A method for transferring two-dimensional materials
By designing a method of carrying mesh and platinum reinforcement combined with focused ion beam processing, the problem of damage during the transfer of two-dimensional materials is solved, achieving efficient, precise transfer and structural integrity of materials, and is suitable for the application of various two-dimensional materials.
Patent Information
- Application Number
- CN202410895082.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing two-dimensional material transfer technology lacks control over material damage, resulting in possible damage to the material structure during the transfer process, affecting its physical and chemical properties, and limiting its effectiveness in precision applications.
A carrier net is used to transfer two-dimensional materials. The carrier net consists of at least two layers of stacked circular hole meshes, with the apertures decreasing from top to bottom. It is combined with platinum reinforcement and focused ion beam processing to reduce material damage and ensure structural integrity. .
It effectively reduces the damage of two-dimensional materials during the transfer process, maintains its physical and chemical properties, and is suitable for precision applications of various two-dimensional materials.
Smart Images

Figure CN118458773B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of two-dimensional material transfer, and in particular relates to a two-dimensional material transfer method. Background Art
[0002] Since physicists Andre Geim and Konstantin Novoselov from the University of Manchester in the UK successfully separated graphene from graphite for the first time using microcomputer exfoliation in 2004, two-dimensional materials have become a hot research hotspot in recent years due to their unique optical, thermal and electromagnetic properties. As the first two-dimensional material to be successfully exfoliated, graphene has attracted great attention from the scientific and industrial communities for its excellent physical properties, such as high electron mobility, excellent electrical and thermal conductivity, and outstanding mechanical strength. In addition to graphene, other two-dimensional materials such as transition metal sulfides, boron nitride and phosphorene have also become the focus of research due to their unique properties and broad application prospects.
[0003] Two-dimensional materials have broad application prospects in the field of new energy. In terms of solar cells, two-dimensional materials are considered to be ideal candidates to replace traditional transparent electrode materials due to their high conductivity and transparency. In addition, the high carrier mobility and excellent mechanical flexibility of two-dimensional materials make them have broad application prospects in flexible electronic devices. In the field of supercapacitors and batteries, the large specific surface area of two-dimensional materials helps to improve the energy and power density, while their excellent electrical conductivity can also effectively improve the charge and discharge performance of the device. For example, graphene-based supercapacitors have demonstrated ultra-high capacitance and excellent cycle stability. Although two-dimensional materials have great potential in these fields, the reliability of their mechanical properties is still a key factor in achieving their widespread application.
[0004] In addition to their applications in new energy technologies, two-dimensional materials also show great potential in the field of environmental protection. For example, graphene and other two-dimensional materials have important applications in water purification, air purification, and environmental monitoring. Due to their high surface area and rich surface chemistry, two-dimensional materials can effectively remove heavy metal ions, dyes, and organic pollutants from water. In addition, two-dimensional materials can also serve as efficient catalysts to promote the decomposition and transformation of harmful gases, thereby improving air quality.
[0005] In order to achieve safe and efficient application of two-dimensional materials in the fields of new energy and environmental protection, its mechanical properties must be studied in depth to ensure its reliability during use. The application of two-dimensional materials in energy devices requires not only excellent electrical and optical properties, but also stability under mechanical stress. Therefore, systematic research on the mechanical properties of two-dimensional materials and exploring the effects of different preparation and processing methods on their properties are the key to achieving their widespread application.
[0006] However, existing 2D material transfer technologies, such as mechanical exfoliation, usually lack control over material damage, which may lead to damage to the material structure during the transfer process. This damage affects the physical and chemical properties of the material during mechanical experiments, limiting its effectiveness in precision applications. Therefore, how to reduce the damage to the 2D material during the transfer process and maintain its original physical and chemical properties has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0007] The purpose of the present invention is to provide a method for transferring a two-dimensional material. The transfer method provided by the present invention can reduce the damage to the two-dimensional material during the transfer process.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] The present invention provides a method for transferring a two-dimensional material, comprising the following steps:
[0010] (1) dropping a suspension containing a two-dimensional material onto a carrier mesh, and then drying the carrier mesh to obtain a carrier mesh containing the two-dimensional material; the carrier mesh is composed of at least two layers of stacked circular hole meshes; and the pore size of the carrier mesh decreases from top to bottom;
[0011] (2) depositing a circle of platinum around the desired sample of the grid containing the two-dimensional material obtained in step (1), and then removing the two-dimensional material outside the platinum to obtain a reinforced two-dimensional material;
[0012] (3) Using a focused ion beam to process the reinforced two-dimensional material obtained in step (2) into a target shape to obtain a target sample; the current of the focused ion beam is 5-10 pA.
[0013] Preferably, the carrier mesh in step (1) is composed of two stacked layers of round hole mesh or three stacked layers of round hole mesh.
[0014] Preferably, when the carrier mesh is composed of two stacked layers of round hole meshes, the pore sizes of the two layers of round hole meshes are 35-40 μm and 25-30 μm, 35-40 μm and 15-20 μm, or 25-30 μm and 15-20 μm from top to bottom.
[0015] Preferably, when the carrier mesh is composed of three layers of stacked circular hole meshes, the apertures of the three layers of circular hole meshes are 35-40 μm, 25-30 μm and 15-20 μm from top to bottom, respectively.
[0016] Preferably, the apertures of the three-layer circular hole mesh are 39 μm, 29 μm and 19 μm from top to bottom.
[0017] Preferably, the sizes of the circular hole meshes in step (1) are the same; and the shape of the circular hole meshes is square.
[0018] Preferably, in the step (1), the circular holes in each layer of the circular hole mesh are arranged in a straight row, and adjacent circular holes are arranged tangentially.
[0019] Preferably, the drying temperature in step (1) is 40-60° C., and the drying time is 5-12 hours.
[0020] Preferably, before processing the reinforced two-dimensional material into the target shape in step (3), the step further includes overlapping the reinforced two-dimensional material with a push-pull device.
[0021] Preferably, the current of the focused ion beam in step (3) is 5 pA.
[0022] The present invention provides a method for transferring a two-dimensional material, comprising the following steps: dripping a suspension containing a two-dimensional material onto a carrier net, and then drying to obtain a carrier net containing the two-dimensional material; the carrier net is composed of at least two layers of stacked circular hole nets; the aperture of the carrier net decreases from top to bottom; depositing a circle of platinum around the desired sample of the carrier net containing the two-dimensional material, and then removing the two-dimensional material outside the platinum to obtain a reinforced two-dimensional material; using a focused ion beam to process the reinforced two-dimensional material into a target shape to obtain a target sample; the current of the focused ion beam is 5-10pA. The present invention designs the structure of the carrier net, and through the graded aperture design, utilizes the coordination of gravity and aperture size, which can not only provide physical support, but also protect the structural integrity of the two-dimensional material through the buffering effect between layers. Afterwards, in order to prevent the two-dimensional material from bending or breaking during the transfer and focused ion beam operation, a circle of platinum (Pt) is deposited around the desired sample to reinforce the two-dimensional material; and then the two-dimensional material is processed into the target shape, and by controlling the current, the damage of the ion beam to the sample can be reduced to ensure the structural integrity of the sample. Experimental results show that the transfer method provided by the present invention can reduce the transfer damage of two-dimensional materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of the structure of a three-layer circular hole mesh provided by the present invention;
[0024] Figure 2 It is a schematic structural diagram of a carrier network containing two-dimensional materials of the present invention;
[0025] Figure 3 A schematic diagram of depositing a circle of platinum around a sample required for a grid containing a two-dimensional material according to the present invention;
[0026] Figure 4 This is a schematic diagram of removing the two-dimensional material on the outside of platinum according to the present invention;
[0027] Figure 5A schematic diagram of the reinforced two-dimensional material of the present invention overlapping with the push-pull device;
[0028] Figure 6 It is a schematic diagram of the structure of the target sample of the present invention;
[0029] Figure 7 This is an electron microscope image of the target sample prepared in Example 1;
[0030] Figure 8 This is an electron microscope image of the target sample prepared in Comparative Example 1;
[0031] Fig. 9 This is an electron microscope image of the target sample prepared in Example 2. DETAILED DESCRIPTION
[0032] The present invention provides a method for transferring a two-dimensional material, comprising the following steps:
[0033] (1) dropping a suspension containing a two-dimensional material onto a carrier mesh, and then drying the carrier mesh to obtain a carrier mesh containing the two-dimensional material; the carrier mesh is composed of at least two layers of stacked circular hole meshes; and the pore size of the carrier mesh decreases from top to bottom;
[0034] (2) depositing a circle of platinum around the desired sample of the grid containing the two-dimensional material obtained in step (1), and then removing the two-dimensional material outside the platinum to obtain a reinforced two-dimensional material;
[0035] (3) Using a focused ion beam to process the reinforced two-dimensional material obtained in step (2) into a target shape to obtain a target sample; the current of the focused ion beam is 5-10 pA.
[0036] The transfer method provided by the present invention is applicable to any two-dimensional material, preferably to two-dimensional materials in suspension, such as MXenes. MXenes are derived from the parent MAX phase and have the general formula M n+1 X n T x (n is 1, 2, or 3), wherein M represents a transition metal (Ti, Mo, Nb, V, etc.), X represents carbon and / or nitrogen, T x Represents surface functional groups (-O, -OH, -F), MXenes including Ti3C2T x , Ti2CT x wait.
[0037] The present invention has no particular limitation on the sources of the raw materials used, and any raw materials may be prepared using commercially available products or well-known preparation methods known to those skilled in the art.
[0038] The invention drips a suspension containing the two-dimensional material onto a carrier mesh, and then dries the carrier mesh to obtain the carrier mesh containing the two-dimensional material.
[0039] The present invention has no special limitation on the preparation method of the suspension containing the two-dimensional material, and the suspension may be prepared by methods well known to those skilled in the art.
[0040] The present invention has no particular limitation on the rate of the dripping, and operations familiar to those skilled in the art may be used.
[0041] In the present invention, the grid is composed of at least two layers of stacked circular hole grids, preferably two layers of stacked circular hole grids or three layers of stacked circular hole grids. The present invention designs the structure of the grid, and through graded aperture design, utilizes the coordination of gravity and aperture size, which can not only provide physical support, but also protect the structural integrity of the two-dimensional material through the buffering effect between layers.
[0042] In the present invention, the apertures of the carrier mesh decrease from top to bottom.
[0043] In the present invention, when the carrier mesh is composed of two layers of stacked circular hole meshes, the apertures of the two layers of circular hole meshes are preferably 35-40 μm and 25-30 μm, 35-40 μm and 15-20 μm, or 25-30 μm and 15-20 μm, and more preferably 39 μm and 29 μm, 39 μm and 19 μm, or 29 μm and 19 μm, respectively. The present invention can further improve the structural integrity of the two-dimensional material by controlling the aperture of the circular hole mesh.
[0044] In the present invention, when the carrier mesh is composed of three layers of stacked circular hole meshes, the apertures of the three layers of circular hole meshes are preferably 35-40 μm, 25-30 μm and 15-20 μm from top to bottom, and more preferably 39 μm, 29 μm and 19 μm. The present invention can further improve the structural integrity of the two-dimensional material by controlling the aperture of the circular hole mesh.
[0045] In the present invention, the sizes of the circular hole mesh are preferably the same; the shape of the circular hole mesh is preferably square; and the hole diameter size of each layer of the circular hole mesh is preferably the same.
[0046] In the present invention, the arrangement of the circular holes in each layer of circular hole net is preferably in a straight row; the adjacent circular holes are preferably arranged tangentially; the distance between the centers of the adjacent circular holes is preferably 1 to 2 times the hole diameter, more preferably 1.5 times; the thickness of each layer of circular hole net is independently preferably 0.15 mm. The present invention can further reduce transfer damage by limiting the arrangement of the circular holes, the distance between the centers of the circles, and the thickness; and the strength of the carrier net can be ensured by controlling the distance between the centers of the circles, thereby avoiding structural weaknesses.
[0047] The structural schematic diagram of the three-layer circular hole net provided by the present invention is as follows Figure 1 shown.
[0048] from Figure 1 It can be seen that it is a three-layer multi-aperture grid, and the three layers are connected in a prism-like manner, which is convenient for combination and disassembly; the rectangular hole on the right is the designed clamping part, which is designed to facilitate the use of tweezers or hand-held, which is convenient for experiments and can also avoid hands touching the two-dimensional material on the device.
[0049] The at least two-layer circular hole mesh design of the present invention can effectively capture and support two-dimensional materials.
[0050] Hierarchical aperture design: The multi-level aperture size design can catch fragments of two-dimensional materials of different sizes, thereby optimizing the capture rate of materials and reducing losses. By utilizing the combination of gravity and aperture size, two-dimensional materials can be captured more gently, which is especially suitable for two-dimensional materials that are stable in liquid media. It also avoids the phenomenon that when using large-aperture gridless copper mesh on the market, when the two-dimensional material solution is added, the two-dimensional material often leaks out of the pores. Decreasing aperture: The aperture that decreases layer by layer allows large pieces of two-dimensional materials to be screened first, and smaller two-dimensional materials are then captured by the next layer. This decreasing method can avoid excessive movement of materials in the device and reduce the risk of damage.
[0051] Hierarchical structure: This structure not only provides physical support but also protects the structural integrity of the 2D material through buffering between layers.
[0052] In the present invention, the material of the carrier mesh is preferably silicon. The carrier mesh of the present invention is a silicon carrier mesh, which has the following advantages compared to using a copper mesh to support two-dimensional materials:
[0053] Smoothness: Silicon grids provide a very smooth surface, which is especially important for 2D materials that require precise properties.
[0054] Chemical inertness: Pure silicon grids are relatively chemically inert, meaning they are less likely to chemically react with 2D materials, reducing unwanted chemical adsorption.
[0055] Thermal Stability: Silicon has good thermal stability and thermal conductivity, making it suitable for processes that may involve heat treatment.
[0056] Optical Properties: The transparency of silicon grids makes them suitable for optical applications such as sample preparation for scanning electron microscopy (SEM).
[0057] Processability: Silicon grids can be precisely processed by standard photolithography and etching techniques, making it easy to manufacture multi-layer porous structures.
[0058] In the present invention, the drying temperature is preferably 40-60°C, more preferably 50°C; the drying time is preferably 5-12h, more preferably 12h; the drying pressure is preferably 0.1-50MPa, more preferably 50MPa.
[0059] After obtaining a carrier mesh containing a two-dimensional material, the present invention deposits a circle of platinum around the sample required for the carrier mesh containing the two-dimensional material, and then removes the two-dimensional material outside the platinum to obtain a reinforced two-dimensional material. The present invention deposits a circle of platinum around the required sample according to its size to reinforce the two-dimensional material, thereby reducing damage to the two-dimensional material when it is transferred from the carrier mesh to the push-pull device; the present invention removes the two-dimensional material outside the platinum to separate the two-dimensional material from the carrier mesh.
[0060] In the present invention, the platinum is preferably not in contact with the grid.
[0061] The present invention has no special limitation on the deposition operation, and the operation can be selected according to common sense.
[0062] In the present invention, the thickness of the platinum is preferably 0.1 μm, and the width of the platinum is preferably 0.5 μm.
[0063] In the present invention, the operation of removing the two-dimensional material on the outside of the platinum is preferably to remove the two-dimensional material on the left side of the platinum, then use platinum to bond the manipulator and the left side of the two-dimensional material together, and then remove the two-dimensional materials on the other three sides.
[0064] The present invention has no special limitation on the operations of removing the two-dimensional material on the left side of platinum, then using platinum to adhere the robot and the left side of the two-dimensional material together, and then removing the two-dimensional materials on the other three sides, and conventional operations familiar to those skilled in the art can be used.
[0065] After obtaining the reinforced two-dimensional material, the present invention uses a focused ion beam to process the reinforced two-dimensional material into a target shape to obtain a target sample.
[0066] In the present invention, before processing the reinforced two-dimensional material into the target shape, the reinforced two-dimensional material is preferably overlapped with the push-pull device; the reinforced two-dimensional material is preferably aligned with the stretching area of the push-pull device. The present invention overlaps the two-dimensional material with the push-pull device in order to transfer the two-dimensional material to the test gap of the push-pull device.
[0067] In the present invention, after the reinforced two-dimensional material overlaps with the push-pull device, platinum is preferably deposited at both ends of the two-dimensional material. The present invention has no particular limitation on the operation of depositing platinum at both ends of the two-dimensional material, and an operation well known to those skilled in the art can be used. Depositing platinum at both ends of the two-dimensional material can make the two-dimensional material and the push-pull device adhere firmly.
[0068] In the present invention, the current of the focused ion beam is 5-10 pA, preferably 5 pA. The present invention reduces the damage of the ion beam to the sample by adopting a smaller current.
[0069] The structural schematic diagram of the carrier network containing two-dimensional materials of the present invention is as follows Figure 2 As shown; the schematic diagram of the present invention depositing a circle of platinum around the sample required for the grid containing the two-dimensional material is as shown Figure 3 As shown; the schematic diagram of the present invention when removing the two-dimensional material outside the platinum is as shown Figure 4 As shown; the schematic diagram of the reinforced two-dimensional material of the present invention overlapping with the push-pull device is as shown Figure 5 As shown; the structural schematic diagram of the target sample of the present invention is as shown Figure 6 shown.
[0070] from Figures 2 to 6 The process of preparing the target sample of the present invention can be clearly understood, which shows a series of finely controlled steps of preparation to ensure the quality of the two-dimensional material and maintain it in the best state before the stretching experiment.
[0071] The transfer method provided by the present invention can minimize the damage that may be caused to the sample during the preparation process, laying the foundation for the subsequent effective evaluation of the mechanical properties of the two-dimensional material.
[0072] The invention can handle a wider range of 2D material types, including those synthesized by chemical vapor deposition (CVD) and those in suspension. This versatility enables research and application development to cover a wider variety of 2D materials, thereby exploring and utilizing the unique properties of these materials.
[0073] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0074] Example 1
[0075] The transfer method of the two-dimensional material MXene is as follows:
[0076] (1) 1.6 g LiF was slowly dissolved in 40 mL 6 mol / L hydrochloric acid and stirred for 15 min to ensure complete dissolution. Then, 1 g Ti3AlC2 (200 mesh MAX phase Ti3AlC2) was slowly added and etched at 35 °C for 30 h. The etched solution was first washed twice with 1 mol / L hydrochloric acid, then washed with deionized water and centrifuged for 5 min, and repeated 6 times until the pH value of the solution was greater than 6. The precipitate was collected by vacuum filtration and finally placed in a vacuum drying oven, dried at 50 °C for 12 h, then dissolved with deionized water, and manually shaken for 30 min and centrifuged for 30 min to obtain a single layer of Ti3C2T x Suspension;
[0077] (2) dripping the suspension obtained in step (1) onto a silicon carrier mesh, and then drying to obtain a carrier mesh containing a two-dimensional material; wherein the carrier mesh is composed of three layers of circular hole mesh stacked in sequence from top to bottom; the apertures of the three layers of circular hole mesh are 39 μm, 29 μm and 19 μm, respectively; the three layers of circular hole mesh have the same size; the three layers of circular hole mesh are in the shape of a square; the circular holes in each layer of the circular hole mesh are arranged in a straight row, adjacent circular holes are tangent to each other, and the distance between the centers of adjacent circular holes is 1.5 times the aperture; the thickness of each layer of the circular hole mesh is 0.15 mm; the drying temperature is 50°C, the drying time is 12 h, and the pressure is 50 MPa;
[0078] (3) depositing a circle of platinum around the desired sample of the grid containing the two-dimensional material obtained in step (2), then removing the two-dimensional material on the left side of the platinum, and then using platinum to adhere the manipulator and the left side of the two-dimensional material together, and then removing the two-dimensional materials on the other three sides to obtain a reinforced two-dimensional material; wherein the platinum has a thickness of 0.1 μm and a width of 0.5 μm; and the platinum does not contact the grid;
[0079] (4) Overlapping the reinforced two-dimensional material obtained in step (3) with a push-pull device so that the two-dimensional material is aligned with the stretching area of the push-pull (PTP) device, and then platinum is deposited on both ends of the two-dimensional material. After that, a focused ion beam is used to cut the two-dimensional material into a target shape to obtain a target sample; wherein the current of the focused ion beam is 5 pA.
[0080] The electron microscope image of the target sample prepared in Example 1 is as follows: Figure 7 shown.
[0081] Comparative Example 1
[0082] On the basis of Example 1, the silicon carrier mesh was changed to a 400-mesh copper mesh, and other conditions remained unchanged to obtain the target sample.
[0083] The electron microscope image of the target sample prepared in Comparative Example 1 is as follows: Figure 8 shown.
[0084] from Figure 7 and 8 It can be seen that the transfer method of the present invention can transfer the two-dimensional material completely without holes, while the two-dimensional material cannot be completely transferred using the transfer method of comparative example 1 and holes exist, indicating that the transfer method of the present invention can reduce the damage to the two-dimensional material during the transfer process.
[0085] Example 2
[0086] On the basis of Example 1, the structure of the carrier grid was changed, that is, the carrier grid consisted of two stacked layers of round hole grids; the apertures of the two layers of round hole grids were 35 μm and 25 μm from top to bottom, respectively, and other conditions remained unchanged, to prepare the target sample.
[0087] The electron microscope image of the target sample prepared in Example 2 is as follows: Fig. 9 shown.
[0088] from Fig. 9 It can be seen that the transfer method of the present invention can reduce the damage to the two-dimensional material during the transfer process.
[0089] It can be seen from the above embodiments and comparative examples that the transfer method provided by the present invention can reduce the damage to the two-dimensional material during the transfer process.
[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for transferring a two-dimensional material, comprising the following steps: (1) dropping a suspension containing a two-dimensional material onto a carrier mesh, and then drying the carrier mesh to obtain a carrier mesh containing the two-dimensional material; the carrier mesh is composed of at least two layers of stacked circular hole meshes; and the pore size of the carrier mesh decreases from top to bottom; (2) depositing a circle of platinum around the desired sample of the grid containing the two-dimensional material obtained in step (1), and then removing the two-dimensional material outside the platinum to obtain a reinforced two-dimensional material; (3) Using a focused ion beam to process the reinforced two-dimensional material obtained in step (2) into a target shape to obtain a target sample; the current of the focused ion beam is 5-10 pA.
2. The transfer method according to claim 1, characterized in that: The carrier mesh in step (1) is composed of two layers of stacked circular hole meshes or three layers of stacked circular hole meshes.
3. The transfer method according to claim 2, characterized in that: When the carrier mesh is composed of two stacked layers of round hole meshes, the apertures of the two layers of round hole meshes are 35-40 μm and 25-30 μm, 35-40 μm and 15-20 μm, or 25-30 μm and 15-20 μm from top to bottom.
4. The transfer method according to claim 2, characterized in that: When the carrier mesh is composed of three layers of stacked circular hole meshes, the apertures of the three layers of circular hole meshes are 35-40 μm, 25-30 μm and 15-20 μm from top to bottom.
5. The transfer method according to claim 4, characterized in that: The apertures of the three-layer circular hole mesh are 39 μm, 29 μm and 19 μm from top to bottom.
6. The transfer method according to claim 1, characterized in that: The sizes of the circular hole meshes in step (1) are the same; and the shape of the circular hole meshes is square.
7. The transfer method according to claim 1, characterized in that: In the step (1), the circular holes in each layer of the circular hole mesh are arranged in a straight row, and adjacent circular holes are arranged tangentially.
8. The transfer method according to claim 1, characterized in that: The drying temperature in step (1) is 40-60° C. and the drying time is 5-12 hours.
9. The transfer method according to claim 1, characterized in that: Before processing the reinforced two-dimensional material into the target shape in the step (3), the step also includes overlapping the reinforced two-dimensional material with the push-pull device.
10. The transfer method according to claim 1, characterized in that: The current of the focused ion beam in step (3) is 5 pA.
Citation Information
Patent Citations
Preparation method of electrical test microelectrode for two-dimensional layered material sample
CN109946340A
Post-treatment of nonwoven webs
EP0695383A1
Nanoparticle production and corresponding structures
US20060147369A1
Method for the fabrication of a pore comprising metallic membrane and a pore comprising membrane
US20220008870A1