Metal matrix composite material and preparation method thereof, fin, heat exchanger and application thereof

By adding graphene derivatives with specific sheet diameters and contents on the surface of the metal substrate to form a functional coating, the problem of reduced thermal conductivity and corrosion resistance caused by the aging of the heat exchanger coating is solved, and high thermal conductivity, corrosion resistance and corrosion resistance are achieved. The combination of weather resistance performance improves the overall performance of the air conditioner.

CN118442873BActive Publication Date: 2024-10-11GD MIDEA AIR CONDITIONING EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410903326.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The coating on the surface of the metal substrate of the existing heat exchanger ages in a complex environment, resulting in reduced thermal conductivity and increased energy consumption. It is also difficult to balance corrosion resistance, weather resistance and processing and production problems.

Method used

Add graphene and/or its derivatives to the surface of the metal substrate to form a functional coating with a thickness of 0.8~1.5 microns. Combined with graphene and/or its derivatives of specific sheet diameter and content, it improves thermal conductivity and maintains corrosion resistance. and weather resistance.

Benefits of technology

With a thin coating thickness, the high thermal conductivity, corrosion resistance and weather resistance of metal matrix composites are achieved, simplifying processing and production, reducing energy consumption, and improving the reliability and service life of the heat exchanger.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118442873B_ABST
    Figure CN118442873B_ABST
Patent Text Reader

Abstract

The present invention discloses a metal-based composite material and a preparation method thereof, a fin, a heat exchanger and its application, and relates to the technical field of heat exchange materials. The metal-based composite material comprises a metal substrate and a functional coating; the functional coating is arranged on at least one surface of the metal substrate; the functional coating comprises at least an anti-corrosion layer; the anti-corrosion layer comprises an organic coating containing graphene and / or its derivatives; the thickness of the solidified anti-corrosion layer is 0.8 to 1.5 microns; the sheet diameter of graphene and / or its derivatives is 1 to 8 microns, and the content thereof in the solidified anti-corrosion layer is 0.5 to 4.5 wt%; the thermal diffusion coefficient of the composite material in the vertical direction is ≥28 mm 2 / s. The metal-based composite material of the present invention can have excellent thermal conductivity with a thin coating thickness, and has both corrosion resistance and weather resistance, and is easy to process and produce, and can be applied to make fins, heat exchangers or air handling devices, which can greatly improve their reliability, service life and energy-saving and long-term effectiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat exchange materials, and in particular to a metal-based composite material and a preparation method thereof, a fin, a heat exchanger and applications thereof. Background Art

[0002] As the core heat exchange component of the air conditioner, the performance of the heat exchanger is directly related to the overall performance of the air conditioner. In order to improve drainage performance and reduce performance degradation caused by corrosion, a hydrophilic anti-corrosion functional coating is generally applied to the surface of the metal substrate of the heat exchanger. However, during the use of the air conditioner, the coating on the surface of the metal heat sink will crack and fall off at the edge in a complex service environment, which will not only directly affect the performance of the organic coating, but also cause large-scale corrosion of the substrate. Taking the aluminum foil substrate as an example, after testing, aluminum foil corrosion can reduce the heat exchange performance of the air conditioner by more than 20% and increase energy consumption by 16%.

[0003] In response to the above problems, existing technical solutions include using a high corrosion protection system or increasing the coating thickness. At present, the mainstream high corrosion protection system mostly uses an epoxy system or a fluorine-containing system. The epoxy system has poor light aging resistance, which causes its corrosion resistance to decay rapidly during service; the fluorine-containing system has a high cost and is not suitable for large-scale promotion and use. It also has poor compatibility with the topcoat hydrophilic layer and poor performance balance. As for increasing the coating thickness, although the initial corrosion resistance can be improved, the thermal conductivity of the organic coating is significantly lower than that of the metal substrate. After the coating is thickened, the energy consumption of the air conditioner increases, which leads to energy waste. In addition, the increase in coating thickness will also bring difficulties in coating manufacturing and processing. Therefore, the existing heat exchanger coating cannot solve the above technical contradictions, and there are problems such as failure to take into account corrosion resistance, weather resistance and thermal conductivity, or difficulty in processing and production. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art.

[0005] By adding graphene and / or its derivatives to the anti-corrosion layer on the surface of the metal substrate, the present invention can achieve a metal-based composite material with a thin coating thickness that can take into account thermal conductivity, corrosion resistance and weather resistance, and is easy to process and produce.

[0006] To this end, one of the purposes of the present invention is to provide a metal-based composite material that can reduce the impact on thermal conductivity while meeting long-term anti-corrosion requirements and has good aging resistance. At the same time, it can be processed and prepared under the process conditions of existing production equipment and has broad prospects for application in heat exchangers and air treatment devices.

[0007] A second object of the present invention is to provide a method for preparing the above-mentioned metal-based composite material.

[0008] A third object of the present invention is to provide a fin.

[0009] A fourth object of the present invention is to provide a heat exchanger.

[0010] A fifth object of the present invention is to provide an air treatment device.

[0011] A first aspect of the present invention provides a metal matrix composite material, comprising a metal substrate and a functional coating; the functional coating is disposed on at least one surface of the metal substrate;

[0012] Wherein, the functional coating at least includes an anti-corrosion layer;

[0013] The anti-corrosion layer includes an organic coating containing graphene and / or its derivatives;

[0014] The thickness of the cured anti-corrosion layer is 0.8 microns to 1.5 microns;

[0015] The sheet diameter of the graphene and / or its derivatives is 1 micron to 8 microns;

[0016] The content of the graphene and / or its derivatives in the cured anti-corrosion layer is 0.5wt% to 4.5wt%;

[0017] The thermal diffusion coefficient of the metal matrix composite material in the vertical direction is ≥28 mm 2 / s.

[0018] The metal matrix composite material according to the embodiment of the present invention has at least the following beneficial effects:

[0019] Metal-based composite materials use graphene high-corrosion protection coatings, which can have excellent thermal conductivity at a thin coating thickness, while taking into account corrosion resistance and weather resistance, and are easy to process and prepare under the process conditions of existing production equipment.

[0020] Furthermore, the anti-corrosion layer of the metal-based composite material contains graphene and / or its derivatives with specific flake diameter specifications and content, which can have high thermal conductivity, corrosion resistance and high weather resistance at a coating thickness as thin as 0.8~1.5 microns, and is easy to process and produce.

[0021] Specifically, by selecting graphene and / or its derivatives with a sheet diameter of 1 micron to 8 microns and a content of 0.5wt% to 4.5wt% in the solidified anti-corrosion layer, the prepared metal-based composite material can have high weather resistance, high thermal conductivity and corrosion resistance at the same time. If the sheet diameter of graphene and / or its derivatives is too small or too large, or the content of graphene and / or its derivatives is too small or too large, it cannot be matched with the thickness of the anti-corrosion layer to take into account corrosion resistance, weather resistance and thermal conductivity at the same time. For example, if the sheet diameter of graphene and / or its derivatives is too large, it will penetrate the anti-corrosion layer and affect corrosion resistance and weather resistance; if the content of graphene and / or its derivatives in the anti-corrosion layer is too small, it cannot play its role; if the content of graphene and / or its derivatives in the anti-corrosion layer is too large, it is easy to be unevenly dispersed or agglomerated, which will also affect corrosion resistance and weather resistance.

[0022] The thickness of the anti-corrosion layer described in the embodiment of the present invention refers to the thickness of the single-sided coating.

[0023] According to some embodiments of the present invention, the number of layers of the graphene and / or its derivatives is 1 to 10 layers.

[0024] According to some embodiments of the present invention, the maximum sheet diameter of the graphene and / or its derivatives is ≤ 5 times the thickness of the anti-corrosion layer.

[0025] The maximum sheet diameter of the graphene and / or its derivatives described in the embodiments of the present invention refers to the maximum value among the sheet diameters of the graphene and / or its derivatives.

[0026] According to some embodiments of the present invention, the sheet diameter of the graphene and / or its derivatives is 1 micron to 3 microns. The selection of graphene and / or its derivatives in such a sheet diameter range can better match the thickness of the anti-corrosion layer and the content of graphene and / or its derivatives in the anti-corrosion layer, so that the prepared metal-based composite material has high corrosion resistance and high weather resistance in addition to high thermal conductivity.

[0027] According to some embodiments of the present invention, the thermal diffusion coefficient of the metal matrix composite material in the vertical direction is 28 mm 2 / s~40mm 2 / s. The metal matrix composite material has such a range of thermal diffusion coefficients, reflecting high thermal conductivity. Among them, the vertical direction is also called the longitudinal direction, which refers to the thickness direction of the metal matrix composite material.

[0028] According to some embodiments of the present invention, the thermal diffusion coefficient is measured at a temperature of 50°C.

[0029] According to some embodiments of the present invention, in the organic coating forming the anti-corrosion layer, the mass percentage of graphene and / or its derivatives is 0.5% to 2%. By adding such a range of graphene and / or its derivatives to the organic coating forming the anti-corrosion layer, the content of graphene and / or its derivatives in the finally formed solidified anti-corrosion layer can be 0.5wt% to 4.5wt%.

[0030] According to some embodiments of the present invention, the anti-corrosion layer is an amide-modified acrylic resin coating or an epoxy-modified acrylic resin coating, and the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating contains graphene and / or its derivatives. By using the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating containing graphene and / or its derivatives as the anti-corrosion layer, the metal-based composite material can have good anti-corrosion performance.

[0031] According to some embodiments of the present invention, the graphene derivatives include graphene oxide, reduced graphene oxide or grafted modified graphene, etc.

[0032] According to some embodiments of the present invention, the overall weight loss rate of the metal-based composite material in the alkali resistance test is less than 6%. In this way, the metal-based composite material has good alkali resistance and high corrosion resistance. The alkali resistance test refers to testing the metal-based composite material in 100g / L sodium hydroxide solution, the test temperature is 20℃±2℃, and the test time is 1 hour.

[0033] According to some embodiments of the present invention, after 1500 hours of neutral salt spray test, the corrosion area of ​​the metal-based composite material is ≤0.02%. Thus, the metal-based composite material has good neutral salt spray resistance and high corrosion resistance.

[0034] According to some embodiments of the present invention, the corrosion area grade of the weather resistance test of the metal-based composite material is ≥ grade 8. In this way, the metal-based composite material has high weather resistance and excellent aging resistance. The weather resistance test refers to subjecting the metal-based composite material to 120 hours of ultraviolet light and 72 hours of neutral salt spray test in sequence.

[0035] According to some embodiments of the present invention, two surfaces of the metal substrate that are opposite to each other in the thickness direction are provided with functional coatings, and the functional coatings include an anti-corrosion layer.

[0036] According to some embodiments of the present invention, the functional coating further comprises a hydrophilic layer, which is disposed on the surface of the anti-corrosion layer away from the metal substrate. Providing the hydrophilic layer can enhance the hydrophilic effect of the metal matrix composite material and improve the decontamination ability.

[0037] According to some embodiments of the present invention, the functional coating further comprises:

[0038] A hydrophilic layer, the hydrophilic layer being disposed on a surface of the anti-corrosion layer away from the metal substrate;

[0039] A lubricating layer is disposed on a surface of the hydrophilic layer away from the metal substrate.

[0040] Further providing a lubricating layer can protect the hydrophilic layer and the anti-corrosion layer, so that the functional coating has better corrosion resistance and hydrophilicity.

[0041] According to some embodiments of the present invention, the metal substrate includes aluminum, copper, iron or alloys thereof. All of these substrates have good thermal conductivity.

[0042] The second aspect of the present invention provides a method for preparing the metal matrix composite material according to the first aspect of the present invention, comprising the following steps:

[0043] A coating is applied on at least one surface of a metal substrate to form a functional coating to obtain the metal-based composite material.

[0044] The method for preparing the metal-based composite material according to the embodiment of the present invention has at least the following beneficial effects:

[0045] The preparation method of the metal matrix composite material is simple to operate and easy to control. It can be processed and prepared under the process conditions of existing production equipment and is suitable for large-scale industrial production applications.

[0046] The third aspect of the present invention provides a fin having a thickness of 0.05 mm to 0.12 mm, and the fin comprises the metal-based composite material described in the first aspect of the present invention, or the metal-based composite material obtained by the preparation method described in the second aspect of the present invention.

[0047] The fin according to the embodiment of the present invention has at least the following beneficial effects:

[0048] The fin has all the characteristics and advantages of the aforementioned metal-based composite materials, and also has corrosion resistance, weather resistance and thermal conductivity, and is easy to produce.

[0049] A fourth aspect of the present invention provides a heat exchanger, comprising the fins described in the third aspect of the present invention.

[0050] The heat exchanger according to the embodiment of the present invention has at least the following beneficial effects:

[0051] The heat exchanger has all the characteristics and advantages of the aforementioned fins, and can also take into account corrosion resistance, weather resistance and thermal conductivity. It is easy to produce and manufacture, and can greatly improve the reliability, service life and energy saving of the heat exchanger.

[0052] The fifth aspect of the present invention provides an air treatment device, comprising the metal-based composite material described in the first aspect of the present invention, or the metal-based composite material obtained by the preparation method described in the second aspect of the present invention, or the fin described in the third aspect of the present invention, or the heat exchanger described in the fourth aspect of the present invention.

[0053] The air treatment device according to the embodiment of the present invention has at least the following beneficial effects:

[0054] The air handling device has all the characteristics and advantages of the aforementioned metal matrix composite materials, fins or heat exchangers, and can achieve a significant improvement in reliability, service life and energy saving and long-term effectiveness.

[0055] According to some embodiments of the present invention, the air treatment device is an air conditioner or a dehumidifier.

[0056] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 is a schematic diagram of a metal matrix composite material according to an embodiment of the present invention;

[0058] Figure 2 is a schematic diagram of a metal matrix composite material according to another embodiment of the present invention;

[0059] Figure 3 is a schematic diagram of a metal matrix composite material according to another embodiment of the present invention;

[0060] Figure 4 is a schematic diagram of a metal matrix composite material according to another embodiment of the present invention;

[0061] Figure 5 is a schematic diagram of a metal matrix composite material according to another embodiment of the present invention;

[0062] Figure 6 is a schematic diagram of a fin according to an embodiment of the present invention;

[0063] Figure 7 It is the thermal diffusion coefficient diagram of the coated aluminum foil sample in the vertical direction at 50°C;

[0064] Figure 8 This is the overall weight loss percentage chart of the coated aluminum foil sample in the alkali resistance test;

[0065] Fig. 9 It is the corrosion rating diagram of the coated aluminum foil specimen after acetic acid salt spray test at different times;

[0066] Fig.10It is the weather resistance test rating chart of the coated aluminum foil sample;

[0067] Fig.11 This is a performance comparison chart of two types of heat exchanger prototypes 9 months after the air conditioner was installed.

[0068] Reference numerals:

[0069] The metal substrate 100,

[0070] Functional coating 200,

[0071] Anti-corrosion layer 210, first anti-corrosion layer 211, second anti-corrosion layer 212,

[0072] hydrophilic layer 220, first hydrophilic layer 221, second hydrophilic layer 222,

[0073] Lubricating layer 230, first lubricating layer 231, second lubricating layer 232,

[0074] Fins 300. DETAILED DESCRIPTION

[0075] Embodiments of the present invention are described in detail below. The embodiments described with reference to the accompanying drawings are exemplary and are only used to explain the present invention, but should not be construed as limiting the present invention.

[0076] In the description of the present invention, it should be understood that the terms "length", "width", "thickness", "upper", "lower", "inner", "outer" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, features defined as "first" or "second" may explicitly or implicitly include one or more of the features.

[0077] One aspect of the present invention provides an embodiment of a metal matrix composite material. Figures 1 to 5 A metal matrix composite material according to an embodiment of the present invention is described.

[0078] Reference Figure 1The metal matrix composite material of the embodiment of the present invention comprises a metal substrate 100 and a functional coating 200, wherein the functional coating 200 is disposed on one surface of the metal substrate 100. The functional coating 200 comprises an anti-corrosion layer; the anti-corrosion layer comprises an organic coating containing graphene and / or its derivatives; the thickness of the cured anti-corrosion layer is 0.8 microns to 1.5 microns; the sheet diameter of the graphene and / or its derivatives is 1 micron to 8 microns; the content of the graphene and / or its derivatives in the cured anti-corrosion layer is 0.5wt% to 4.5wt%; the thermal diffusion coefficient of the metal matrix composite material in the vertical direction is ≥28mm 2 / s. According to the embodiments of the present invention, the anti-corrosion layer of the metal-based composite material contains graphene and / or its derivatives with specific sheet diameter specifications and contents, and the two are combined with the anti-corrosion layer thickness of 0.8 to 1.5 microns to play a synergistic role, and can take into account corrosion resistance and weather resistance at a thin coating thickness while having excellent thermal conductivity, which is convenient for processing and preparation under the process conditions of existing production equipment.

[0079] In some embodiments of the present invention, the thickness of the solidified anti-corrosion layer may be 0.8 microns, 0.9 microns, 1.0 microns, 1.1 microns, 1.2 microns, 1.3 microns, 1.4 microns, or 1.5 microns, etc. In some examples, the thickness of the solidified anti-corrosion layer may be 0.8 microns to 1.4 microns. In other examples, the thickness of the solidified anti-corrosion layer may be 0.8 microns to 1.2 microns. In other examples, the thickness of the solidified anti-corrosion layer may be 1 micron to 1.2 microns.

[0080] In some embodiments of the present invention, the sheet diameter of graphene and / or its derivatives may be 1 micron to 6 microns or 3 microns to 8 microns, etc. In some examples, the sheet diameter of graphene and / or its derivatives may be 1 micron to 3 microns. In some examples, the sheet diameter of graphene and / or its derivatives may be 3 microns to 6 microns. In some examples, the sheet diameter of graphene and / or its derivatives may be 3 microns to 8 microns. Graphene and / or its derivatives may be a mixture of graphene and / or its derivatives with multiple different sheet diameters, and the sheet diameter of graphene and / or its derivatives may be a range.

[0081] In some embodiments of the present invention, the content of graphene and / or its derivatives in the cured anti-corrosion layer may be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt% or 4.5wt%, etc. In some examples, the content of graphene and / or its derivatives in the cured anti-corrosion layer may be 0.5wt% to 3.5wt%. In some examples, the content of graphene and / or its derivatives in the cured anti-corrosion layer may be 2wt% to 3.5wt%. In other examples, the content of graphene and / or its derivatives in the cured anti-corrosion layer may be 2.4wt% to 3wt%.

[0082] In some embodiments of the present invention, the thermal diffusion coefficient of the metal matrix composite material in the vertical direction can be 28 mm 2 / s, 29mm 2 / s, 30mm 2 / s, 31mm 2 / s, 32mm 2 / s、33mm 2 / s, 34mm 2 / s, 35mm 2 / s or higher. In some examples, the thermal diffusivity of the metal matrix composite material in the vertical direction is greater than 29 mm 2 / s. In some examples, the thermal diffusion coefficient of the metal matrix composite material in the vertical direction is greater than 30 mm 2 / s.

[0083] According to an embodiment of the present invention, the number of layers of graphene and / or its derivatives is 1 to 10. In some embodiments of the present invention, the number of layers of graphene and / or its derivatives is 1 to 3, or 3 to 10.

[0084] In some specific embodiments of the present invention, the number of layers of graphene and / or its derivatives is 3 to 10 layers. Graphene and / or its derivatives with such a number of layers are easier to disperse and convenient to process, so that the prepared metal-based composite material can take into account corrosion resistance, weather resistance and thermal conductivity. In some examples, the number of layers of graphene and / or its derivatives is selected from 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, 8 layers, 9 layers or 10 layers. In some examples, graphene and / or its derivatives can be a mixture of graphene and / or its derivatives with different numbers of layers, and the number of layers of graphene and / or its derivatives can be a range.

[0085] In some embodiments of the present invention, the aspect ratio of graphene and / or its derivatives is 0.1-1.

[0086] According to an embodiment of the present invention, the maximum sheet diameter of graphene and / or its derivatives is ≤ 5 times the thickness of the anti-corrosion layer. In some embodiments of the present invention, the maximum sheet diameter of graphene and / or its derivatives is ≤ 3 times the thickness of the anti-corrosion layer.

[0087] In some specific embodiments of the present invention, the sheet diameter of graphene and / or its derivatives is 1 micron to 3 microns. The selection of graphene and / or its derivatives in such a sheet diameter range can better match the thickness of the anti-corrosion layer and the content of graphene and / or its derivatives in the anti-corrosion layer, so that the prepared metal-based composite material has high corrosion resistance and high weather resistance in addition to high thermal conductivity.

[0088] In some specific embodiments of the present invention, the thermal diffusion coefficient of the metal matrix composite material in the vertical direction is 28 mm 2 / s~40mm 2 / s. The metal matrix composite material has such a range of thermal diffusion coefficients, reflecting high thermal conductivity. In some examples of the present invention, the thermal diffusion coefficient of the metal matrix composite material in the vertical direction is 30 mm 2 / s~35mm 2 / s.

[0089] In some embodiments of the present invention, the thermal diffusivity is measured at a temperature of 50° C., that is, the thermal diffusivity of the metal matrix composite material in the vertical (thickness) direction is measured at 50° C. The test method for the thermal diffusivity can refer to ASTM E1461-13 "Standard Test Method for Thermal Diffusivity by the Flash Method Test".

[0090] According to an embodiment of the present invention, in the organic coating forming the anti-corrosion layer, the mass percentage of graphene and / or its derivatives is 0.5% to 2%. By adding such a range of graphene and / or its derivatives to the organic coating forming the anti-corrosion layer, the content of graphene and / or its derivatives in the finally formed solidified anti-corrosion layer can be 0.5wt% to 4.5wt%.

[0091] According to an embodiment of the present invention, the anti-corrosion layer is an amide-modified acrylic resin coating or an epoxy-modified acrylic resin coating, and the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating contains graphene and / or its derivatives. By using the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating containing graphene and / or its derivatives as the anti-corrosion layer, the metal-based composite material can have good anti-corrosion performance.

[0092] According to an embodiment of the present invention, an amide-modified acrylic resin coating can be made of organic coatings such as amide-modified acrylic resin coatings, and an epoxy-modified acrylic resin coating can be made of organic coatings such as epoxy-modified acrylic resin coatings, and its proportion composition and preparation method belong to the common technical scheme in this field. For example, the raw materials for preparing the amide-modified acrylic resin coating may include acrylic monomers, amide monomers, initiators, and optional solvents and auxiliary agents, and the selected auxiliary agents are such as coupling agents, surfactants or cross-linking agents. The raw materials for preparing the epoxy-modified acrylic resin coating may include acrylic monomers, epoxy-containing alkenyl monomers, initiators, and optional solvents and auxiliary agents. Among them, the optional acrylic monomers include one or more of acrylic acid, methacrylic acid, methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, propyl methacrylate, butyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, hydroxyhexyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate. Optional amide monomers include one or more of acrylamide, methacrylamide, N,N-dimethylacrylamide, N-hydroxyethylacrylamide, N-vinylformamide, and N-vinylacetamide. Optional epoxy monomers containing alkenyl groups include one or more of glycidyl acrylate, glycidyl methacrylate, and allyl alcohol glycidyl ether. Optional initiators include one or a combination of persulfate and azo compounds. In some examples, the amount of amide monomers or epoxy monomers containing alkenyl groups can be 1% to 30% of the mass of acrylic monomers, the amount of initiator can be 0.5% to 5% of the sum of the mass of acrylic monomers and amide monomers (or acrylic monomers and epoxy monomers containing alkenyl groups), the amount of solvent can be selected and added according to actual conditions, and the amount of other additives can be 0.1% to 5% of the sum of the mass of acrylic monomers and amide monomers (or acrylic monomers and epoxy monomers containing alkenyl groups). Amide-modified acrylic resin or epoxy-modified acrylic resin can increase the cross-linking degree and density of the anti-corrosion layer, thereby improving the corrosion resistance of the coating.

[0093] According to an embodiment of the present invention, the derivative of graphene includes graphene oxide, reduced graphene oxide or grafted modified graphene. That is, graphene and / or its derivatives include one or more of graphene, graphene oxide, reduced graphene oxide and grafted modified graphene. In some embodiments of the present invention, graphene is used to prepare metal-based composite materials.

[0094] In some embodiments of the present invention, the overall weight loss rate of the metal-based composite material in the alkali resistance test is less than 6%. In this way, the metal-based composite material has good alkali resistance and high corrosion resistance. The alkali resistance test refers to testing the metal-based composite material in a 100g / L sodium hydroxide solution, a test temperature of 20°C±2°C, and a test time of 1 hour. The overall weight loss rate refers to the weight loss rate of the metal-based composite material including the metal substrate and the anti-corrosion layer as a whole in the alkali resistance test. In some examples, the alkali resistance test is tested with reference to T / CAS 734-2023 "Technical Specifications for Long-term Weathering and Anti-corrosion Coated Aluminum Foil for Air Conditioner Heat Sinks".

[0095] In some embodiments of the present invention, the metal-based composite material has a corrosion area of ​​≤0.02% after 1500 hours of neutral salt spray test. In this way, the metal-based composite material has good resistance to neutral salt spray and high corrosion resistance. In some examples, the neutral salt spray test is tested with reference to GB / T 10125-2021 "Artificial Atmosphere Corrosion Test Salt Spray Test". In some specific embodiments of the present invention, the metal-based composite material has a corrosion area of ​​less than 0.02% after 1500 hours of neutral salt spray test.

[0096] In some embodiments of the present invention, the corrosion area grade of the weather resistance test of the metal-based composite material is ≥ grade 8. In this way, the metal-based composite material has high weather resistance and excellent aging resistance. The weather resistance test refers to subjecting the metal-based composite material to 120 hours of ultraviolet light and 72 hours of neutral salt spray test in sequence. In some examples, the weather resistance test is carried out with reference to T / CAS 734-2023 "Technical Specifications for Long-term Weathering and Anti-corrosion Coated Aluminum Foil for Air Conditioner Heat Sinks". In some specific examples of the present invention, the corrosion area grade of the weather resistance test of the metal-based composite material is greater than grade 8.

[0097] In some specific embodiments of the present invention, the corrosion area grades of the weather resistance test of the metal matrix composite material are 8 and 9. According to some examples, in the weather resistance test of the metal matrix composite material, the proportion of corrosion ratings of 8 or above is ≥85%. According to some specific examples, in the weather resistance test of the metal matrix composite material, the proportion of corrosion ratings of 8 or above is ≥90%. In some examples, in the weather resistance test of the metal matrix composite material, the proportion of corrosion ratings of 9 is ≥60%. In some examples, in the weather resistance test of the metal matrix composite material, the proportion of corrosion ratings of 9 is ≥65%. In some examples, in the weather resistance test of the metal matrix composite material, the proportion of corrosion ratings of 9 is ≥70%.

[0098] According to an embodiment of the present invention, the metal substrate is provided with functional coatings on two opposite surfaces in the thickness direction, and the functional coatings include an anti-corrosion layer. In some embodiments of the present invention, the functional coatings are provided on the upper surface and the lower surface in the thickness direction of the metal substrate, respectively. In some examples, the metal substrate is in the form of a sheet, and its thickness is less than its length and less than its width.

[0099] In some embodiments of the present invention, the functional coating is an anti-corrosion layer. In some examples, the anti-corrosion layer is an organic coating containing graphene and / or its derivatives.

[0100] According to an embodiment of the present invention, the functional coating further comprises a hydrophilic layer, which is arranged on the surface of the anti-corrosion layer away from the metal substrate. The hydrophilic layer can enhance the hydrophilic effect of the metal matrix composite material and improve the decontamination ability.

[0101] In some embodiments of the present invention, reference Figure 2 The functional coating of the metal-based composite material includes an anti-corrosion layer 210 and a hydrophilic layer 220 ; wherein the anti-corrosion layer 210 is disposed on one surface of the metal substrate 100 , and the hydrophilic layer 220 is disposed on the surface of the anti-corrosion layer 210 away from the metal substrate 100 .

[0102] According to an embodiment of the present invention, the functional coating further comprises a hydrophilic layer and a lubricating layer, wherein the hydrophilic layer is arranged on the surface of the anti-corrosion layer away from the metal substrate; the lubricating layer is arranged on the surface of the hydrophilic layer away from the metal substrate. The hydrophilic layer can enhance the hydrophilic effect of the metal matrix composite material and improve the decontamination ability; further arranging the lubricating layer can protect the hydrophilic layer and the anti-corrosion layer and enhance the punching processing performance, so that the functional coating has better anti-corrosion and hydrophilic properties.

[0103] In some embodiments of the present invention, reference Figure 3 The functional coating of the metal-based composite material includes an anti-corrosion layer 210, a hydrophilic layer 220 and a lubricating layer 230; wherein the anti-corrosion layer 210 is arranged on a surface of the metal substrate 100, the hydrophilic layer 220 is arranged on the surface of the anti-corrosion layer 210 away from the metal substrate 100, and the lubricating layer 230 is arranged on the surface of the hydrophilic layer 220 away from the metal substrate 100.

[0104] In some embodiments of the present invention, reference Figure 4 The functional coating of the metal-based composite material includes a first anti-corrosion layer 211, a second anti-corrosion layer 212, a first hydrophilic layer 221 and a second hydrophilic layer 222; wherein the first anti-corrosion layer 211 and the second anti-corrosion layer 212 are respectively arranged on two surfaces of the metal substrate 100; the first hydrophilic layer 221 is arranged on the surface of the first anti-corrosion layer 211 away from the metal substrate 100, and the second hydrophilic layer 222 is arranged on the surface of the second anti-corrosion layer 212 away from the metal substrate 100.

[0105] In some embodiments of the present invention, reference Figure 5 The functional coating of the metal-based composite material includes a first anti-corrosion layer 211, a second anti-corrosion layer 212, a first hydrophilic layer 221, a second hydrophilic layer 222, a first lubricating layer 231 and a second lubricating layer 232; wherein the first anti-corrosion layer 211 and the second anti-corrosion layer 212 are respectively arranged on two surfaces of the metal substrate 100; the first hydrophilic layer 221 is arranged on the surface of the first anti-corrosion layer 211 away from the metal substrate 100, and the second hydrophilic layer 222 is arranged on the surface of the second anti-corrosion layer 212 away from the metal substrate 100; the first lubricating layer 231 is arranged on the surface of the first hydrophilic layer 221 away from the metal substrate 100, and the second lubricating layer 232 is arranged on the surface of the second hydrophilic layer 222 away from the metal substrate 100.

[0106] In some embodiments of the present invention, when the functional coating further comprises a hydrophilic layer, the single-sided coating thickness of the hydrophilic layer is 0.2 micrometers to 0.5 micrometers. In some specific embodiments of the present invention, the single-sided coating thickness of the hydrophilic layer is 0.2 micrometers to 0.4 micrometers.

[0107] In some embodiments of the present invention, when the functional coating further includes a lubricating layer, the single-sided coating thickness of the lubricating layer is 0.1 micrometer to 0.5 micrometer. In some specific embodiments of the present invention, the single-sided coating thickness of the lubricating layer is 0.2 micrometer to 0.4 micrometer.

[0108] The method of forming a hydrophilic layer or a lubricating layer on a metal-based composite material belongs to a conventional method in the art. For example, a coating with a hydrophilic effect (such as an acrylic resin coating) can be selected and coated, and then cured to form a hydrophilic layer; a material with a lubricating effect (such as a material containing a lubricant) can be selected and coated, and then cured to form a lubricating layer.

[0109] According to an embodiment of the present invention, the metal substrate comprises aluminum, copper, iron or their respective alloys. The substrates of these components all have good thermal conductivity. In some embodiments of the present invention, the metal substrate is selected from aluminum alloy, copper alloy or iron alloy, and the optional iron alloy is such as stainless steel. In some specific embodiments of the present invention, the metal substrate is an aluminum alloy. In some examples of the present invention, when the metal substrate is an aluminum alloy, the obtained metal matrix composite material is a coated aluminum foil.

[0110] In some embodiments of the present invention, the thickness of the metal substrate is 0.02 mm to 0.2 mm. In some specific embodiments of the present invention, the thickness of the metal substrate is 0.05 mm to 0.12 mm.

[0111] Another aspect of the present invention provides a method for preparing an embodiment of a metal-based composite material. According to an embodiment of the present invention, the preparation method comprises the following steps: coating a coating on at least one surface of a metal substrate to form a functional coating to obtain a metal-based composite material. According to an embodiment of the present invention, the preparation method of the metal-based composite material is simple to operate, easy to control, can be processed and prepared under the process conditions of existing production equipment, and is suitable for large-scale industrial production applications.

[0112] In some embodiments of the present invention, a coating material capable of forming a functional coating is applied on at least one surface of a metal substrate to form a functional coating. In some examples, a coating material capable of forming a functional coating is applied on two surfaces opposite to each other in a thickness direction of the metal substrate to form a functional coating.

[0113] In some embodiments of the present invention, an organic coating containing graphene and / or its derivatives is coated on at least one surface of a metal substrate and cured to form an anti-corrosion layer. In some specific embodiments of the present invention, the organic coating containing graphene and / or its derivatives is an amide-modified acrylic resin coating or an epoxy-modified acrylic resin coating, and the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating contains graphene and / or its derivatives.

[0114] In some embodiments of the present invention, a hydrophilic coating is coated on the surface of the anti-corrosion layer and cured to form a hydrophilic layer. In some specific embodiments of the present invention, the hydrophilic coating is an acrylic resin coating.

[0115] In some embodiments of the present invention, a material containing a lubricant is coated on the surface of the hydrophilic layer and cured to form a lubricating layer.

[0116] In some embodiments of the present invention, the coating method includes roller coating, spray coating or dip coating.

[0117] In some embodiments of the present invention, the method of curing to form the functional coating includes thermal curing or photocuring. In other embodiments of the present invention, the organic coating forming the anti-corrosion layer may contain a resin and a solvent in addition to graphene and / or its derivatives, and the solvent may be water, for example. The method of curing to form the functional coating includes removing the solvent in the coating layer to form a resin film.

[0118] Another aspect of the present invention provides a fin embodiment, such as Figure 6As shown, the fin 300 includes the metal-based composite material of the aforementioned embodiment of the present invention, or the metal-based composite material obtained by the method for preparing the metal-based composite material of the aforementioned embodiment. The thickness of the fin 300 can be 0.05 mm to 0.12 mm. The fin 300 can be provided with through holes and cutouts that penetrate the fin in the thickness direction of the fin. The through holes are used for the heat exchange tubes of the heat exchanger to pass through, and the cutouts such as bridges or shutters can be used to improve the heat dissipation effect of the fin. The metal substrate 100 in the metal-based composite material constituting the fin 300 can be an aluminum foil, and the functional coating 200 can be provided on two opposite surfaces of the metal substrate 100 in the thickness direction. According to an embodiment of the present invention, the fin can take into account corrosion resistance, weather resistance and thermal conductivity, has a good heat dissipation effect, and has a long service life.

[0119] Another aspect of the present invention provides a heat exchanger embodiment, including the fin of the above embodiment of the present invention. According to the embodiment of the present invention, the heat exchanger can take into account corrosion resistance, weather resistance and thermal conductivity, is easy to manufacture, and can greatly improve the reliability, service life and energy saving of the heat exchanger.

[0120] In some embodiments of the present invention, the heat exchanger further comprises a heat exchange tube for passing the refrigerant, wherein the heat exchange tube passes through the fin of the aforementioned embodiment or the metal matrix composite material of the aforementioned embodiment. In some examples, the heat exchanger is a tube-fin structure.

[0121] Another aspect of the present invention provides an embodiment of an air treatment device, comprising the metal-based composite material of the aforementioned embodiment of the present invention, or the metal-based composite material obtained by the method for preparing the metal-based composite material of the aforementioned embodiment, or the fin of the aforementioned embodiment, or the heat exchanger of the aforementioned embodiment. According to the embodiment of the present invention, the air treatment device can achieve a significant improvement in reliability, service life, and energy saving and long-term effectiveness.

[0122] According to an embodiment of the present invention, the air processing device is an air conditioner or a dehumidifier.

[0123] According to the embodiment of the present invention, the type of the air conditioner is not particularly limited, and can be a wall-mounted air conditioner, a cabinet air conditioner, a window air conditioner or a ceiling air conditioner. In addition to the aforementioned heat exchanger, the structure of the air conditioner also includes conventional structures of the air conditioner, such as a compressor, a fan, etc.

[0124] The present invention is further described in detail below by means of specific examples. Unless otherwise specified, the raw materials, reagents or devices used below can be obtained from conventional commercial sources. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0125] Unless otherwise specified, the raw materials used in the following examples / comparative examples are commercially available products and are used directly without further treatment.

[0126] The aluminum foil substrate in Examples 1 to 9 and Comparative Examples 1 to 2 is made of aluminum alloy with a grade of 3102 (according to GB / T3190-2020) and a thickness of 0.095 mm. The amide-modified acrylic resin coatings used in Examples 1 to 9 are all the same.

[0127] Example 1

[0128] 0.8 wt% of graphene was added to an amide-modified acrylic resin coating, and the mixture was mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter was 1-3 μm, and the number of layers was 3-10. The acrylic resin coating containing graphene was coated on the upper and lower surfaces of an aluminum foil substrate, and cured to form an anti-corrosion layer with a single-sided coating thickness of 1.08 μm, thereby obtaining an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer was 2.4 wt%.

[0129] Acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-side coating thickness of about 0.25 μm, thereby obtaining the coated aluminum foil of this embodiment.

[0130] Example 2

[0131] 1 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 3 to 6 μm, and the number of layers is 1 to 3. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 1.20 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 3 wt%.

[0132] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0133] Example 3

[0134] 1 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 1-3 μm, and the number of layers is 1-3. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 0.80 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 3 wt%.

[0135] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0136] Example 4

[0137] 1 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 3 to 6 μm, and the number of layers is 3 to 10. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 1.46 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 3 wt%.

[0138] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0139] Example 5

[0140] 1 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 1 to 3 μm, and the number of layers is 3 to 10. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 1.70 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 3 wt%.

[0141] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0142] Example 6

[0143] 3 wt% of graphene was added to an amide-modified acrylic resin coating, and the mixture was mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter was 1-3 μm, and the number of layers was 1-3. The acrylic resin coating containing graphene was coated on the upper and lower surfaces of an aluminum foil substrate, and cured to form an anti-corrosion layer with a single-sided coating thickness of 1.41 μm, thereby obtaining an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer was 9 wt%.

[0144] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0145] Example 7

[0146] 4 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 1 to 3 μm, and the number of layers is 3 to 10. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 1.37 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 12 wt%.

[0147] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0148] Example 8

[0149] 3 wt% of graphene was added to an amide-modified acrylic resin coating, and the mixture was mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter was 3-8 μm, and the number of layers was 1-3. The acrylic resin coating containing graphene was coated on the upper and lower surfaces of an aluminum foil substrate, and cured to form an anti-corrosion layer with a single-sided coating thickness of 1.43 μm, thereby obtaining an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer was 9 wt%.

[0150] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0151] Example 9

[0152] 1 wt% of graphene is added to an amide-modified acrylic resin coating, and the mixture is mixed to obtain an acrylic resin coating containing graphene. The graphene sheet diameter is 9-12 μm, and the number of layers is 3-10. The acrylic resin coating containing graphene is coated on the upper and lower surfaces of an aluminum foil substrate, cured, and an anti-corrosion layer with a single-sided coating thickness of 1.48 μm is formed to obtain an aluminum foil sample with an anti-corrosion layer coated on the upper and lower surfaces. The content of graphene in the cured anti-corrosion layer is 3 wt%.

[0153] Referring to Example 1, acrylic resin coating was coated on the surfaces of the upper and lower anti-corrosion layers of the aluminum foil sample respectively, and cured to form a hydrophilic layer with a single-sided coating thickness of about 0.25 μm to obtain the coated aluminum foil of this example.

[0154] Comparative Example 1

[0155] This comparative example is an aluminum foil sample with a basecoat and a common coating. The common coating is a water-based acrylic system coating according to Model P11 in YS / T 95.2-2016 "Aluminum Foil for Air Conditioner Heat Sink Part 2: Coated Aluminum Foil". In the coated aluminum foil of this example, the basecoat (common coating) has a single-sided coating thickness of 1.35 μm, and the topcoat hydrophilic layer is the same as that in Example 1. Among them, the anti-corrosion layer of the basecoat is mainly formed by coating and curing a thermosetting acrylic emulsion.

[0156] Comparative Example 2

[0157] This comparative example is an aluminum foil sample with a high anti-corrosion coating as the base coat. The high anti-corrosion coating is an epoxy system coating according to Model P31 in YS / T 95.2-2016 "Aluminum Foil for Air Conditioner Heat Sink Part 2: Coated Aluminum Foil". In the coated aluminum foil of this example, the single-side coating thickness of the base coat anti-corrosion layer (high anti-corrosion coating) is 1.89 μm, and the top coat hydrophilic layer is the same as that in Example 1. Among them, the base coat anti-corrosion layer is mainly formed by coating and curing the epoxy resin coating.

[0158] The comparison of the coated aluminum foil solutions of Examples 1 to 9 and Comparative Examples 1 to 2 is shown in Table 1.

[0159] Table 1 Comparison of coated aluminum foil solutions of Examples 1 to 9 and Comparative Examples 1 to 2

[0160]

[0161] The structures of the coated aluminum foil samples prepared in Examples 1 to 9 and Comparative Examples 1 to 2 are shown in Figure 4 In both methods, an anti-corrosion layer is applied as a primer and a hydrophilic layer is applied as a top coat on the upper and lower surfaces of the aluminum foil substrate in the thickness direction, thereby forming a double-layer coating structure.

[0162] The coated aluminum foil samples prepared in the embodiments and comparative examples are subjected to thermal conductivity test, alkali resistance test, salt spray test, weather resistance test and long-term operation test respectively.

[0163] 1. Thermal conductivity test

[0164] According to ASTM E1461-13 "Standard Test Method for Thermal Diffusivity by the Flash Method Test", the thermal conductivity of the coated aluminum foil was tested.

[0165] The thermal diffusion coefficients of the coated aluminum foils of Examples 1 to 9 and Comparative Examples 1 to 2 in the vertical (thickness) direction at 50° C. are shown in Table 2.

[0166] Table 2 Thermal diffusion coefficient of coated aluminum foil in vertical direction

[0167]

[0168] Attached Figure 7 It is a thermal diffusion coefficient diagram of the coated aluminum foil sample in the vertical direction at 50°C, wherein the ordinary aluminum foil is the comparative example 1 sample, the high corrosion resistance aluminum foil is the comparative example 2 sample, and the graphene aluminum foil is the embodiment 1 sample. The longitudinal thermal diffusion coefficient is the thermal diffusion coefficient in the vertical direction.

[0169] Combining Table 2 and Figure 7 It can be seen that the graphene aluminum foils of Examples 1 to 9 have improved thermal conductivity compared to the ordinary aluminum foil and high anti-corrosion aluminum foil of the comparative example, and thus are beneficial to improving the overall performance of the heat exchanger or air conditioner. Among them, Examples 1 to 4 have more obvious improvements in thermal conductivity, and can better improve the heat exchange effect of the heat exchanger or air conditioner; Example 5 with a relatively large thickness of the solidified anti-corrosion layer, Examples 6 to 8 with a high content of graphene in the solidified anti-corrosion layer, and Example 9 with a larger graphene sheet diameter do not improve the thermal conductivity as well as Examples 1 to 4.

[0170] 2. Alkali resistance test

[0171] According to Section 5.2.3 of T / CAS 734-2023 "Technical Specifications for Long-lasting Weather-Resistant and Anti-corrosion Coated Aluminum Foil for Air Conditioner Heat Sinks", the coated aluminum foil samples were tested for alkaline resistance in 100g / L NaOH solution, with the test temperature at 20℃±2℃ and the test time for 1 hour.

[0172] Attached Figure 8 This is the overall weight loss percentage of the coated aluminum foil sample in the alkali resistance test. Figure 8 It can be seen that in the alkali resistance test of the common coating in comparative example 1, 32.00% of the coatings had a weight loss rate of >10%, 52.00% of the coatings had a weight loss rate of 6% to 10%, and 16.00% of the coatings had a weight loss rate of <6%. The overall weight loss rate of the graphene coating in the alkali resistance test of Example 1 <6% accounted for 100.00%, which was comparable to the alkali resistance test result of the high corrosion resistance coating in comparative example 2, and the alkali corrosion resistance was significantly better than that of the common coating samples.

[0173] 3. Salt spray test

[0174] According to Section 5.2.2 and Section 5.2.3 of GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", the coated aluminum foil was tested by neutral salt spray test and acetic acid salt spray test respectively.

[0175] The coated aluminum foils of Examples 1-9 and Comparative Examples 1-2 were subjected to acetic acid salt spray tests for 24 h, 72 h, and 96 h, respectively. The corrosion rating results of the acetic acid salt spray tests are shown in Table 3.

[0176] Table 3 Corrosion rating of coating samples after acetic acid salt spray test at different times

[0177]

[0178] Attached Fig. 9 This is the corrosion rating diagram of the coated aluminum foil sample after the acetic acid salt spray test at different times. Fig. 9 The corrosion ratings of the common coating sample of comparative example 1, the high corrosion protection coating sample of comparative example 2, and the graphene coating sample of embodiment 1 after 24h, 72h, and 96h acetic acid salt spray test are shown. Among them, the corrosion ratings of the common coating sample after 24h, 72h, and 96h acetic acid salt spray test are 9.8, 9, and 8 respectively; the corrosion ratings of the high corrosion protection coating sample after 24h, 72h, and 96h acetic acid salt spray test are 9.8, 9.8, and 9 respectively; the corrosion ratings of the graphene coating sample after 24h, 72h, and 96h acetic acid salt spray test are 9.8, 9.8, and 9 respectively.

[0179] The coated aluminum foils of Examples 1-9 and Comparative Examples 1-2 were subjected to a 1500 h neutral salt spray test, and the corrosion ratings of the samples are shown in Table 4.

[0180] Table 4 Corrosion rating of coating after neutral salt spray test

[0181]

[0182] Combined with Table 3-4 and Fig. 9 The test results show that the acid salt spray and neutral salt spray resistance of the graphene coating samples of Examples 1 to 5 are comparable to those of the high anti-corrosion coating samples, and are significantly better than those of the ordinary coating samples of the same thickness. However, the corrosion ratings of the acetic acid salt spray test and neutral salt spray performance of Examples 6 to 8 with higher graphene content in the solidified anti-corrosion layer and Example 9 with a larger graphene sheet diameter are not significantly improved compared with the ordinary coating sample of Comparative Example 1.

[0183] 4. Weather resistance test

[0184] The weather resistance test refers to Section 5.3 of the standard T / CAS 734-2023 "Technical Specifications for Long-term Weathering and Anti-corrosion Coated Aluminum Foil for Air Conditioner Heat Sinks". The neutral salt spray test is carried out after aging under the conditions of 120h UVB (ultraviolet light) + 72h NSS (neutral salt spray).

[0185] The coated aluminum foils of Examples 1-9 and Comparative Examples 1-2 were subjected to weather resistance tests, and the test results are shown in Table 5. Table 5 shows the proportions of the coated aluminum foils in different corrosion ratings.

[0186] Table 5 Weathering test results of coated aluminum foil samples

[0187]

[0188] Attached Fig.10 It is a weather resistance test rating chart of coated aluminum foil samples. Fig.10 The corrosion rating ratios of the ordinary coated aluminum foil sample of comparative example 1, the high anti-corrosion coated aluminum foil sample of comparative example 2, and the graphene coated aluminum foil sample of embodiment 1 are shown. Fig.10 It can be seen that after aging and the salt spray test, 62.00% of the ordinary coated aluminum foil in Comparative Example 1 was rated as level 6, 38.00% was rated as level 7, and there was no level 8 and 9; 78.00% of the high-corrosion protection coated aluminum foil in Comparative Example 2 was rated as level 6, 22.00% was rated as level 7, and there was no level 8 and 9; 4.00% of the graphene coated aluminum foil in Example 1 was rated as level 7, 20.00% was rated as level 8, 76.00% was rated as level 9, and there was no level 6.

[0189] Combination Fig.10 As shown in Table 5, the results of the salt spray test after aging show that the graphene-coated aluminum foil samples of Examples 1 to 5 have higher ratings and better corrosion resistance than the ordinary aluminum foil and high-corrosion-resistant aluminum foil of the comparative example, showing good weather resistance. However, the weathering corrosion ratings of Examples 6 to 8 with higher graphene content in the solidified anti-corrosion layer and Example 9 with a larger graphene sheet diameter are not significantly improved compared with the ordinary coated aluminum foil samples.

[0190] 5. Long-term operation test

[0191] The coated aluminum foils of Examples 1-9 and Comparative Examples 1-2 were used as fins to make outdoor heat exchangers, which were then made into air conditioner prototypes. They were operated in Hainan for a long time to compare power consumption and cooling effects.

[0192] The long-term test method is described as follows: The environmental adaptability test field of the air conditioner is located in Lingao County, Hainan Province. Lingao County is located at 19°34′~20°02′ north latitude and 109°03′~109°53′ east longitude. Lingao County has a tropical monsoon climate, with high temperatures and heavy rains, sufficient sunshine, an average altitude of 306 meters, an average air pressure of 1011.3hPa, an average annual temperature of 23 to 24°C, an average temperature of 16.9°C in January, and an average temperature of 28.3°C in July. The average relative humidity is 87%, the average annual rainy days are 135.9 days, the rainfall is 1417.8 mm, and the annual total radiation is 5001MJ / m 2, the annual total sunshine hours are 2175h, the annual total precipitation is 1417.8mm, and the sea salt particles (gauze method) are 0.107mg / 100cm 2 ·d. The tropical marine climate environment adaptability test site for refrigeration products in Lingao County, Hainan Province (Lingao Test Station) is about 100 meters away from the sea. In accordance with Q / CVC 0035-2020 "General Test Methods for Engineering Sites", the indoor unit of the air-conditioning unit is installed in the room, and the outdoor unit faces the ocean. The air-conditioning unit is turned on and operated in cooling mode, and the same operating mode is operated for 8 hours a day (9:00~17:00). The power of the whole unit, the temperature and humidity of the outlet and return air, and the temperature and humidity of the room are recorded in real time, and a set of data is recorded every 1 minute.

[0193] The long-term performance test results of the heat exchanger prototypes of Examples 1 to 9 and Comparative Examples 1 to 2 are shown in Table 6. Table 6 shows the energy consumption comparison results of different heat exchanger prototypes.

[0194] Table 6 Long-term performance test results of heat exchanger prototypes of Examples 1 to 9 and Comparative Examples 1 to 2

[0195]

[0196] Attached Fig.11 This is a performance comparison chart of two types of heat exchanger prototypes 9 months after the air conditioner was installed. Fig.11 The energy consumption per unit temperature difference of the graphene-coated heat exchanger prototype and the ordinary-coated heat exchanger prototype is shown. Compared with the prototype of the ordinary-coated heat exchanger of Comparative Example 1, the energy consumption per unit temperature difference of the prototype of the graphene-coated heat exchanger of Example 1 is reduced by about 37.8%.

[0197] From Table 6 and Fig.11 It can be seen that the unit temperature difference energy consumption of the prototypes of the graphene-coated heat exchangers of Examples 1 to 4 of the present invention is relatively lower, and the corrosion resistance is improved during long-term operation, so the air conditioner performance decays more slowly, and finally achieves the effect of long-term energy saving. The unit temperature difference energy consumption of the prototypes prepared in other Examples 5 to 9 is relatively large, and there is no significant improvement over the prototypes of the comparative examples, and it cannot effectively save energy.

[0198] In summary, the metal-based composite material embodiment of the present invention uses a coating containing graphene and / or its derivatives as an anti-corrosion layer, which can reduce the impact on thermal conductivity while meeting the long-term anti-corrosion requirements, and has good aging resistance, and can be processed and prepared under the process conditions of existing production equipment. Specifically, in the metal-based composite material embodiment of the present invention, the sheet diameter of graphene and / or its derivatives is 1 micron to 8 microns, and the content of graphene and / or its derivatives in the solidified anti-corrosion layer is 0.5wt% to 4.5wt%, which can have high thermal conductivity, corrosion resistance and high weather resistance at such a thin anti-corrosion coating thickness of 0.8 to 1.5 microns. However, in the embodiment where the thickness of the anti-corrosion coating, or the sheet diameter of graphene and / or its derivatives, or the content of graphene and / or its derivatives in the solidified anti-corrosion layer exceeds the above range, the thermal conductivity is poor, and the corrosion resistance and high weather resistance are not significantly improved or even deteriorated relative to the comparative example using ordinary primer. It can be seen that graphene and / or its derivatives use specific sheet diameters and contents, and are combined with the specific thickness of the anti-corrosion layer to work synergistically to achieve the best effect, so that the fins and heat exchangers made of metal-based composite materials have the advantages of high weather resistance, high thermal conductivity and corrosion resistance. Their application in air treatment devices such as air conditioners and dehumidifiers can greatly improve the reliability, service life and long-term energy saving of these air treatment devices, thereby improving the overall performance of these air treatment devices.

[0199] In the description of this specification, the description with reference to the terms "some embodiments", "some specific embodiments", "some examples" or "some specific examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0200] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. A metal matrix composite material, characterized in that: It comprises a metal substrate and a functional coating; the functional coating is arranged on at least one surface of the metal substrate; Wherein, the functional coating at least includes an anti-corrosion layer; The anti-corrosion layer includes an organic coating containing graphene and / or its derivatives; The thickness of the cured anti-corrosion layer is 0.8 microns to 1.5 microns; The sheet diameter of the graphene and / or its derivatives is 1 micron to 8 microns; The content of the graphene and / or its derivatives in the cured anti-corrosion layer is 0.5wt% to 4.5wt%; The thermal diffusion coefficient of the metal matrix composite material in the vertical direction is ≥28 mm 2 / s; The anti-corrosion layer is an amide-modified acrylic resin coating or an epoxy-modified acrylic resin coating, and the amide-modified acrylic resin coating or the epoxy-modified acrylic resin coating contains graphene and / or its derivatives.

2. The metal matrix composite material according to claim 1, characterized in that: The number of layers of the graphene and / or its derivatives is 1 to 10.

3. The metal matrix composite material according to claim 1, characterized in that: The maximum sheet diameter of the graphene and / or its derivatives is ≤ 5 times the thickness of the anti-corrosion layer.

4. The metal matrix composite material according to claim 1 or 3, characterized in that: The sheet diameter of the graphene and / or its derivatives is 1 micron to 3 microns.

5. The metal matrix composite material according to claim 1, characterized in that: The thermal diffusion coefficient of the metal matrix composite material in the vertical direction is 28 mm 2 / s~40mm 2 / s.

6. The metal matrix composite material according to claim 1 or 5, characterized in that: The thermal diffusion coefficient was measured at 50°C.

7. The metal matrix composite material according to claim 1, characterized in that: In the organic coating forming the anti-corrosion layer, the mass percentage of the graphene and / or its derivatives is 0.5% to 2%.

8. The metal matrix composite material according to claim 1, characterized in that: The overall weight loss rate of the metal-based composite material in the alkali resistance test is less than 6%; the alkali resistance test refers to testing the metal-based composite material in a 100g / L sodium hydroxide solution, a test temperature of 20°C±2°C, and a test time of 1 hour.

9. The metal matrix composite material according to claim 1, characterized in that: After 1500 hours of neutral salt spray test, the corrosion area of ​​the metal matrix composite material is ≤0.02%.

10. The metal matrix composite material according to claim 1, characterized in that: The corrosion area grade of the weather resistance test of the metal-based composite material is ≥ grade 8; the weather resistance test refers to subjecting the metal-based composite material to a 120-hour ultraviolet light test and a 72-hour neutral salt spray test in sequence.

11. The metal matrix composite material according to claim 1, characterized in that: The two surfaces of the metal substrate opposite to each other in the thickness direction are both provided with functional coatings, and the functional coatings include an anti-corrosion layer.

12. The metal matrix composite material according to claim 1 or 11, characterized in that: The functional coating further comprises a hydrophilic layer, and the hydrophilic layer is arranged on the surface of the anti-corrosion layer away from the metal substrate.

13. The metal matrix composite material according to claim 1 or 11, characterized in that: The functional coating also includes: A hydrophilic layer, the hydrophilic layer being disposed on a surface of the anti-corrosion layer away from the metal substrate; A lubricating layer is disposed on a surface of the hydrophilic layer away from the metal substrate.

14. The metal matrix composite material according to claim 1 or 11, characterized in that: The metal substrate includes aluminum, copper, iron or alloys thereof.

15. The method for preparing the metal matrix composite material according to any one of claims 1 to 14, characterized in that: The following steps are involved: A coating is applied on at least one surface of a metal substrate to form a functional coating to obtain the metal-based composite material.

16. A fin, characterized in that The thickness of the fin is 0.05 mm to 0.12 mm; the fin comprises the metal-based composite material according to any one of claims 1 to 14, or the metal-based composite material obtained by the preparation method according to claim 15.

17. A heat exchanger, characterized in that Comprising the fin according to claim 16.

18. An air treatment device, characterized in that It comprises the metal-based composite material according to any one of claims 1 to 14, or the metal-based composite material obtained by the preparation method according to claim 15, or the fin according to claim 16, or the heat exchanger according to claim 17.

19. The air treatment device according to claim 18, characterized in that: The air treatment device is an air conditioner or a dehumidifier.