An α-hemihydrate gypsum and its preparation method

By controlling the dissolution and crystal growth process of dihydrate phosphogypsum, short columnar high-strength α-hemihydrate gypsum was prepared, solving the problems of high energy consumption in phosphogypsum storage and preparation methods, and realizing the recycling of phosphorus resources and environmental protection.

CN118459130BActive Publication Date: 2026-11-10HUBEI UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410755648.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2026-11-10
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

In existing technologies, the storage of phosphogypsum leads to land occupation and environmental pollution. At the same time, existing methods for preparing α-hemihydrate gypsum are energy-intensive, have crystal morphologies that are not conducive to filtration, and have low strength, making them difficult to apply on a large scale.

Method used

By mixing dihydrate phosphogypsum with dilute phosphoric acid and concentrated sulfuric acid, dissolving it at low temperature, and adding a crystallization agent and hemihydrate phosphogypsum seed crystals, and controlling crystal growth at high temperature, short columnar α-hemihydrate gypsum is prepared. The process conditions are matched with the dihydrate process, and phosphorus resources are recycled.

Benefits of technology

The preparation of α-hemihydrate gypsum with low energy consumption and high strength has been achieved, solving the problem of phosphogypsum storage. It has environmental and economic advantages, wide applicability, and good crystal morphology control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118459130B_ABST
    Figure CN118459130B_ABST
Patent Text Reader

Abstract

This invention provides an α-hemihydrate gypsum and its preparation method. The method for preparing α-hemihydrate gypsum of this invention promotes the initial dissolution of dihydrate phosphogypsum in an acidic environment at a relatively low temperature (60–90°C), removing impurities such as organic matter adsorbed on the surface of the phosphogypsum. Then, the reaction temperature (95–110°C) and acidity are increased, and a crystal-transforming agent is added to promote the crystal-transforming reaction and effectively control the morphology. Furthermore, the process conditions of this method can be matched with existing dihydrate processes. By mixing the dihydrate phosphogypsum produced by the dihydrate process with phosphoric acid and adding a crystal-transforming agent, it is transformed into high-strength α-hemihydrate phosphogypsum crystals with a short columnar morphology. Simultaneously, residual phosphorus in the dihydrate phosphogypsum can be recovered, and the filtrate and washing water after crystal transformation can be recycled. This method has the advantages of low energy consumption, wide applicability, and low pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of α-hemihydrate gypsum preparation technology, and in particular to an α-hemihydrate gypsum and its preparation method. Background Technology

[0002] Phosphogypsum is a solid waste generated during the wet-process phosphoric acid production by decomposing phosphate rock with sulfuric acid. Its main component is calcium sulfate dihydrate. Currently, the dihydrate process is the mainstream wet-process phosphoric acid production technology both domestically and internationally. For every ton of phosphoric acid produced (calculated as phosphorus pentoxide), approximately 5 tons of phosphogypsum are generated. With the development of my country's phosphorus chemical industry over the past decades, the stockpiled phosphogypsum has exceeded 600 million tons, and is increasing at a rate of approximately 75 million tons per year. The large-scale open-air stockpiling of phosphogypsum not only occupies significant land resources, but also causes serious environmental problems due to the continuous release of acidic substances. Therefore, how to dispose of and utilize phosphogypsum at low cost on a large scale has become an urgent problem to be solved.

[0003] Alpha-hemihydrate gypsum is a high-performance and widely used building material. High-strength gypsum products made from it can also be used in ceramic molds, precision casting, and medical fields, making it an ideal direction for the resource utilization and high-value utilization of phosphogypsum. Currently, the main methods for preparing α-hemihydrate gypsum from dihydrate gypsum include autoclaving, hydrothermal methods, atmospheric pressure salt solution methods, and atmospheric pressure alcohol solution methods. However, while autoclaving, hydrothermal methods, and atmospheric pressure salt solution methods can yield high-strength α-hemihydrate gypsum, they cannot recover residual phosphorus from phosphogypsum and are energy-intensive, hindering large-scale applications. Furthermore, α-hemihydrate gypsum prepared by other conventional methods exhibits a needle-like morphology, which is unfavorable for filtration and results in lower strength.

[0004] The existing methods for preparing α-hemihydrate gypsum have shortcomings and need to be improved. Summary of the Invention

[0005] In view of this, the present invention provides an α-hemihydrate gypsum, its preparation method and application, to solve the problems existing in the prior art.

[0006] In a first aspect, the present invention provides a method for preparing α-hemihydrate gypsum, comprising the following steps:

[0007] A slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid, and then a crystallization reaction is carried out at 60–90 °C.

[0008] Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals are added to the product after the reaction, and the crystallization reaction is continued at 95-110℃. After the reaction is completed, the solid and liquid products are separated, and the solid product is collected to obtain α-hemihydrate gypsum.

[0009] Preferably, the mass concentration of the dilute phosphoric acid is 15-25%;

[0010] And / or, the concentrated sulfuric acid has a mass concentration of 96-98%.

[0011] Preferably, in the step of mixing phosphogypsum dihydrate, dilute phosphoric acid, and concentrated sulfuric acid to obtain a slurry, the mass ratio of phosphogypsum dihydrate, dilute phosphoric acid, and concentrated sulfuric acid is 1:(3-5):(0.1-0.4).

[0012] The mass ratio of concentrated sulfuric acid used in the step of mixing dihydrate phosphogypsum, dilute phosphoric acid and concentrated sulfuric acid to obtain a slurry is 1:(0.7~1.2).

[0013] Preferably, a slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid and concentrated sulfuric acid, and then reacting it at 20-100 rpm and 60-90°C for 0.5-3 hours.

[0014] Preferably, concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals are added to the product after the reaction, and the crystallization reaction is continued at 60-150 rpm and 95-110°C for 0.5-2 hours. After the reaction is completed, the product is separated into solid and liquid phases, and the solid product is collected to obtain α-hemihydrate gypsum.

[0015] Preferably, the crystal-transforming agent includes inorganic crystal-transforming agents and organic crystal-transforming agents;

[0016] The inorganic crystal-transforming agent includes those containing Al. 3+ Mg 2+ Fe 3+ At least one of the water-soluble inorganic salts;

[0017] The organic crystallization agent includes K + Na + NH4 + At least one of the organic acid salts;

[0018] And / or, the seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with a particle size of less than or equal to 10 μm.

[0019] Preferably, the amount of the inorganic crystallizing agent added is 0.05 to 1% of the mass of the slurry;

[0020] The amount of the organic crystallization agent added is 0.001 to 0.05% of the mass of the slurry;

[0021] The amount of hemihydrate phosphogypsum seed crystals added is 0.1 to 3% of the mass of dihydrate phosphogypsum.

[0022] Preferably, the water-soluble inorganic salt includes at least one of water-soluble nitrate and water-soluble sulfate;

[0023] The organic acid includes at least one of citric acid, carboxylic acid, lignin sulfonic acid, benzene sulfonic acid, and dodecylbenzene sulfonic acid.

[0024] Preferably, after the reaction is completed, the product is separated into solid and liquid phases. The solid product is washed with water at 80-90°C and then dried to obtain α-hemihydrate gypsum.

[0025] In the solid-liquid separation process, the filtrate is collected, the solid product is washed with water and the washing water is collected, and the filtrate and washing water are mixed to obtain a mixture.

[0026] Dihydrate phosphogypsum was mixed with a mixed liquid to obtain a slurry, and then a crystallization reaction was carried out at 60–90 °C.

[0027] Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals were added to the product after the reaction. The crystallization reaction was continued at 95-110℃. After the reaction was completed, the solid and liquid products were separated and the solid product was collected to obtain α-hemihydrate gypsum.

[0028] The mass ratio of the filtrate to the washing water is (8-12):1;

[0029] The mass ratio of the dihydrate phosphogypsum to the mixed liquid is 1:(3-4).

[0030] Secondly, the present invention also provides an α-hemihydrate gypsum, which is prepared by the preparation method described above.

[0031] The present invention has the following advantages over the prior art:

[0032] The preparation method of α-hemihydrate gypsum of the present invention, in the dissolution stage, involves mixing dihydrate phosphogypsum with phosphoric acid and concentrated sulfuric acid, and then carrying out a surface dissolution reaction of the dihydrate phosphogypsum at a relatively low temperature (60-90°C). This promotes the dissociation of surface impurities, increases the supersaturation of the solution, controls the precipitation of hemihydrate phosphogypsum crystals, reduces the nucleation rate of hemihydrate phosphogypsum crystals, and prevents the formation of excessive hemihydrate phosphogypsum crystal nuclei. In the crystallization stage, concentrated sulfuric acid, hemihydrate phosphogypsum seed crystals and a crystallization agent are added, and the temperature is increased (95-110°C) to promote the crystallization reaction and effectively control the morphology, ultimately promoting the growth of short columnar α-hemihydrate phosphogypsum crystals. Through this technical solution, it is possible to prevent... At the initial stage of the reaction, the organic crystallizing agent combines with impurities on the surface of dihydrate phosphogypsum, resulting in slow dissolution and poor morphology control of the dihydrate phosphogypsum. At the same time, it can also inhibit the generation of a large number of hemihydrate phosphogypsum crystal nuclei in the early stage and promote the growth of large-sized, short columnar α-hemihydrate phosphogypsum. In addition, the process conditions of this method can be matched with the existing dihydrate process. By mixing the dihydrate phosphogypsum produced by the dihydrate process with phosphoric acid and adding the crystallizing agent, it is transformed into high-strength α-hemihydrate phosphogypsum crystals with short columnar morphology. At the same time, it can recover and utilize residual phosphorus in dihydrate phosphogypsum and recycle the filtrate and washing water after crystallization. It has the advantages of low energy consumption, wide applicability and low pollution. Attached Figure Description

[0033] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0034] Figure 1 An optical microscope image of the α-hemihydrate gypsum prepared in Example 1;

[0035] Figure 2 An optical microscope image of the α-hemihydrate gypsum prepared in Example 2;

[0036] Figure 3 The XRD patterns of the raw material dihydrate phosphogypsum used in Example 1 and the α-hemihydrate gypsum crystals obtained in the final preparation are shown.

[0037] Figure 4 An optical microscope image of the α-hemihydrate gypsum prepared in Example 3;

[0038] Figure 5 An optical microscope photograph of the phosphogypsum crystals prepared in Comparative Example 1;

[0039] Figure 6The image shows the XRD pattern of the phosphogypsum crystals prepared in Comparative Example 1. Detailed Implementation

[0040] The technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0041] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single digits within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any referenced number (fraction or integer) within the indicated range.

[0042] This application provides a method for preparing α-hemihydrate gypsum, comprising the following steps:

[0043] S1. Mix phosphogypsum dihydrate, dilute phosphoric acid and concentrated sulfuric acid to obtain a slurry, and then perform a crystallization reaction at 60-90℃;

[0044] S2. Add concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals to the product after the reaction, and continue the crystallization reaction at 95-110℃. After the reaction is completed, separate the solid and liquid products and collect the solid product to obtain α-hemihydrate gypsum.

[0045] The basic principle of the preparation method of α-hemihydrate gypsum of the present invention is as follows: Since the transformation of dihydrate phosphogypsum into hemihydrate phosphogypsum is a microscopic process of dissolution and crystallization, it is controlled in stages. In the dissolution stage, dihydrate phosphogypsum is mixed with phosphoric acid and concentrated sulfuric acid, and the surface dissolution reaction of dihydrate phosphogypsum is carried out at a relatively low temperature (60-90°C) to promote the dissociation of surface impurities, increase the supersaturation of the solution, control the precipitation of hemihydrate phosphogypsum crystals, reduce the nucleation rate of hemihydrate phosphogypsum crystals, and prevent over-precipitation. A large number of hemihydrate phosphogypsum crystal nuclei are generated. During the crystallization stage, concentrated sulfuric acid, hemihydrate phosphogypsum seed crystals, and a crystal-transforming agent are added, and the temperature is increased (95-110℃) to promote the growth of short columnar α-hemihydrate phosphogypsum crystals. This technical solution can prevent the organic crystal-transforming agent from combining with impurities on the surface of dihydrate phosphogypsum in the initial stage of the reaction, which would otherwise cause slow dissolution of dihydrate phosphogypsum and poor morphology control. At the same time, it can also inhibit the generation of a large number of hemihydrate phosphogypsum crystal nuclei in the early stage and promote the growth of large-sized, short columnar α-hemihydrate phosphogypsum.

[0046] The method for preparing α-hemihydrate gypsum of the present invention promotes the initial dissolution of dihydrate phosphogypsum in an acidic environment at a relatively low temperature (60-90°C), which removes impurities such as organic matter adsorbed on the surface of the phosphogypsum. Then, the reaction temperature (95-110°C) and acidity are increased, and a crystal-transforming agent is added to promote the crystal-transforming reaction and effectively control the morphology. Furthermore, the process conditions of this method can be matched with existing dihydrate processes. By mixing the dihydrate phosphogypsum produced by the dihydrate process with phosphoric acid and adding a crystal-transforming agent, it is transformed into high-strength α-hemihydrate phosphogypsum crystals with a short columnar morphology. Simultaneously, residual phosphorus in the dihydrate phosphogypsum can be recovered, and the filtrate and washing water after crystal transformation can be recycled. This method has the advantages of low energy consumption, wide applicability, and low pollution.

[0047] In some embodiments, the mass concentration of dilute phosphoric acid is 15-25%.

[0048] In some embodiments, the mass concentration of concentrated sulfuric acid is 96-98%.

[0049] In some embodiments, in the step of mixing dihydrate phosphogypsum, dilute phosphoric acid and concentrated sulfuric acid to obtain a slurry, the mass ratio of dihydrate phosphogypsum, dilute phosphoric acid and concentrated sulfuric acid is 1:(3-5):(0.1-0.4).

[0050] In some embodiments, the mass ratio of concentrated sulfuric acid used in the step of mixing dihydrate phosphogypsum, dilute phosphoric acid and concentrated sulfuric acid to obtain a slurry to the mass ratio of concentrated sulfuric acid used in the step of adding concentrated sulfuric acid to the product after reaction is 1:(0.7 to 1.2).

[0051] In some embodiments, phosphogypsum dihydrate, dilute phosphoric acid, and concentrated sulfuric acid are mixed to obtain a slurry, which is then subjected to a crystallization reaction at 20–100 rpm and 60–90 °C for 0.5–3 h to carry out the initial dissolution process of phosphogypsum dihydrate, increase the supersaturation of the solution, and control the precipitation of phosphogypsum hemihydrate crystals.

[0052] In some embodiments, concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals are added to the product after the reaction, and the crystallization reaction is continued at 60-150 rpm and 95-110°C for 0.5-2 h. After the reaction is completed, the product is separated into solid and liquid phases, and the solid product is collected to obtain α-hemihydrate gypsum.

[0053] In some embodiments, the crystallization agent includes inorganic crystallization agents and organic crystallization agents.

[0054] In some embodiments, inorganic crystal-transforming agents include those containing Al 3+ Mg 2+ Fe 3+ At least one of the water-soluble inorganic salts;

[0055] In some embodiments, the organic transcrystallization agent includes K + Na + NH4 + At least one of the organic acid salts;

[0056] In some embodiments, the seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with a particle size of less than or equal to 10 μm.

[0057] In some embodiments, the amount of inorganic crystallizing agent added is 0.05 to 1% of the slurry mass.

[0058] In some embodiments, the amount of organic crystallizing agent added is 0.001 to 0.05% of the slurry mass.

[0059] In some embodiments, the amount of hemihydrate phosphogypsum seed crystals added is 0.1 to 3% of the mass of dihydrate phosphogypsum.

[0060] In some embodiments, the water-soluble inorganic salt includes at least one of water-soluble nitrates and water-soluble sulfates. Specifically, the inorganic crystallizing agent includes magnesium nitrate, aluminum nitrate, ferric nitrate, magnesium sulfate, aluminum sulfate, ferric sulfate, etc.

[0061] In some embodiments, the organic acid includes at least one of citric acid, carboxylic acid, lignin sulfonic acid, benzene sulfonic acid, and dodecylbenzene sulfonic acid. Specifically, the organic crystallizing agent includes ammonium citrate, potassium citrate, sodium citrate, sodium dodecylbenzene sulfonate, potassium dodecylbenzene sulfonate, sodium lignin sulfonate, potassium lignin sulfonate, etc.

[0062] In some embodiments, after the reaction is completed, the product is separated into solid and liquid phases. The solid product is washed with water at 80-90°C and then dried to obtain α-hemihydrate gypsum.

[0063] In the solid-liquid separation process, the filtrate is collected, the solid product is washed with water and the washing water is collected, and the filtrate and washing water are mixed to obtain a mixture.

[0064] Dihydrate phosphogypsum was mixed with a mixed liquid to obtain a slurry, and then a crystallization reaction was carried out at 60–90 °C.

[0065] Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals were added to the product after the reaction. The crystallization reaction was continued at 95-110℃. After the reaction was completed, the solid and liquid products were separated and the solid product was collected to obtain α-hemihydrate gypsum.

[0066] The mass ratio of filtrate to washing water is (8-12):1;

[0067] The mass ratio of dihydrate phosphogypsum to the mixed solution is 1:(3-4).

[0068] Specifically, in the above embodiments, the filtrate and washing water can be mixed and used to prepare slurry, and then used again to prepare α-hemihydrate gypsum, that is, the filtrate and washing water can be recycled; specifically, the amount of crystallizing agent used in the filtrate and washing water is about 0.25 times the amount used in the previous use.

[0069] Based on the same inventive concept, the present invention also provides an α-hemihydrate gypsum, which is prepared by the above-described preparation method.

[0070] The preparation method of α-hemihydrate gypsum according to this application is further illustrated below with specific embodiments. This section further illustrates the content of the present invention in conjunction with specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0071] Example 1

[0072] This embodiment provides a method for preparing α-hemihydrate gypsum, including the following steps:

[0073] S1. A slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid (mass concentration of 18%) and concentrated sulfuric acid (mass concentration of 98%), and then the slurry is subjected to a crystallization reaction at 40 rpm and 85°C for 2 hours to carry out the initial dissolution process of dihydrate phosphogypsum.

[0074] S2. Add concentrated sulfuric acid (98% by mass), crystal conversion agent and hemihydrate phosphogypsum seed crystals to the product after the reaction in S1, and continue the crystal conversion reaction at 100 rpm and 100 °C for 1.5 h.

[0075] After the reaction in steps S3 and S2 is completed, the reaction product is separated into solid and liquid. The solid product obtained by solid-liquid separation is washed with water at 85°C and then dried to obtain α-hemihydrate phosphogypsum. At the same time, the filtrate is collected during solid-liquid separation. The solid product is washed with water and the washing water is collected. The filtrate and washing water are mixed to obtain a mixture, which can be used to prepare slurry.

[0076] In step S1, the mass ratio of dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid is 1:4:0.25.

[0077] The mass ratio of concentrated sulfuric acid in step S1 to concentrated sulfuric acid in step S2 is 1:1;

[0078] In step S2, the crystallization agent includes aluminum sulfate and sodium dodecylbenzene sulfonate. The amount of aluminum sulfate added is 1% of the slurry mass, and the amount of sodium dodecylbenzene sulfonate added is 0.02% of the slurry mass.

[0079] The seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with an average particle size of 5 μm.

[0080] The amount of hemihydrate phosphogypsum seed crystals added is 1% of the mass of dihydrate phosphogypsum.

[0081] Example 2

[0082] This embodiment provides a method for preparing α-hemihydrate gypsum, including the following steps:

[0083] S1. A slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid (25% by mass) and concentrated sulfuric acid (98% by mass). The slurry is then subjected to a crystallization reaction at 60 rpm and 90°C for 1.5 h to carry out the initial dissolution process of dihydrate phosphogypsum.

[0084] S2. Add concentrated sulfuric acid (98% by mass), crystal conversion agent and hemihydrate phosphogypsum seed crystals to the product after the reaction in S1, and continue the crystal conversion reaction at 150 rpm and 110 °C for 1 h.

[0085] After the reaction in step S3 and S2 is completed, the reaction product is separated into solid and liquid. The solid product obtained by solid-liquid separation is washed with water at 85°C and then dried to obtain α-hemihydrate phosphogypsum.

[0086] In step S1, the mass ratio of dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid is 1:3.5:0.3.

[0087] The mass ratio of concentrated sulfuric acid in step S1 to concentrated sulfuric acid in step S2 is 1:1;

[0088] In step S2, the crystallizing agent includes ferric sulfate and sodium lignosulfonate. The amount of ferric sulfate added is 0.8% of the slurry mass, and the amount of sodium lignosulfonate added is 0.05% of the slurry mass.

[0089] The seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with an average particle size of 5 μm.

[0090] The amount of hemihydrate phosphogypsum seed crystals added is 1% of the mass of dihydrate phosphogypsum.

[0091] Example 3

[0092] This embodiment provides a method for preparing α-hemihydrate gypsum, including the following steps:

[0093] S1. Collect the filtrate and washing water according to the method in Example 1, and mix the filtrate and washing water at a mass ratio of 10:1 to obtain a mixture.

[0094] The slurry was prepared by mixing dihydrate phosphogypsum and the mixed liquid, and then the slurry was subjected to a crystallization reaction at 40 rpm and 85 ℃ for 2 hours to carry out the initial dissolution process of dihydrate phosphogypsum.

[0095] S2. Add concentrated sulfuric acid (98% by mass), crystal conversion agent and hemihydrate phosphogypsum seed crystals to the product after the reaction in S1, and continue the crystal conversion reaction at 100 rpm and 100 °C for 1.5 h.

[0096] After the reaction in step S3 and S2 is completed, the reaction product is separated into solid and liquid. The solid product obtained by solid-liquid separation is washed with water at 85°C and then dried to obtain α-hemihydrate phosphogypsum.

[0097] In step S1, the mass ratio of dihydrate phosphogypsum to the mixed solution is 1:3.8.

[0098] In step S2, the mass ratio of concentrated sulfuric acid to dihydrate phosphogypsum in step S1 is 0.2:1;

[0099] In step S2, the crystallization agent includes aluminum sulfate and sodium dodecylbenzene sulfonate. The amount of aluminum sulfate added is 0.25% of the slurry mass, and the amount of sodium dodecylbenzene sulfonate added is 0.005% of the slurry mass.

[0100] The seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with an average particle size of 5 μm.

[0101] The amount of hemihydrate phosphogypsum seed crystals added is 1% of the mass of dihydrate phosphogypsum.

[0102] Comparative Example 1

[0103] This comparative example provides a method for preparing α-hemihydrate gypsum, similar to Example 1, except that it does not involve a preliminary reaction at 85°C and all raw materials and crystal-changing agents are added at the initial stage of the reaction; instead, the crystal-changing reaction is carried out directly. Specifically, the preparation method of α-hemihydrate gypsum in Comparative Example 1 includes the following steps:

[0104] S1. Mix dihydrate phosphogypsum, dilute phosphoric acid (mass concentration of 25%) and concentrated sulfuric acid (mass concentration of 98%) to obtain a slurry, and add a crystallization agent and hemihydrate phosphogypsum seed crystals. The crystallization reaction is carried out at 150 rpm and 110℃ for 3 hours.

[0105] S2. After the reaction in step S1 is completed, the reaction product is separated into solid and liquid. The solid product obtained by solid-liquid separation is washed with water at 85°C and then dried.

[0106] In step S1, the mass ratio of dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid is 1:4:0.35.

[0107] In step S1, the crystallizing agent includes ferric sulfate and sodium lignosulfonate. The amount of ferric sulfate added is 0.8% of the slurry mass, and the amount of sodium lignosulfonate added is 0.05% of the slurry mass.

[0108] The seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with an average particle size of 5 μm.

[0109] The amount of hemihydrate phosphogypsum seed crystals added is 1% of the mass of dihydrate phosphogypsum.

[0110] Performance testing

[0111] Figures 1-2 The images shown are optical microscope photographs of the α-hemihydrate gypsum prepared in Examples 1 and 2, respectively.

[0112] from Figures 1-2 As can be seen, the prepared α-hemihydrate gypsum all have a short columnar morphology with an average aspect ratio of 1 to 2.

[0113] Figure 3 The XRD patterns are those of the raw material dihydrate phosphogypsum used in Example 1 and the final α-hemihydrate gypsum crystals obtained. Specifically, Figure 3 The original dihydrate phosphogypsum is the dihydrate phosphogypsum used in step S1 of Example 1, and the α-hemihydrate gypsum is the α-hemihydrate gypsum prepared in S3 of Example 1.

[0114] from Figure 3 As can be seen, the α-hemihydrate gypsum product has high purity, and no residual dihydrate phosphogypsum was observed.

[0115] Figure 4 This is an optical microscope image of the α-hemihydrate gypsum prepared in Example 3.

[0116] from Figure 4 As can be seen from the results, the morphology of the α-hemihydrate gypsum prepared in Example 3 is quite similar to that in Example 1, which demonstrates that the filtrate can still be recycled for crystallization.

[0117] Figure 5 An optical microscope image of the phosphogypsum crystals prepared in Comparative Example 1.

[0118] Figure 6 The image shows the XRD pattern of the phosphogypsum crystals prepared in Comparative Example 1. Specifically, Figure 6 The original dihydrate phosphogypsum is the dihydrate phosphogypsum used in step S1 of Comparative Example 1. Comparative Example 1 means the phosphogypsum crystals prepared in Comparative Example 1.

[0119] from Figure 5 As can be seen, after 1.5 hours of reaction, the crystals still exhibit the rhombic platy structure of phosphogypsum dihydrate. Figure 6 The XRD pattern also showed that the reaction product was still phosphogypsum dihydrate. This is because the phosphogypsum dihydrate in Comparative Example 1 had many impurities on its surface. After the crystallization agent was added, it was tightly bound to the surface, which inhibited the crystallization reaction.

[0120] The 2-hour flexural strength and oven compressive strength of the α-hemihydrate gypsum prepared in Examples 1 to 3 were tested according to GB / T17669.3-1999, and the results are shown in Table 1 below.

[0121] Table 1 - Mechanical strength test results of α-hemihydrate gypsum prepared in Examples 1-3

[0122] Example Flexural strength at 2 hours (MPa) Dry compressive strength (MPa) Example 1 4.4 35.6 Example 2 4.7 36.3 Example 3 4.6 32.2

[0123] As can be seen from Table 1, the 2-hour flexural strength and oven compressive strength of the α-hemihydrate gypsum prepared in Examples 1 to 3 both reached the α30 level in the JC / T 2038-2010 standard for α-type high-strength gypsum, indicating that they have high mechanical properties.

[0124] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing α-hemihydrate gypsum, characterized in that, Includes the following steps: A slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid, and then subjected to a crystallization reaction at 85-90℃ for 1.5-2 hours. Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals were added to the product after the reaction. The crystallization reaction was continued at 100~110℃ for 1~1.5h. After the reaction was completed, the solid and liquid products were separated and the solid product was collected to obtain α-hemihydrate gypsum. The mass concentration of the dilute phosphoric acid is 18-25%; The concentrated sulfuric acid has a mass concentration of 96-98%; In the step of mixing phosphogypsum dihydrate, dilute phosphoric acid, and concentrated sulfuric acid to obtain a slurry, the mass ratio of phosphogypsum dihydrate, dilute phosphoric acid, and concentrated sulfuric acid is 1:(3.5~4.0):(0.2.5~0.3). The mass ratio of concentrated sulfuric acid used in the step of mixing dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid to the mass ratio of concentrated sulfuric acid used in the step of adding concentrated sulfuric acid to the reaction product is 1:

1. The crystal-transforming agent includes inorganic crystal-transforming agents and organic crystal-transforming agents; The inorganic crystal-transforming agent includes aluminum sulfate or ferric sulfate; The organic crystallizing agent includes sodium dodecylbenzene sulfonate or sodium lignin sulfonate; The seed crystals of hemihydrate phosphogypsum are α-hemihydrate phosphogypsum crystals with a particle size of less than or equal to 10 μm. The amount of the inorganic crystal-transforming agent added is 0.8-1% of the mass of the slurry; The amount of the organic crystallizing agent added is 0.02~0.05% of the mass of the slurry; The amount of hemihydrate phosphogypsum seed crystals added is 1% of the mass of the dihydrate phosphogypsum.

2. The method for preparing α-hemihydrate gypsum as described in claim 1, characterized in that, A slurry is prepared by mixing dihydrate phosphogypsum, dilute phosphoric acid, and concentrated sulfuric acid, and then subjected to a crystallization reaction at 20-100 rpm and 85-90℃ for 1.5-2 hours.

3. The method for preparing α-hemihydrate gypsum as described in claim 1, characterized in that, Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals were added to the product after the reaction. The crystallization reaction was continued at 60-150 rpm and 100-110℃ for 1-1.5 h. After the reaction was completed, the solid and liquid products were separated and the solid product was collected to obtain α-hemihydrate gypsum.

4. The method for preparing α-hemihydrate gypsum according to any one of claims 1 to 3, characterized in that, After the reaction is complete, the product is separated into solid and liquid phases. The solid product is washed with water at 80-90℃ and then dried to obtain α-hemihydrate gypsum. In the solid-liquid separation process, the filtrate is collected, the solid product is washed with water and the washing water is collected, and the filtrate and washing water are mixed to obtain a mixture. Dihydrate phosphogypsum was mixed with a mixed liquid to obtain a slurry, which was then subjected to a crystallization reaction at 85-90℃. Concentrated sulfuric acid, a crystallization agent, and hemihydrate phosphogypsum seed crystals were added to the product after the reaction. The crystallization reaction was continued at 100~110℃. After the reaction was completed, the solid and liquid products were separated and the solid product was collected to obtain α-hemihydrate gypsum. The mass ratio of the filtrate to the washing water is (8~12):1; The mass ratio of the dihydrate phosphogypsum to the mixed solution is 1:(3~4).

5. An α-hemihydrate gypsum, characterized in that, It is prepared by any one of the preparation methods described in claims 1 to 4.

Citation Information

Patent Citations

  • Method for preparing alpha semi-hydrated gypsum from dihydrate gypsum

    CN105174760A

  • Method for preparing high-strength alpha semi-hydrated gypsum by using alpha semi-hydrated gypsum seed crystal

    CN117303427A