A multi-sheet cadmium zinc telluride composite substrate, preparation method and application thereof
Through the polishing, cleaning, Ar atomic beam bombardment and bonding of multiple zinc tellurium substrates, the composite substrate is formed, which solves the defect problem caused by the difference in the crystal lattice of zinc tellurium substrate and mercury tellurium tellurium materials and improves the material Uniformity and crystallization quality, and reduce the cost of use, achieving efficient production of infrared detectors.
Patent Information
- Application Number
- CN202410745329.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-06-11
AI Technical Summary
In the prior art, there is a difference in the lattice constant between zinc tellurium substrate and mercury tellurium material, resulting in high defect density of molecular beam epitaxial materials, limiting its application in infrared detectors, and the cost of using alternative substrates is relatively high. high.
Multiple irregular zinc tellurium substrates are used for double-side polishing and cleaning. By bombarding and bonding Ar atomic beams, composite substrates are formed and annealed to improve the uniformity of the material and crystallization quality, while reducing zinc tellurium tellurium Cost of use of substrate.
Improve the uniformity and crystallization quality of molecular beam epitaxial zinc tellurium-based mercury tellurium materials, reduce the cost of zinc tellurium substrates, and realize the transformation from manual to automated production, improve the production capacity and reduce the Process difficulty and cost.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparing mercury cadmium telluride epitaxial materials, and in particular relates to a multi-piece cadmium zinc telluride composite substrate, a preparation method and application thereof. Background Art
[0002] At present, countries around the world are vigorously developing the third-generation infrared focal plane detectors represented by large arrays, very long waves, dual multi-color and even multi-band, and low cost. The third-generation infrared focal plane detectors have put forward higher requirements on the area, performance, reliability and other parameters of HgCdTe materials. CdZnTe substrates can achieve lattice matching with HgCdTe epitaxial materials by controlling the zinc component, and realize quasi-homogeneous epitaxy, thereby improving the performance of HgCdTe epitaxial materials. Therefore, CdZnTe substrates have become the preferred substrate for the preparation of third-generation infrared focal plane detectors such as long-wave and very long-wave, dual multi-color, APD, etc., which have extremely high requirements for HgCdTe epitaxial materials.
[0003] Common methods for epitaxy of HgCdTe materials include liquid phase epitaxy and molecular beam epitaxy. Liquid phase epitaxy usually uses square CdZnTe substrates with fixed and small size. If CdZnTe substrates are used for molecular beam epitaxy, square substrates are generally used, and adhesive wafers and molybdenum trays or graphite trays are generally used; in addition, molecular beam epitaxy will also use alternative substrates such as silicon and gallium arsenide to achieve large size and low cost. However, due to the large lattice constant difference between such alternative substrates and HgCdTe materials, a large lattice mismatch is formed, thereby increasing the defect density of HgCdTe epitaxial materials, which seriously restricts the application of alternative substrates in infrared detectors such as very long wave, dual multicolor, and APD. Summary of the invention
[0004] The purpose of the present invention is to provide a multi-piece cadmium zinc telluride composite substrate, a preparation method and application thereof. The multi-piece cadmium zinc telluride composite substrate in the present invention can improve the uniformity and crystal quality of molecular beam epitaxy cadmium zinc telluride-based mercury cadmium telluride materials, while improving the utilization rate of cadmium zinc telluride materials and reducing the use cost of cadmium zinc telluride substrates.
[0005] The present invention provides a method for preparing a plurality of cadmium zinc telluride composite substrates, comprising the following steps:
[0006] A) double-sided polishing of a plurality of irregular CdZnTe substrate sheets, and then cleaning the double-sided polished CdZnTe substrate sheets and germanium wafers;
[0007] B) Under vacuum conditions, an Ar atomic beam is used to bombard the bonding surfaces of the cleaned CdZnTe substrate and the Ge wafer;
[0008] C) contacting the bombarded germanium wafer with the bonding surfaces of a plurality of cadmium zinc telluride substrate sheets to bond them to obtain a bonded substrate;
[0009] D) annealing the bonded substrates to obtain multiple pieces of CdZnTe composite substrates;
[0010] The annealing temperature is 500-600° C., and the annealing time is 2-3 hours.
[0011] Preferably, among the plurality of irregular CdZnTe substrate sheets, the thickness difference between any two irregular CdZnTe substrate sheets is less than 3 μm.
[0012] Preferably, the cleaning in step A) is specifically:
[0013] The CdZnTe substrate and the Ge wafer were rinsed with acetone and methanol and then dried with nitrogen.
[0014] Preferably, the vacuum degree in step B) is 1×10 -8 Torr or less;
[0015] The radio frequency power of Ar atom bombardment is 80~100W, and the bombardment time is 4~6s.
[0016] Preferably, the bombarded germanium wafer is bonded to a plurality of cadmium zinc telluride substrate sheets using a wafer bonding device, and the minimum distance between any two cadmium zinc telluride substrate sheets is greater than 1 cm.
[0017] Preferably, the bonding pressure is 9-11 MPa; and the bonding time is 50-60 min.
[0018] The present invention provides a plurality of cadmium zinc telluride composite substrates prepared by the preparation method described above.
[0019] The present invention provides the use of multiple pieces of cadmium zinc telluride composite substrates as described in the invention in preparing mercury cadmium telluride materials by epitaxial growth.
[0020] Preferably, the plurality of cadmium zinc telluride composite substrates are polished and cleaned in sequence and then used for epitaxial growth to prepare mercury cadmium telluride materials.
[0021] Preferably, the cleaning includes acetone washing, methanol washing, 0.5% bromine methanol solution corrosion, methanol washing and nitrogen drying in sequence.
[0022] The invention provides a method for preparing a plurality of cadmium zinc telluride composite substrates, comprising the following steps: A) double-sided polishing a plurality of irregular cadmium zinc telluride substrate sheets, and then cleaning the double-sided polished cadmium zinc telluride substrate sheets and germanium wafers; B) bombarding the bonding surfaces of the cleaned cadmium zinc telluride substrate sheets and the germanium wafers with an Ar atomic beam under vacuum conditions; C) contacting the bombarded germanium wafers with the bonding surfaces of the plurality of cadmium zinc telluride substrate sheets, bonding them, and obtaining bonded substrates; D) annealing the bonded substrates to obtain the plurality of cadmium zinc telluride composite substrates; the annealing temperature is 500-600° C., and the annealing time is 2-3 hours. The present invention realizes maximum utilization of the existing CdZnTe single crystal area, improves the utilization rate of CdZnTe materials and reduces the use cost of CdZnTe substrates, and at the same time, the liquid phase epitaxial process can simultaneously epitaxially grow multiple pieces of CdZnTe-based HgCdTe materials; the composite substrate bonded according to the method of the present invention has no temperature unevenness problem in heat transfer, and can improve the uniformity and crystal quality of molecular beam epitaxial CdZnTe-based HgCdTe materials; because the germanium wafer material is used as the base composite substrate, the existing mature wafer silicon process equipment can be used in the later device process, and the preparation of HgCdTe infrared detector chips can be transformed from manual and semi-automatic to automatic, thereby improving the batch production capacity and reducing the process difficulty and cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0024] Figure 1 It is a schematic diagram of the process flow of the method for preparing multiple pieces of cadmium zinc telluride composite substrates in the present invention;
[0025] Figure 2 This is a schematic diagram of the structure of multiple cadmium zinc telluride composite substrates in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing a plurality of cadmium zinc telluride composite substrates, comprising the following steps:
[0027] A) double-sided polishing of a plurality of irregular CdZnTe substrate sheets, and then cleaning the double-sided polished CdZnTe substrate sheets and germanium wafers;
[0028] B) Under vacuum conditions, an Ar atomic beam is used to bombard the bonding surfaces of the cleaned CdZnTe substrate and the Ge wafer;
[0029] C) contacting the bombarded germanium wafer with the bonding surfaces of a plurality of cadmium zinc telluride substrate sheets to bond them to obtain a bonded substrate;
[0030] D) annealing the bonded substrates to obtain multiple pieces of CdZnTe composite substrates;
[0031] The annealing temperature is 500-600° C., and the annealing time is 2-3 hours.
[0032] The process flow for preparing multiple pieces of cadmium zinc telluride composite substrates in the present invention is as follows: Figure 1 As shown, it mainly includes pre-cleaning of substrate and germanium wafer, bombarding the surface to be bonded with argon atoms in a vacuum chamber, wafer bonding and high-temperature annealing.
[0033] The present invention uses a single crystal CdZnTe wafer which is not diced or cut and has an irregular shape. The present invention preferably performs double-sided polishing on the irregular-shaped CdZnTe substrate to obtain a double-sided polished CdZnTe substrate.
[0034] In the present invention, the double-sided polishing is a polishing method well known to those skilled in the art, and the present invention will not be described in detail here.
[0035] Then the germanium wafer and the plurality of double-sided polished cadmium zinc telluride substrate sheets are cleaned to obtain cleaned germanium wafer and the plurality of cleaned cadmium zinc telluride substrate sheets.
[0036] In the present invention, the size of the germanium wafer is preferably 6 inches or 8 inches. Selecting a germanium wafer as a bonding substrate can ensure that the wafer does not fall off, has little deformation, and has a low risk of cracking during high-temperature annealing and subsequent processes.
[0037] In the present invention, among the plurality of CdZnTe substrates, the thickness difference between any two CdZnTe substrates is less than 3 μm.
[0038] In the present invention, the cleaning is preferably: washing with acetone and methanol followed by drying with nitrogen. Preferably, in the present invention, acetone is first used for washing and then methanol is used for washing. The cleaning in the present invention is preferably carried out by conventional methods for washing germanium wafers, which will not be described in detail in the present invention.
[0039] After cleaning, the cleaned CdZnTe substrates and Ge wafers are quickly loaded into the vacuum chamber to reduce the exposure time of the substrate surface to air, reduce surface contamination and thickness after oxidation; the vacuum chamber is evacuated to 1×10 -8 Torr or less, reducing gas adsorption on the substrate surface.
[0040] Then, neutral atoms such as Ar atoms are used to bombard the bonding surfaces of multiple CdZnTe substrates and Ge wafers to remove the surface oxide layer of the bonding surface to form a pure surface. At the same time, the root mean square roughness of the bonding surface after atomic bombardment is ensured to be less than 1nm, the smaller the better, so as to improve the subsequent wafer bonding strength and avoid bonding failure.
[0041] In the present invention, Ar plasma can be generated by electron cyclotron resonance (ECR) method to bombard the bonding surface; the RF power of the bombardment is preferably 80-100 W, more preferably 85-95 W; the bombardment time is preferably 4-6 s, more preferably 5-6 s.
[0042] After obtaining the bombarded CdZnTe substrate sheets and the germanium sheet, multiple CdZnTe substrate sheets are arranged on the surface of the germanium wafer, the bonding surfaces of the two are in contact, and the wafer bonding equipment is loaded to perform bonding to obtain a bonded composite substrate.
[0043] The present invention has no special requirements for the specific arrangement and quantity of the CdZnTe substrate sheets arranged on the surface of the germanium wafer. It is sufficient to utilize the space as much as possible while ensuring that they do not affect each other.
[0044] In the present invention, the bonding temperature is preferably 20-30°C, more preferably 25-30°C; the bonding pressure is preferably 9-11 MPa, more preferably 10-11 MPa; the bonding time is preferably 50-60 min, more preferably 55-60 min.
[0045] In the present invention, in order to avoid mutual influence between multiple CdZnTe substrate sheets during the bonding process, the minimum distance between any two CdZnTe substrate sheets is preferably greater than 1 cm.
[0046] After bonding is completed, in order to improve the bonding strength and avoid debonding in the subsequent high-temperature process, the present invention performs an annealing treatment on the bonded composite substrate.
[0047] In the present invention, the annealing temperature is preferably higher than the treatment temperature in the subsequent process, preferably, it can be 500-600°C, more preferably 520-580°C, most preferably 550-560°C; the annealing time is preferably 2-3 hours.
[0048] The present invention provides a plurality of cadmium zinc telluride composite substrates, which are prepared according to the preparation method described above. The plurality of cadmium zinc telluride composite substrates include a germanium wafer substrate and a plurality of cadmium zinc telluride substrate sheets bonded to the surface of the germanium wafer substrate.
[0049] In the present invention, the CdZnTe substrate sheet is an irregularly shaped single crystal CdZnTe wafer that has not been diced or cut. The present invention does not impose any special restriction on the number of bonded CdZnTe substrate sheets.
[0050] The present invention also provides an application of the above-mentioned multiple pieces of cadmium zinc telluride composite substrate in preparing mercury cadmium telluride material by epitaxial growth.
[0051] In the present invention, the epitaxial growth can be carried out by liquid phase epitaxy or molecular beam epitaxy; the epitaxial growth process can adopt the liquid phase epitaxy or molecular beam epitaxy growth process commonly used by technical personnel in this field, and the subsequent device process can be directly compatible with semiconductor equipment of wafer silicon process, which greatly reduces the difficulty and cost of preparing CdZnTe-based HgCdTe infrared detector chips.
[0052] In the present invention, the epitaxial surface of the CdZnTe substrate of the multiple CdZnTe composite substrates obtained after annealing needs to be polished twice, preferably using SiC polishing materials with a particle size of 0.1 and 0.03 microns for single-sided mechanical chemical polishing, the polishing pressure is 3Kg~4Kg pressure, the polishing disk speed is 9r / min~11 r / min, and the final root mean square roughness of the CdZnTe substrate surface is less than 1nm to ensure the quality of the epitaxial HgCdTe material in the later stage.
[0053] Before the formal epitaxial HgCdTe process, the CdZnTe substrate needs to be pre-cleaned after the secondary polishing, including rinsing with acetone, rinsing with methanol, etching with 0.5% bromine methanol solution for 5s~6s, rinsing with methanol and drying with nitrogen. Then, it is quickly loaded into the epitaxial equipment and vacuum pumping is started to prevent the oxidation time from being too long and reduce the subsequent deoxidation temperature and time.
[0054] The invention provides a method for preparing a plurality of cadmium zinc telluride composite substrates, comprising the following steps: A) double-sided polishing a plurality of irregular cadmium zinc telluride substrate sheets, and then cleaning the double-sided polished cadmium zinc telluride substrate sheets and germanium wafers; B) bombarding the bonding surfaces of the cleaned cadmium zinc telluride substrate sheets and the germanium wafers with an Ar atomic beam under vacuum conditions; C) contacting the bombarded germanium wafers with the bonding surfaces of the plurality of cadmium zinc telluride substrate sheets, bonding them, and obtaining bonded substrates; D) annealing the bonded substrates to obtain the plurality of cadmium zinc telluride composite substrates; the annealing temperature is 500-600° C., and the annealing time is 2-3 hours. The present invention realizes maximum utilization of the existing CdZnTe single crystal area, improves the utilization rate of CdZnTe materials and reduces the use cost of CdZnTe substrates, and at the same time, the liquid phase epitaxial process can simultaneously epitaxially grow multiple pieces of CdZnTe-based HgCdTe materials; the composite substrate bonded according to the method of the present invention has no temperature unevenness problem in heat transfer, and can improve the uniformity and crystal quality of molecular beam epitaxial CdZnTe-based HgCdTe materials; because the germanium wafer material is used as the base composite substrate, the existing mature wafer silicon process equipment can be used in the later device process, and the preparation of HgCdTe infrared detector chips can be transformed from manual and semi-automatic to automatic, thereby improving the batch production capacity and reducing the process difficulty and cost.
[0055] In order to further illustrate the present invention, a multi-piece cadmium zinc telluride composite substrate, a preparation method and an application thereof provided by the present invention are described in detail below in combination with embodiments, but it should not be understood as limiting the protection scope of the present invention.
[0056] Example 1
[0057] Pre-clean the CdZnTe substrate (A side) and the germanium wafer that have been double-sided polished, select a CdZnTe substrate with a thickness difference of less than 3μm, rinse with acetone and methanol, and then blow dry with nitrogen. The germanium wafer can be 6 inches.
[0058] The cleaned substrate material is quickly loaded into the vacuum chamber, and the vacuum chamber is evacuated to 1×10 -8 Torr or less.
[0059] The electron cyclotron resonance plasma (ECR) method was used to bombard the bonding surfaces of the CdZnTe and Ge sheets with Ar atoms at a radio frequency power of 80 W for 6 seconds to remove the surface oxide layer of the bonding surface and form a pure surface. At the same time, the root mean square roughness of the surface after atomic bombardment was ensured to be less than 1 nm.
[0060] The surface treated CdZnTe substrate and germanium wafer are loaded into the wafer bonding equipment. At room temperature, the pressure is 9MPa for 60min to ensure that the CdZnTe substrate and the germanium wafer are firmly bonded. The minimum spacing between the two CdZnTe substrates is controlled to be more than 1cm. The specific arrangement diagram is shown in the figure. Figure 2 shown.
[0061] After the wafer bonding is completed, the composite substrate is subjected to high temperature annealing heat treatment, the annealing temperature is 500°C, and the annealing time is 3 hours.
[0062] The epitaxial surface (B side) of the CdZnTe substrate needs to be polished twice, and the CdZnTe substrate surface of the composite substrate is single-sided polished using SiC polishing materials with a particle size of 0.1 and 0.03 microns for mechanical chemical polishing. The polishing pressure is 3 kg and the polishing disk speed is 11 r / min. Finally, the root mean square roughness of the CdZnTe substrate surface is less than 1 nm.
[0063] Before the formal epitaxial HgCdTe process, the CdZnTe substrate needs to be pre-cleaned, including rinsing with acetone, rinsing with methanol, etching with 0.5% bromine methanol solution for 5 seconds, rinsing with methanol and drying with nitrogen. It is then quickly loaded into the epitaxial equipment and vacuumed to prepare for epitaxial growth.
[0064] Example 2
[0065] Pre-clean the CdZnTe substrate (A side) and the germanium wafer that have been double-sided polished, select a CdZnTe substrate with a thickness difference of less than 3μm, rinse with acetone and methanol, and then blow dry with nitrogen. The germanium wafer can be 8 inches.
[0066] The cleaned substrate material is quickly loaded into the vacuum chamber, and the vacuum chamber is evacuated to 1×10 -8 Torr or less.
[0067] The electron cyclotron resonance plasma (ECR) method was used to bombard the bonding surfaces of the CdZnTe and Ge wafers with Ar atoms at a radio frequency power of 100W for 6s to remove the surface oxide layer of the bonding surface and form a pure surface. At the same time, the root mean square roughness of the surface after atomic bombardment was ensured to be less than 1nm.
[0068] The surface treated CdZnTe substrate and germanium wafer are loaded into the wafer bonding equipment. At room temperature, the pressure is 11MPa for 50 minutes to ensure that the CdZnTe substrate and the germanium wafer are firmly bonded. The minimum spacing between the two CdZnTe substrates is controlled to be more than 1cm. The specific arrangement diagram is shown in the figure. Figure 2 shown.
[0069] The composite substrate after wafer bonding is subjected to high temperature annealing heat treatment, the annealing temperature is 600°C, and the annealing time is 2h.
[0070] The epitaxial surface (B side) of the CdZnTe substrate needs to be polished twice, and the CdZnTe substrate surface of the composite substrate is single-sided polished. SiC polishing materials with particle sizes of 0.1 and 0.03 microns are used for mechanical chemical polishing. The polishing pressure is 4Kg and the polishing disk speed is 9r / min. Finally, the root mean square roughness of the CdZnTe substrate surface is less than 1nm.
[0071] Before the formal epitaxial HgCdTe process, the CdZnTe substrate needs to be pre-cleaned, including rinsing with acetone, rinsing with methanol, etching with 0.5% bromine methanol solution for 5 seconds, rinsing with methanol and drying with nitrogen. It is then quickly loaded into the epitaxial equipment and vacuumed to prepare for epitaxial growth.
[0072] Comparative Example 1
[0073] A composite substrate was prepared according to the method in Example 1 and prepared for epitaxial growth, except that the radio frequency power of the Ar atom bombardment in Comparative Example 1 was 60W.
[0074] Comparative Example 2
[0075] A composite substrate was prepared according to the method in Example 1 and prepared for epitaxial growth, except that the Ar atom bombardment time in Comparative Example 2 was 10 s.
[0076] Comparative Example 3
[0077] A composite substrate was prepared according to the method in Example 1 and was ready for epitaxial growth, except that the bonding pressure in Comparative Example 3 was 6 MPa.
[0078] Comparative Example 4
[0079] A composite substrate was prepared according to the method in Example 1 and prepared for epitaxial growth, except that the annealing temperature in Comparative Example 4 was 500°C.
[0080] The composite substrates obtained in Examples 1-2 and Comparative Examples 1-4 were subjected to liquid phase epitaxial growth (maximum temperature of 540°C-550°C, growth process temperature of 450°C-490°C) and molecular beam epitaxial growth (temperature of 170°C-190°C), respectively. During the liquid phase epitaxial growth and molecular beam epitaxial growth processes, no bonding failure occurred in the composite substrates in Examples 1 and 2 of the present application. However, during the grinding and polishing and epitaxy processes after bonding, the composite substrates in Comparative Examples 1-4 experienced strain deformation due to lateral force or high temperature caused by grinding and polishing, and the stress exceeded the bonding force, resulting in debonding (the proportion of debonded cadmium zinc telluride sheets to all bonded cadmium zinc telluride sheets on a single germanium wafer was 30%-50%).
[0081] Finally, the HgCdTe material epitaxially grown on the composite substrate in Example 1 of the present invention and the HgCdTe material grown by bonding were used. In addition to the relatively lower cost of more epitaxial materials in batches, the temperature difference between CdZnTe sheets was reduced from 2% to 0.5%, and the thickness of the HgCdTe material and the difference between the component sheets were finally reduced from 3% to 0.5%.
[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a multi-sheet cadmium zinc telluride composite substrate, comprising the following steps: A) double-sided polishing of a plurality of irregular CdZnTe substrate sheets, and then cleaning the double-sided polished CdZnTe substrate sheets and germanium wafers; Among the plurality of irregular CdZnTe substrate sheets, the thickness difference between any two irregular CdZnTe substrate sheets is less than 3 μm; B) Under vacuum conditions, an Ar atomic beam is used to bombard the bonding surfaces of the cleaned CdZnTe substrate and the Ge wafer; The vacuum degree in step B) is 1×10 -8 Torr or less; the RF power of Ar atom bombardment is 80~100W, and the bombardment time is 4~6s; C) contacting the bombarded germanium wafer with the bonding surfaces of the plurality of cadmium zinc telluride substrate sheets, bonding the bombarded germanium wafer with the plurality of cadmium zinc telluride substrate sheets using a wafer bonding device, wherein the minimum spacing between any two cadmium zinc telluride substrate sheets is greater than 1 cm, thereby obtaining a bonded substrate; D) annealing the bonded substrates to obtain multiple pieces of CdZnTe composite substrates; The annealing temperature is 500-600° C., and the annealing time is 2-3 hours.
2. The preparation method according to claim 1, characterized in that: The cleaning in step A) is specifically as follows: The CdZnTe substrate and the Ge wafer were rinsed with acetone and methanol and then dried with nitrogen.
3. The preparation method according to claim 1, characterized in that: The bonding pressure in step C) is 9-11 MPa; the bonding time in step C) is 50-60 min.
4. A plurality of cadmium zinc telluride composite substrates prepared by the preparation method according to any one of claims 1 to 3.
5. Use of the multiple CdZnTe composite substrates as claimed in claim 4 in preparing HgCdTe materials by epitaxial growth.
6. The use according to claim 5, characterized in that: The multiple pieces of cadmium zinc telluride composite substrates are polished and cleaned in sequence and then used for epitaxial growth to prepare mercury cadmium telluride materials.
7. The use according to claim 6, characterized in that: The cleaning includes acetone washing, methanol washing, 0.5% bromine methanol solution corrosion, methanol washing and nitrogen blowing.