A composite filler for denitrification and dephosphorization, preparation method and application thereof
Composite fillers prepared from polysulfone polymers and mixed denitrification electron donor materials solve the problems of poor nitrogen and phosphorus removal stability and insufficient rainfall impact resistance in rainwater runoff treatment, achieving efficient and stable pollutant treatment. and system performance improvements.
Patent Information
- Application Number
- CN202410799265.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-20
AI Technical Summary
In the existing rainwater runoff treatment, it is difficult for the improved medium to ensure long-term, efficient and stable nitrogen and phosphorus removal, and the slow-release carbon source has insufficient ability to impact rainfall, and the pores are difficult to control, resulting in a decline in system performance.
Polysulfone polymer is used as the skeleton, and a denitrification and phosphorus removal composite filler with a spherical structure is prepared by immersion precipitation phase transformation method and mixed culture denitrification electron donor materials, and the proportion of pores and electron donors is controlled to construct a highly adaptable, Composite filler with good stability, used in bioretention systems.
It achieves efficient treatment of pollutants NO3--N and PO43--P, ensures the long-term operation stability of the system, improves the strength and slow-release performance of the composite filler, and adapts to complex and changeable rainwater conditions.
Smart Images

Figure CN118458938B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water treatment, and more particularly to a denitrification and dephosphorization composite filler, a preparation method and application thereof. Background Art
[0002] The continuous development of urbanization has led to the prominent problem of rainwater runoff pollution. Rainwater runoff contains a large amount of nitrate nitrogen (NO3 - -N) and phosphate phosphorus (PO4 3- -P) and other substances can pose serious threats to aquatic ecosystems, human health and the economy.
[0003] At present, the bioretention system is mainly used to treat rainwater runoff pollution. It has a flexible design and can treat rainwater through physical, chemical and biological synergy. However, most improved media cannot guarantee the long-term, efficient and stable removal of the above substances. At the same time, there is a lack of sufficient biodegradable organic matter in rainwater runoff to maintain heterotrophic denitrification. In addition, it is challenging to accurately control the amount of carbon source added in decentralized treatment facilities. Inadequate control may lead to problems such as organic matter and nitrogen and phosphorus leaching and system performance degradation.
[0004] Therefore, how to develop a composite filler or improved medium filler with high efficiency, stability, adaptability and sustainability for nitrogen and phosphorus removal to simultaneously remove NO3 in sewage? - -N and PO4 3- -P, has important practical needs. Summary of the invention
[0005] The present invention aims at the problems that the denitrification and phosphorus removal stability of the dispersed granular and powdery modified media is poor, easy to cause clogging, easy to lose, and the slow-release carbon source composite filler has insufficient ability to resist rainfall impact and difficult to control the pores. The present invention provides a denitrification and phosphorus removal composite filler, a preparation method and its application in rainwater runoff treatment and other low carbon-nitrogen ratio wastewater treatment. The present invention can specifically control the pores and electron donor ratio of the composite filler according to the characteristics of the pollutants, construct a denitrification and phosphorus removal composite filler with strong adaptability and good stability, and realize the removal of NO3 in the pollutants. - -N and PO4 3- -P High efficiency processing and ensuring the stability of long-term operation of the system.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A denitrification and dephosphorization composite filler, the denitrification and dephosphorization composite filler is a spherical structure, the particle size is 3-5 mm, and the specific surface area is 2-4 m 2 / g, load-bearing ≥500 g;
[0008] The denitrification and dephosphorization composite filler is prepared with a polysulfone polymer as a skeleton and a mixed culture denitrification electron donor material through an immersion precipitation phase conversion method.
[0009] The above technical solution has at least the following technical effects:
[0010] The composite filler designed by the present invention is suitable as an improved medium for the filler layer of the biological retention system in terms of shape, particle size, specific surface area, and strength performance. The composite filler uses a polysulfone polymer as a skeleton and is composited with a mixed culture denitrification electron donor material. While improving the strength of the composite filler, it can also promote nitrogen and phosphorus removal, which is beneficial for the biological retention system to adapt to complex and changeable rainwater conditions.
[0011] Preferably, the polysulfone polymer includes any one of polysulfone, polyethersulfone and polyarylsulfone;
[0012] The mixed-culture denitrification electron donor material comprises at least one heterotrophic denitrification electron donor material and one autotrophic denitrification electron donor material;
[0013] Wherein, the electron donor for heterotrophic denitrification includes a natural carbon source or an artificial carbon source;
[0014] The natural carbon source can be wood chips, straw, plant debris, etc.
[0015] The artificial carbon source can be polycaprolactone (PCL), a copolymer of 3-hydroxybutyrate and 3-hydroxyvalerate (PHBV), etc.
[0016] The electron donor for the autotrophic denitrification includes one or a mixture of pyrite, pyrite and elemental sulfur;
[0017] Furthermore, the electron donor of the autotrophic denitrification includes pyrite and / or pyrite;
[0018] The mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is 1:3 to 3:1;
[0019] The mass ratio of the polysulfone polymer to the mixed culture denitrification electron donor material is 1:2-4:1.
[0020] The use of the above technical scheme includes at least the following technical effects: the composite filler contains two electron donor materials, heterotrophic denitrification and autotrophic denitrification, which helps to promote mixed denitrification. Mixed denitrification has the advantages of high nitrogen removal efficiency, low by-products, stable pH, fast startup, and long operating cycle. The added ferrous sulfide compounds, such as pyrite and / or pyrite, help to remove phosphorus through the precipitation of dissolved divalent iron.
[0021] The second object of the present invention is to provide a method for preparing a denitrification and dephosphorization composite filler, which specifically comprises the following steps:
[0022] S1, placing a polysulfone polymer in an organic solvent and stirring to dissolve;
[0023] S2, adding the solution obtained in S1 to the mixed culture denitrification electron donor material and stirring evenly;
[0024] S3, dripping the solution obtained in S2 into a non-solvent to form a ball, with a dripping speed of 60 to 100 drops per minute, and letting it stand for more than 2 days;
[0025] S4, washing and drying the composite material prepared in S3 for later use.
[0026] Preferably, the mass fraction of the polysulfone polymer in the solution obtained in step S2 is 5% to 20%.
[0027] Preferably, the organic solvent in step S1 is any one of N, N-dimethylformamide, N, N-dimethylacetamide or N-methylpyrrolidone;
[0028] The non-solvent includes water or ethanol.
[0029] The beneficial effects of adopting the above technical solution include at least that the composite filler can achieve control of filler pores by changing the mass fraction of the polysulfone polymer during the preparation process, thereby achieving control of the carbon release rate.
[0030] Preferably, the mass fraction of the polyculture denitrification electron donor material in the solution obtained in step S2 is 5% to 10%.
[0031] Preferably, the solution obtained in step S2 is further added with a material having an adsorption property and / or a porogen;
[0032] The adsorption material is selected to be activated carbon and / or biochar;
[0033] The porogen is selected from polyethylene glycol.
[0034] The beneficial effects of adopting the above technical solution include at least: the composite filler can control the function of the filler by changing the mass fraction of the mixed culture denitrification electron donor material, which is beneficial to denitrification under rainwater conditions with different carbon-nitrogen ratios. Adding adsorption performance materials to the composite filler is beneficial to further improve the adsorption capacity of the composite filler for other pollutants, and adding porogens can further increase the pores on the surface of the composite filler and increase the carbon release rate.
[0035] The third object of the present invention is to apply the above-mentioned composite filler in sewage treatment systems, chemical production, biological research and artificial wetlands;
[0036] Further, the composite filler is used in bioretention systems, biofilters, packed bed reactors and artificial wetlands in urban sewage and / or rainwater treatment systems;
[0037] The composite filler designed by the present invention includes but is not limited to the above-mentioned applications.
[0038] A fourth object of the present invention is to provide a novel bioretention system, comprising the above-mentioned composite filler, wherein the composite filler is arranged in a flooded area of the novel bioretention system;
[0039] The proportion of the polysulfone polymer and the mixed culture denitrification electron donor material in the composite filler is determined according to the rainwater runoff water quality and rainfall characteristics in the target area.
[0040] Preferably, when the carbon-nitrogen ratio of rainwater in the target area is ≤3, the mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is ≥1:1;
[0041] When the carbon-nitrogen ratio of rainwater is greater than 3, the mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is less than 1:1;
[0042] and / or,
[0043] If the dry period before rain in the target area is ≥ 10 days, the mass fraction of the polysulfone polymer is selected as follows: 12% ≤ the mass fraction of the polysulfone polymer ≤ 20%,
[0044] Regulating the total pore volume: 0.01 mL / g<total pore volume≤0.02 mL / g to reduce the carbon source release rate of the composite material;
[0045] If the dry period before rain in the target area is less than 10 days, the mass fraction of the polysulfone polymer is selected as follows: 5% ≤ the mass fraction of the polysulfone polymer < 12%
[0046] The total pore volume was adjusted to: 0.02 mL / g<total pore volume≤0.03 mL / g to increase the carbon source release rate of the composite material.
[0047] The beneficial effects of adopting the above technical solution include at least: the composite filler can control the carbon release rate by regulating the pores, and then be applied to target areas with different pre-rain drying periods, reducing the carbon release rate in target areas with longer drying periods, and increasing the carbon release rate in target areas with shorter drying periods.
[0048] Preferably, the volume ratio of the composite filler to the flooded area is 20% to 100%;
[0049] The composite filler can be added alone or mixed with traditional fillers.
[0050] Furthermore, the traditional filler is selected from one or a mixture of quartz sand, zeolite or ceramsite.
[0051] The adding method is selected from mixed filling or layered filling.
[0052] Furthermore, the bioretention system is started by natural biofilm formation or inoculated biofilm formation, and promotes microbial enrichment through continuous water inflow of artificially prepared simulated rainwater runoff, and receives actual rainwater runoff after 1 to 2 weeks of startup.
[0053] According to the above technical solution, the present invention at least includes the following technical effects:
[0054] (1) The present invention uses an immersion precipitation phase transformation method to composite a powdered electron donor material that is cheap, easily available, has excellent denitrification performance, and is difficult to recycle with a polysulfone polymer skeleton. This method is not only simple and easy to operate, and the ball formation is uniform; the prepared new composite filler also has the advantages of good sustained release performance, high strength, stable structure, easy pore control, and strong electron donor synergy.
[0055] (2) The new composite filler designed in the present invention is added to the flooded area of the biological retention system. The appropriate preparation parameters and addition method of the new composite filler can be selected according to the rainwater runoff water quality characteristics and rainfall characteristics of the application scenario. It is targeted and flexible. The constructed biological retention system has excellent nitrogen and phosphorus removal performance and has broad application prospects in rainwater runoff treatment and other low carbon-nitrogen ratio wastewater treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0057] Figure 1 It is a physical picture of the composite filler prepared in Examples 1-2 of the present invention and Comparative Example 1;
[0058] Figure 2 It is the internal SEM picture of the denitrification and dephosphorization composite filler prepared in Examples 1-2 of the present invention and Comparative Example 1;
[0059] Figure 3 The composite filler prepared in Example 3-5 of the present invention is a real picture and a real picture after being immersed in pure water for 100 days;
[0060] Figure 4 is a graph of carbon release performance of the composite filler prepared in Examples 3-5 of the present invention;
[0061] Figure 5It is a schematic diagram of the structural device of the biological retention system of Examples 6-7 and Example 9 of the present invention.
[0062] In the attached figure:
[0063] 1-planting; 2-planting soil layer; 3-filling layer; 4-new composite filler mixed layer; 5-gravel drainage layer; 6-overflow pipe; 7-valve; 8-flooded area drainage pipe. DETAILED DESCRIPTION
[0064] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0065] In the description of the present invention, it is necessary to understand that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0066] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0067] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0068] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature. Example 1
[0069] This embodiment provides a method for preparing a denitrification and dephosphorization composite filler, comprising the following steps:
[0070] S1, placing polysulfone in N, N-dimethylformamide organic solvent and stirring to dissolve;
[0071] S2, adding polycaprolactone (PCL) and pyrite to the polysulfone solution obtained in S1 and stirring evenly, the mass ratio of polycaprolactone (PCL) and pyrite is 1:1, and the total mass fraction of polycaprolactone (PCL) and pyrite in the solution is 5%;
[0072] Wherein, the mass fraction of polysulfone in the solution obtained in step S2 is 15%;
[0073] S3, dripping the solution obtained in step S2 into excess deionized water at room temperature to form balls, with a dripping rate of 60 drops per minute, and letting it stand for 2 days; as long as the obtained solution can be dripped into deionized water to form balls, the amount of deionized water is not limited.
[0074] S4, washing the obtained composite filler P1 with deionized water and drying it for later use. Example 2
[0075] The only difference between Example 2 and Example 1 is that the mass fraction of polysulfone in the solution obtained in step S2 is 20%, and the masses of polysulfone and organic solvent can be adjusted to obtain a composite filler P2.
[0076] Comparative Example 1
[0077] The only difference between Comparative Example 1 and Example 1 is that the mass fraction of polysulfone in the solution obtained in step S2 is 25%, and the masses of polysulfone and organic solvent can be adjusted to obtain a composite filler P3.
[0078] The actual picture of composite filler P1, P2, P3 is as follows Figure 1 As shown:
[0079] P1 and P2 have good sphericity, and P2 is ellipsoidal. The particle size is detected by vernier caliper, and the particle size is between 3 and 5 mm. The compression strength of the three composite materials is measured by electronic universal testing machine. It is found that when the compression degree reaches 85%, the peak stress of P1, P2, and P3 are 350.3 MPa, 420.7 MPa, and 530.9 MPa, respectively.
[0080] P3 has very poor balling properties and severe tailing.
[0081] Figure 2 The internal SEM images of the three composite fillers P1, P2, and P3 obtained by scanning electron microscopy (FEI Qtanta, 250FEG);
[0082] Among them, the pore structure of P1 and P2 composite fillers is obvious, the mixed culture denitrification electron donor material is evenly loaded, and the porosity decreases with the increase of polysulfone concentration; the porosity of P3 composite filler is poor, and the mixed culture denitrification electron donor material is prone to aggregation. Example 3
[0083] This embodiment provides a method for preparing a denitrification and dephosphorization composite filler, comprising the following steps:
[0084] S1, placing polysulfone in N, N-dimethylformamide organic solvent and stirring to dissolve;
[0085] S2, add 5 g sawdust and 5 g pyrite to the polysulfone solution obtained in S1 and stir evenly, the total mass fraction of sawdust and pyrite in the solution is 10%;
[0086] Wherein, the added amount of polysulfone is 8g, and the organic solvent of N, N-dimethylformamide is 82g;
[0087] The mass fraction of polysulfone in the solution obtained in step S2 is 8%;
[0088] S3. Drop the solution obtained in step S2 into excess deionized water at room temperature to form a ball at a rate of 60 drops per minute, and let it stand for 5 days.
[0089] S4, washing the obtained composite filler P4 with deionized water and drying it for later use. Example 4
[0090] The difference between Example 4 and Example 3 is that the amount of polysulfone added is 12 g, and the amount of N, N-dimethylformamide organic solvent is 78 g;
[0091] The mass fraction of polysulfone in the solution obtained in step S2 is 12%, and a composite filler P5 is obtained. Example 5
[0092] The difference between Example 5 and Example 3 is that the amount of polysulfone added is 16 g, and the amount of N, N-dimethylformamide organic solvent is 74 g;
[0093] The mass fraction of polysulfone in the solution obtained in step S2 is 16%, and a composite filler P6 is obtained.
[0094] The actual picture of the composite filler prepared in Example 3-5 is as follows Figure 3 As shown:
[0095] The sphericity of the composite fillers P4, P5, and P6 was good, and the particle size was measured by vernier caliper, and the particle size was between 3 and 4 mm;
[0096] Weigh 1 g of each of the three materials and place them in three 150 mL conical flasks. Add 100 mL of the same batch of deionized water, seal the flasks, control the test temperature at 25°C, and rotate at 100 r / min. Take samples regularly to monitor the DOC concentration. Change the water after each sampling. The test lasts for 100 days. Figure 3 As shown in the figure, the volume and structure of the three materials did not change much after immersion for 100 days, indicating that the composite filler structure was stable. The compressive strength of the three composite materials was measured by an electronic universal testing machine. It was found that when the compression degree reached 85%, the peak stresses of P4, P5, and P6 were 27.2 MPa, 83.0 MPa, and 374.2 MPa, respectively. From P4 to P6, the strength increased and the porosity decreased. The specific surface areas of the three materials were determined by specific surface area and pore size analyzers, which were all between 2.33 and 3.59 m 2 / g.
[0097] Figure 4 The carbon release performance (measured in DOC concentration) of P4, P5, and P6 composite fillers compared with sawdust is shown in the figure below. Figure 4 As shown in the data, compared with the original dispersed sawdust material, the carbon source release rate and release amount of the three composite fillers were significantly reduced, which is sustainable. At the same time, the carbon source release rate decreased with the increase of polysulfone concentration. The new composite filler achieved the regulation of carbon source release rate by regulating the pores. Example 6
[0098] This embodiment provides a bioretention system, the structure of which is as follows Figure 5 As shown: specifically, it includes a planting soil layer 2, a planting plant 1 arranged on the top of the planting soil layer, a filler layer 3, a new composite filler mixed layer 4, and a gravel drainage layer 5 located at the bottom of the planting soil layer in sequence;
[0099] An overflow pipe 6 located at the top side of the planting soil layer;
[0100] A flooded area drainage pipe 8 is located at the side end of the gravel drainage layer 5, and a valve 7 for controlling the opening and closing of the flooded area drainage pipe.
[0101] The bioretention system in this embodiment simulates two application scenarios:
[0102] That is, the dry period before the rainy season is long ≥ 10 days and the dry period before the rainy season is short < 10 days, and the carbon-nitrogen ratio of rainwater is < 3;
[0103] Adding the prepared composite filler P4 to the novel composite filler mixed layer 4, wherein the novel composite filler layer 4 also includes quartz sand;
[0104] The volume ratio of P4 composite filler in the flooded area is 30%;
[0105] A bioretention system P4-BS was constructed to remove nitrogen and phosphorus from rainwater runoff, and inoculation and biofilm were used to start the process.
[0106] During the formal operation phase, it will contain 10 mg / L NO3 - -N and 2 mg / L PO4 3- -P simulated rainwater runoff was introduced into the bioretention system, which was 70 cm high and 20 cm in diameter, with 5.5 L of water in each inlet. The NO3 - -N and PO4 3- The effluent concentrations of -P were 0.30~1.23 mg / L and 0~0.05 mg / L, respectively, and the removal rates were 87.71%~96.98% and 97.32%~100%, respectively. - -N and PO4 3- -P were measured by ion chromatography (881 Basic IC Plus, Metrohm, Switzerland).
[0107] Note: The treatment time of the bioretention system is the same as the length of the dry period, which mainly depends on whether the effluent concentration decreases after the next rainfall after the dry period. Example 7
[0108] The difference between Example 7 and Example 6 is only that:
[0109] Adding the prepared composite filler P6 to the novel composite filler mixed layer 4, wherein the novel composite filler layer 4 also includes quartz sand;
[0110] The volume ratio of P6 composite filler in the flooded area is 25%;
[0111] NO3 in P6-BS system when the dry period before rain is long - -N and PO4 3-The effluent concentrations of -P were 0.26~0.97 mg / L and 0~0.04 mg / L, respectively, and the removal rates were 89.81%~97.41% and 98.21%~100%, respectively. The simultaneous deep removal of nitrogen and phosphorus was achieved, and it can effectively cope with the impact of heavy rainfall, with good sustainability and broad application prospects. Example 8
[0112] This embodiment provides a method for preparing a denitrification and dephosphorization composite filler, comprising the following steps:
[0113] S1, placing polysulfone in N, N-dimethylformamide organic solvent and stirring to dissolve;
[0114] S2, add 3.33 g sawdust and 6.67 g pyrite to the polysulfone solution obtained in S1 and stir evenly, the total mass fraction of sawdust and pyrite in the solution is 10%;
[0115] Among them, the added amount of polysulfone is 16g, and the organic solvent of N, N-dimethylformamide is 74g;
[0116] The mass fraction of polysulfone in the solution obtained in step S2 is 16%;
[0117] S3. Drop the solution obtained in step S2 into excess deionized water at room temperature to form a ball at a rate of 60 drops per minute, and let it stand for 5 days.
[0118] S4, washing the obtained composite filler P7 with deionized water and drying it for later use. Example 9
[0119] The difference between Example 9 and Example 6 is that:
[0120] Adding the prepared composite filler P7 to the novel composite filler mixed layer 4, wherein the novel composite filler layer 4 also includes quartz sand;
[0121] The volume ratio of P7 composite filler in the flooded area is 25%;
[0122] The mass ratio of heterotrophic denitrification electron donors to autotrophic denitrification electron donors of composite filler P7 is about 1:2. The application scenario is when the pre-rain dry period is long ≥10 and the rainwater carbon-nitrogen ratio is >3;
[0123] NO3 in P7-BS system when the dry period before rain is long - -N and PO4 3- The effluent concentrations of -P were 0.48~1.47 mg / L and 0~0.01 mg / L, and the removal rates were 85.32%~95.23% and 99.51%~100%, respectively.
[0124] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0125] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A composite filler for denitrification and dephosphorization, characterized in that: The denitrification and dephosphorization composite filler has a spherical structure, a particle size of 3-5 mm, and a specific surface area of 2-4 m 2 / g, load-bearing ≥500 g; The denitrification and phosphorus removal composite filler is made of a polysulfone polymer as a skeleton and is prepared by an immersion precipitation phase conversion method and a mixed culture denitrification electron donor material; Wherein, the polysulfone polymer includes any one of polysulfone, polyethersulfone and polyarylsulfone; The mixed-culture denitrification electron donor material comprises at least one heterotrophic denitrification electron donor material and one autotrophic denitrification electron donor material; The electron donor of the heterotrophic denitrification includes a natural carbon source or an artificial carbon source; The electron donor of the autotrophic denitrification includes pyrite and / or pyrite; The preparation method of the denitrification and dephosphorization composite filler comprises: S1, placing a polysulfone polymer in an organic solvent and stirring to dissolve; S2, adding the solution obtained in S1 to the mixed culture denitrification electron donor material and stirring evenly; S3, dripping the solution obtained in S2 into a non-solvent to form a ball, with a dripping speed of 60 to 100 drops per minute, and letting it stand for more than 2 days; S4, washing and drying the composite material prepared in S3 for later use; Furthermore, the mass fraction of the polysulfone polymer in the solution obtained in step S2 is 5% to 20%.
2. The denitrification and dephosphorization composite filler according to claim 1, characterized in that: The mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is 1:3 to 3:1; The mass ratio of the polysulfone polymer to the mixed culture denitrification electron donor material is 1:2-4:
1.
3. The denitrification and dephosphorization composite filler according to claim 1, characterized in that: The organic solvent in step S1 is any one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone; The non-solvent includes water or ethanol.
4. The denitrification and dephosphorization composite filler according to claim 1, characterized in that: The mass fraction of the polyculture denitrification electron donor material in the solution obtained in step S2 is 5% to 10%.
5. The denitrification and dephosphorization composite filler according to claim 1, characterized in that: The solution obtained in step S2 is further added with a material having an adsorption property and / or a porogen; The adsorption material is selected as activated carbon; The porogen is selected from polyethylene glycol.
6. Application of the denitrification and dephosphorization composite filler as claimed in any one of claims 1 to 5 in sewage treatment systems, chemical production, biological research and artificial wetlands.
7. A bioretention system, characterized in that: include: The denitrification and phosphorus removal composite filler according to any one of claims 1 to 5, wherein the composite filler is arranged in the flooded area of the bioretention system; wherein the proportion of the polysulfone polymer and the mixed culture denitrification electron donor material in the composite filler is determined according to the rainwater runoff water quality and rainfall characteristics of the target area; When the carbon-nitrogen ratio of rainwater in the target area is ≤3, the mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is ≥1:1; When the carbon-nitrogen ratio of rainwater is greater than 3, the mass ratio of the heterotrophic denitrification electron donor to the autotrophic denitrification electron donor is less than 1:1; and / or, The target area has a drying period before rain of ≥10 days, then 12%≤the mass fraction of the polysulfone polymer≤20%, and 0.01 mL / g<the total pore volume of the composite filler≤0.02 mL / g; If the drying period before rain in the target area is less than 10 days, then 5%≤the mass fraction of the polysulfone polymer is less than 12%, and 0.02 mL / g<the total pore volume of the composite filler is less than 0.03 mL / g; The volume ratio of the composite filler to the flooded area is 20% to 100%; The composite filler is added alone or mixed with traditional fillers; the adding method is selected from mixed filling or layered filling.
Citation Information
Patent Citations
Solid slow-release carbon source for biological denitrification nitrogen removal and preparation method thereof
CN111252892A
Nitrogen and phosphorus removal unfired ceramsite as well as preparation method and application thereof
CN114315293A
Cited By
Sulfur-pyrite synergistic nitrogen and phosphorus removal composite filler as well as preparation method and application thereof
CN120271138A