer is replaced with acrylic acid. The results show that the dispersion performance and the conductive performance are normal, and the carbon-coated aluminum foil can be prepared by the same process, but the peeling force between the foil and the dry positive electrode layer is very small, and the 180° peeling strength is only 9 N / m, which is much lower than the 120 N / m that can be achieved in Example 3.

[0157] Comparative Example 3

[0158] The difference between this comparative example and Example 4 is that no alkenyl-containing functional monomer is added. The results show that its dispersion performance and conductivity are normal, and the carbon-coated copper foil can be prepared using the same process, but its peeling force with the dry-process negative electrode layer is very small, and the 180° peeling strength is only 6N / m, which is much lower than the 37N / m that can be achieved in Example 4. In addition, the resistivity of its dry-process negative electrode sheet is 1.8Ω·cm, which is much worse than the 0.31Ω·cm that can be achieved in Example 4.

[0159] Comparative Example 4

[0160] The difference between this comparative example and Example 5 is that the functional monomer containing alkenyl is replaced with 2-aminoethyl methacrylate with a similar chemical structure. The results show that its dispersion performance and conductivity are normal, and the carbon-coated aluminum foil can be prepared using the same process, but its peeling force with the dry-process positive electrode layer is very small, and the 180° peeling strength is only 13N / m, which is much lower than the 112N / m that can be achieved in Example 5. In addition, the resistivity of its dry-process positive electrode sheet is 69.1Ω·cm, which is much worse than the 18.2Ω·cm that can be achieved in Example 4.

[0161] Comparative Example 5

[0162] The difference between this comparative example and Example 6 is that the functional monomer containing alkenyl is replaced with acrylic acid isooctanoic acid; the results show that its dispersion performance and conductivity are normal, and the carbon-coated aluminum foil can be prepared by the same process, but its peeling force with the dry positive electrode layer is very small, and the 180° peeling strength is only 7N / m, which is much lower than the 116N / m that can be achieved in Example 6. In addition, the resistivity of its dry positive electrode sheet is 71.0Ω·cm, which is much worse than the 21.7Ω·cm that can be achieved in Example 6. After being assembled into a soft-pack battery, its impedance and 3C rate discharge capacity are both inferior to those of Example 6.

[0163] Comparative Example 6

[0164] This comparative example uses a mature functional carbon-coated binder (Derby DC-611) in the market for evaluation. The results show that its dispersion performance and conductivity are normal. The same process as Example 4 can be used to prepare a conventional carbon-coated copper foil. However, when used for a dry-process negative electrode sheet, its 180° peel strength is 5 N / m, and the resistivity of the dry-process negative electrode sheet is 1.9 Ω·cm.

[0165] Comparative Example 7

[0166] This comparative example uses a mature functional carbon-coated binder (Derby DC-611) in the market for evaluation. The results show that its dispersion performance and conductivity are normal. The same process as Example 5 can be used to prepare a conventional carbon-coated aluminum foil. However, when used for a dry-process positive electrode sheet, its 180° peel strength is 7 N / m, and the resistivity of the dry-process positive electrode sheet is 76.1 Ω·cm.

[0167] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A functional coating binder, characterized in that: The raw materials include the following components in parts by weight: 1-80 parts of alkenyl-containing functional monomers; 1-80 parts of ethylenically unsaturated substances; 1-80 parts of unsaturated water-soluble monomer; 1-80 parts of unsaturated oil-soluble monomer; Initiator 0.1-20 parts; 1-60 parts of pH regulator; The alkenyl-containing functional monomer is an amidated acrylic acid monomer; The alkenyl-containing functional monomer is prepared according to the following method: S01: firstly adding a carboxyl-containing acrylic acid monomer to a halogen element to obtain an addition product; S02: chlorinating the addition product with thionyl chloride to obtain an acyl chloride monomer; S03: subjecting the aminoalkane to an amidation reaction with the acyl chloride monomer to eliminate the halogen-reduced double bond, thereby obtaining an olefin-containing functional monomer; The aminoalkane is selected from at least one of di-n-propylamine and diethylamine; The carboxyl-containing acrylic acid monomer is β-carboxyethyl acrylate; The unsaturated water-soluble monomer is ethylene glycol methyl ether acrylate; The unsaturated oil-soluble monomer is isooctyl acrylate.

2. The functional coating binder according to claim 1, characterized in that: The mass ratio of the carboxyl-containing acrylic monomer to the halogen monomer is in the range of 1:(1-6); the mass ratio of the dichlorothionyl to the addition product is in the range of (0.2-1):1; the mass ratio of the aminoalkane to the acyl chloride monomer is in the range of (0.2-1.5):

1.

3. The functional coating binder according to claim 1, characterized in that: The ethylenically unsaturated substance is selected from at least one of acrylic acid, methacrylic acid, itaconic acid, β-carboxyethyl acrylate, fumaric acid, maleic acid, acrylic anhydride, methacrylic anhydride, itaconic anhydride, fumaric anhydride, and maleic anhydride.

4. The functional coating binder according to any one of claims 1 to 3, characterized in that: In parts by weight, it also includes: Reaction aid 0.5-40 parts; The reaction aid is selected from at least one of a thiol aid, a chain transfer agent, and an emulsifier.

5. A method for preparing a functional coating binder according to any one of claims 1 to 4, characterized in that: The steps include: S1: mixing the alkenyl-containing functional monomer, the ethylenically unsaturated substance, the unsaturated water-soluble monomer, the unsaturated oil-soluble monomer and pure water according to the formula amount to obtain a mixed solution; S2: In an inert gas atmosphere, heating a portion of the mixed solution to 40-100° C. to obtain a reaction mixed solution; S3: mixing an initiator with water to prepare an initiator solution; S4: adding the initiator solution and another part of the mixed solution into the reaction mixed solution, keeping the temperature, to obtain an aqueous acrylic copolymer glue solution; S5: adding a pH adjuster to the aqueous acrylic copolymer glue to obtain a functional coating binder.

6. An electrode sheet, characterized in that: The invention comprises the functional coating binder as claimed in any one of claims 1 to 4.

Citation Information

Patent Citations

  • Binder composition for secondary battery

    CN114342124A

  • Modified acrylic resin, preparation method thereof and secondary battery carbon coating

    CN114957522A

  • Water-based water-resistant anode functional coating binder as well as preparation method and application thereof

    CN115304974A

  • Water-soluble binder, battery pole piece and application of water-soluble binder

    CN117720869A

  • Negative electrode for lithium ion secondary battery, and its forming method

    JP2010182548A