Halogen-free low expansion epoxy resin for copper clad laminate and preparation method thereof
By using halogen-free low-expanding epoxy resin formula in copper clad plate, combining silanization and physical copolymerization technology, and combining nanomaterials, the problem of insufficient high-temperature resistance of copper clad plate in the existing technology is solved, and higher thermal stability is achieved and safety performance.
Patent Information
- Application Number
- CN202410703822.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-06-03
AI Technical Summary
The existing environmentally friendly halogen-free flame-retardant epoxy resin for copper clad plates has poor high temperature resistance, large thermal gravity loss, and insufficient safety.
The halogen-free low-expanding epoxy resin formula, including epoxy resin, silane coupling agent KH550, silicone resin, composite filler, etc., is formed by silanization treatment and physical copolymerization, combining nanotitanium dioxide, nanosilicon dioxide and aluminum sol. High performance composite material.
It significantly improves the high temperature resistance and thermal weight loss temperature of copper clad plate, enhances the thermal stability and safety performance of the material, and reduces thermal weight loss loss.
Smart Images

Figure BDA0004871825640000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper clad laminates, and more specifically to a halogen-free low-expansion epoxy resin for copper clad laminates and a preparation method thereof. Background Art
[0002] Copper clad laminate generally refers to copper foil laminate, which is a plate material made by impregnating electronic fiberglass cloth or other reinforcing materials with resin, covering one or both sides with copper foil and hot pressing. It is referred to as copper clad laminate for short. According to the insulating resin used in copper clad laminate, a certain resin is called a certain resin copper clad laminate, such as epoxy resin copper clad laminate, polyester resin copper clad laminate and cyanate resin copper clad laminate, etc.
[0003] The patent (CN105237950B) discloses an environmentally friendly halogen-free flame-retardant epoxy resin for copper-clad laminates, which is prepared from the following components: bisphenol F epoxy resin, bisphenol A epoxy resin, polyoxypropylene diamine, ammonium copper phosphate, talcum powder, bentonite, dioctyltin, sodium dodecyl sulfonate, zinc borate, lignin and coupling agent. The present invention also discloses a method for preparing the environmentally friendly halogen-free flame-retardant epoxy resin for copper-clad laminates. The environmentally friendly halogen-free flame-retardant epoxy resin for copper-clad laminates prepared by the present invention not only has good flame retardancy, but also has better peel strength, lower dielectric loss and thermal expansion coefficient, and is very suitable for processing and manufacturing copper-clad laminates; in addition, the raw materials used in the preparation process are easily available and the preparation process is simple, which is also convenient for promotion and application.
[0004] The above copper clad laminate uses environmentally friendly halogen-free flame-retardant epoxy resin, which has poor high temperature resistance, large thermogravimetric loss, and poor safety of the copper clad laminate. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, an embodiment of the present invention provides a halogen-free low expansion epoxy resin for copper clad laminates and a preparation method thereof.
[0006] A halogen-free low-expansion epoxy resin for copper-clad laminates comprises raw materials calculated by weight percentage: 28-32% of epoxy resin, 2.5-3.5% of silane coupling agent KH550, 2.1-2.9% of curing agent, 18-22% of silicone resin, 11-13% of composite filler, and the rest is organic solvent.
[0007] Furthermore, the raw materials of the composite filler include, by weight percentage, 8.5-9.5% of nano titanium dioxide, 8.5-9.5% of nano silicon dioxide, 9.6-10.6% of aluminum sol, 3.5-4.5% of silane coupling agent KH550, 3.7-4.7% of 4,4′-diaminodiphenyl ether, 4.5-5.5% of pyromellitic anhydride, and the rest is an organic solvent.
[0008] Furthermore, the curing agent is one of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, and diethylaminopropylamine; and the organic solvent is one of butyl acetate, N,N-dimethylacetamide, methyl acetate, and ethyl acetate.
[0009] Furthermore, the raw materials of a halogen-free low-expansion epoxy resin for copper-clad laminates include, by weight percentage, 29-31% of epoxy resin, 2.8-3.2% of silane coupling agent KH550, 2.3-2.7% of curing agent, 19-21% of silicone resin, 11.5-12.5% of composite filler, and the rest is organic solvent; the raw materials of the composite filler include, by weight percentage, 8.8-9.2% of nano titanium dioxide, 8.8-9.2% of nano silicon dioxide, 9.9-10.3% of aluminum sol, 3.8-4.2% of silane coupling agent KH550, 3.9-4.5% of 4,4′-diaminodiphenyl ether, 4.8-5.2% of pyromellitic anhydride, and the rest is organic solvent.
[0010] Furthermore, the raw materials of a halogen-free low-expansion epoxy resin for copper-clad laminates include, by weight percentage, 30% of epoxy resin, 3.0% of silane coupling agent KH550, 2.5% of curing agent, 20% of silicone resin, 12% of composite filler, and the rest is an organic solvent; the raw materials of the composite filler include, by weight percentage, 9.0% of nano titanium dioxide, 9.0% of nano silicon dioxide, 10.1% of aluminum sol, 4.0% of silane coupling agent KH550, 4.2% of 4,4′-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is an organic solvent.
[0011] A method for preparing a halogen-free low expansion epoxy resin for a copper clad laminate, the specific preparation steps are as follows:
[0012] Step 1: weighing epoxy resin, silane coupling agent KH550, curing agent, silicone resin, organic solvent in the raw materials and nano titanium dioxide, nano silicon dioxide, silane coupling agent KH550, 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride, organic solvent and aluminum sol in the composite filler;
[0013] Step 2: adding 4,4′-diaminodiphenyl ether to the organic solvent of the composite filler, magnetically stirring for 10 to 20 minutes, then adding pyromellitic dianhydride, ultrasonically treating for 10 to 20 minutes, and then magnetically stirring for 4 to 6 hours to obtain material A;
[0014] Step 3: adding the silane coupling agent KH550 and aluminum sol in the composite filler to the material A in step 2, magnetically stirring for 4 to 6 hours, and then adding nano titanium dioxide and nano silicon dioxide for ultrasonic treatment for 40 to 60 minutes to obtain a composite filler;
[0015] Step 4: Add the epoxy resin in step 1 to an organic solvent and treat it in a constant temperature water bath for 20 to 40 minutes, then add the silane coupling agent KH550, and then stir it in a constant temperature water bath for 2 to 4 hours to obtain material B;
[0016] Step 5: Blend the silicone resin, curing agent, the composite filler in step 3 and material B in step 4, and stir for 50 to 70 minutes to obtain a halogen-free low expansion epoxy resin for copper clad laminates.
[0017] Furthermore, in step 2, the magnetic stirring speed is 800-1000 r / min, the ultrasonic frequency is 1.3-1.5 MHz, and the ultrasonic power is 400-500 W; in step 3, the magnetic stirring speed is 800-1000 r / min, the ultrasonic frequency is 1.3-1.5 MHz, and the ultrasonic power is 400-500 W; in step 4, the constant temperature water bath temperature is 38-42° C., and the stirring speed is 800-1000 r / min; in step 5, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 800-1000 r / min, the stirring speed in the second stage is 500-700 r / min, and the stirring speed in the third stage is 200-400 r / min.
[0018] Furthermore, in step 2, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 3, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 4, the constant temperature water bath temperature is 40°C, and the stirring speed is 900 r / min; in step 5, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 900 r / min, the stirring speed in the second stage is 600 r / min, and the stirring speed in the third stage is 300 r / min.
[0019] Furthermore, the preparation steps of the aluminum sol are: adding aluminum isopropoxide to deionized water, ultrasonically treating in a water bath until the pH value no longer changes, adding nitric acid solution to adjust the pH to 1.8-2.2, and reflux reaction in a water bath for 1-2 hours to obtain aluminum sol.
[0020] Furthermore, the weight ratio of the aluminum isopropoxide to deionized water is 1:30-40, the concentration of the nitric acid solution is 1.5-2.5 mol / L, and the water bath temperature is 55-65°C.
[0021] Technical effects and advantages of the present invention:
[0022] 1. A halogen-free low-expansion epoxy resin for copper-clad laminate prepared by the raw material formula of the present invention can effectively improve the high temperature resistance of the prepreg in the copper-clad laminate when used in the copper-clad laminate, can effectively ensure the flame retardant performance of the prepreg in the copper-clad laminate, can effectively increase the thermal weight loss temperature of the prepreg in the copper-clad laminate, and has a smaller thermal weight loss loss under the same temperature conditions, which can effectively improve the safety performance of the copper-clad laminate; the silane coupling agent KH550 can perform silanization treatment on the epoxy resin, and the silane coupling agent KH550 undergoes a polycondensation reaction with the epoxy resin. The silanized epoxy resin is generated, and then the epoxy resin is modified by physical copolymerization of the silicone resin and the silanized epoxy resin, which can effectively improve the heat resistance, adhesion and corrosion resistance of the epoxy resin; the composite filler is added to the epoxy resin for supplementary treatment, which can further improve the heat resistance and thermal weight loss temperature of the epoxy resin material; the 4,4'-diaminodiphenyl ether in the composite filler is a diamine monomer, the pyromellitic dianhydride is an acid anhydride monomer, and the silane coupling agent KH550 is a coupling agent. The diamine and acid anhydride monomers are polymerized to form polyamic acid The solution is dehydrated and cyclized to form polyimide. The aluminum isopropoxide in the aluminum sol is the aluminum source. After heat treatment, the aluminum sol finally exists in the form of AlO(OH). The aluminum isopropoxide gradually forms a macromolecular chain similar to an organic polymer during the hydrolysis process. There are a large number of hydroxyl groups (-OH) on its surface. -OH can react with the silane coupling agent KH550 to form a Si-O-Al bond. The amino group (-NH2) at the other end can form a hydrogen bond with the macromolecular polyamic acid. The intermolecular hydrogen bond can improve the thermal stability of the material. When added to the epoxy resin, the thermal stability and heat resistance of the epoxy resin material can be effectively improved. The nano-titanium dioxide and nano-silicon dioxide in the composite filler are combined and added to the epoxy resin material to further improve the heat resistance of the epoxy resin material. The particles of nano-titanium dioxide are much smaller than those of ordinary titanium dioxide and have better thermal stability. The microstructure of nano-silicon dioxide is spherical and the branched structure is a three-dimensional chain structure. It can form a spatial network structure with the polymer compound, which can greatly improve the mechanical properties, heat resistance and corrosion resistance of the composite material.
[0023] 2. The present invention polymerizes 4,4′-diaminodiphenyl ether and pyromellitic acid anhydride in an organic solvent to form a polyamic acid solution; blends the polyamic acid solution with silane coupling agent KH550 and aluminum sol, which can effectively ensure that the polyamic acid solution continues to react; the aluminum sol is hydrolyzed and compounded inside the polyimide, which can effectively enhance the polymerization contact blending effect of AlO(OH) and polyimide; and nano-titanium dioxide and nano-silicon dioxide are ultrasonically blended in the composite filler, which can effectively enhance the polymerization of nano-titanium dioxide and nano-silicon dioxide. The dispersion uniformity and stability inside the composite filler can improve the distribution uniformity of nano-titanium dioxide and nano-silicon dioxide in the epoxy resin material; the epoxy resin is reacted with the silane coupling agent KH550 in an organic solvent to effectively ensure the silanization treatment of the epoxy resin and the subsequent copolymerization and bonding effect of the silanized epoxy resin and the silicone resin; the silicone resin, the curing agent, the composite filler and the material B are blended and stirred to effectively ensure the rapid blending reaction of the above raw materials to obtain a halogen-free low-expansion epoxy resin for copper clad laminates. DETAILED DESCRIPTION
[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Embodiment 1:
[0026] The invention provides a halogen-free low-expansion epoxy resin for copper-clad laminates. The raw materials include, by weight percentage, 28% of epoxy resin, 2.5% of silane coupling agent KH550, 2.1% of triethylenetetramine, 18% of organic silicon resin, 11% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 8.5% of nano titanium dioxide, 8.5% of nano silicon dioxide, 9.6% of aluminum sol, 3.5% of silane coupling agent KH550, 3.7% of 4,4′-diaminodiphenyl ether, 4.5% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide;
[0027] Epoxy resin was purchased from Jinan Yuanxiang Chemical Co., Ltd., item number: 38891-59-7; 4,4′-diaminodiphenyl ether was purchased from Shanghai Qiam Analytical Technology Co., Ltd., CAS number: 139-65-1, item number: C10215500; silane coupling agent KH550 was purchased from Shanghai Huicheng Biotechnology Co., Ltd., item number: RB1032; triethylenetetramine was purchased from Jinan Huifengda Chemical Co., Ltd., item number: HFD-049; silicone resin was purchased from Hubei Xinsihai Chemical Co., Ltd., item number: SH-1053; Butyl acetate was purchased from Shandong Yanshuo Chemical Co., Ltd., item number: YS022; nano titanium dioxide was purchased from Hubei Weideli Chemical Technology Co., Ltd., item number: HBWS-1339; nano silicon dioxide was purchased from Hubei Dahao Chemical Co., Ltd., item number: DH11375; aluminum isopropoxide was purchased from Wuhan Prov Biotechnology Co., Ltd., item number: 0002; pyromellitic dianhydride was purchased from Tianjin Zhongtai Materials Technology Co., Ltd., item number: 064; N,N-dimethylacetamide was purchased from Hubei Xinkang Pharmaceutical Chemical Co., Ltd., item number: xk78;
[0028] The present invention also provides a method for preparing a halogen-free low expansion epoxy resin for a copper clad laminate, and the specific preparation steps are as follows:
[0029] Step 1: weigh epoxy resin, silane coupling agent KH550, triethylenetetramine, silicone resin, butyl acetate in the raw materials and nano titanium dioxide, nano silicon dioxide, silane coupling agent KH550, 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride, N,N-dimethylacetamide and aluminum sol in the composite filler;
[0030] Step 2: Add 4,4′-diaminodiphenyl ether to N,N-dimethylacetamide, stir magnetically for 15 minutes, then add pyromellitic anhydride, perform ultrasonic treatment for 15 minutes, and then stir magnetically for 5 hours to obtain material A;
[0031] Step 3: adding the silane coupling agent KH550 and aluminum sol in the composite filler to the material A in step 2, magnetically stirring for 5 hours, and then adding nano titanium dioxide and nano silicon dioxide for ultrasonic treatment for 50 minutes to obtain a composite filler;
[0032] Step 4: adding the epoxy resin in step 1 to butyl acetate and treating in a constant temperature water bath for 30 minutes, then adding silane coupling agent KH550, and then stirring in a constant temperature water bath for 3 hours to obtain material B;
[0033] Step 5: Blend the silicone resin, triethylenetetramine, the composite filler in step 3 and the material B in step 4, and stir for 60 minutes to obtain a halogen-free low expansion epoxy resin for copper clad laminates.
[0034] In step 2, the magnetic stirring speed is 800 r / min, the ultrasonic frequency is 1.3 MHz, and the ultrasonic power is 400 W; in step 3, the magnetic stirring speed is 800 r / min, the ultrasonic frequency is 1.3 MHz, and the ultrasonic power is 400 W; in step 4, the constant temperature water bath temperature is 38° C., and the stirring speed is 800 r / min; in step 5, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 800 r / min, the stirring speed in the second stage is 500 r / min, and the stirring speed in the third stage is 200 r / min;
[0035] The preparation steps of the aluminum sol are as follows: adding aluminum isopropoxide to deionized water, performing water bath ultrasonic treatment until the pH value no longer changes, adding nitric acid solution to adjust the pH to 2.0, and performing reflux reaction treatment in a water bath for 1.5 hours to obtain the aluminum sol;
[0036] The weight ratio of the aluminum isopropoxide to deionized water is 1:30, the concentration of the nitric acid solution is 1.5 mol / L, and the water bath temperature is 55°C.
[0037] Embodiment 2:
[0038] Different from Example 1, the raw materials of the halogen-free low-expansion epoxy resin for the copper clad laminate include, by weight percentage, 32% of epoxy resin, 3.5% of silane coupling agent KH550, 2.9% of triethylenetetramine, 22% of silicone resin, 13% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 9.5% of nano titanium dioxide, 9.5% of nano silicon dioxide, 10.6% of aluminum sol, 4.5% of silane coupling agent KH550, 4.7% of 4,4′-diaminodiphenyl ether, 5.5% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide.
[0039] Embodiment 3:
[0040] Different from Examples 1-2, the raw materials of the halogen-free low-expansion epoxy resin for the copper clad laminate include, by weight percentage, 30% of epoxy resin, 3.0% of silane coupling agent KH550, 2.5% of triethylenetetramine, 20% of silicone resin, 12% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 9.0% of nano-titanium dioxide, 9.0% of nano-silicon dioxide, 10.1% of aluminum sol, 4.0% of silane coupling agent KH550, 4.2% of 4,4′-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide.
[0041] Embodiment 4:
[0042] Different from Example 3, in step 2, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 3, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 4, the constant temperature water bath temperature is 40°C, and the stirring speed is 900 r / min; in step 5, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 900 r / min, the stirring speed in the second stage is 600 r / min, and the stirring speed in the third stage is 300 r / min; the weight ratio of the aluminum isopropoxide to deionized water is 1:35, the concentration of the nitric acid solution is 2.0 mol / L, and the water bath temperature is 60°C.
[0043] Comparative Example 1:
[0044] The difference from Example 4 is that the raw materials of the halogen-free low-expansion epoxy resin for the copper clad laminate include, by weight percentage, 30% of epoxy resin, 2.5% of triethylenetetramine, 20% of silicone resin, 12% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 9.0% of nano-titanium dioxide, 9.0% of nano-silicon dioxide, 10.1% of aluminum sol, 4.0% of silane coupling agent KH550, 4.2% of 4,4′-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide.
[0045] Comparative Example 2:
[0046] The difference from Example 4 is that the raw materials of the halogen-free low-expansion epoxy resin for the copper clad laminate include, by weight percentage, 30% of epoxy resin, 3.0% of silane coupling agent KH550, 2.5% of triethylenetetramine, 20% of silicone resin, 12% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 9.0% of nano-silica, 10.1% of aluminum sol, 4.0% of silane coupling agent KH550, 4.2% of 4,4′-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide.
[0047] Comparative Example 3:
[0048] The difference from Example 4 is that the raw materials of the halogen-free low-expansion epoxy resin for copper-clad laminates include, by weight percentage, 30% of epoxy resin, 3.0% of silane coupling agent KH550, 2.5% of triethylenetetramine, 20% of silicone resin, 12% of composite filler, and the rest is butyl acetate; the raw materials of the composite filler include, by weight percentage, 9.0% of nano titanium dioxide, 9.0% of nano silicon dioxide, 4.0% of silane coupling agent KH550, 4.2% of 4,4′-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is N,N-dimethylacetamide.
[0049] Comparative Example 4:
[0050] The difference from Example 3 is: a method for preparing a halogen-free low expansion epoxy resin for a copper clad laminate, and the specific preparation steps are as follows:
[0051] Step 1: weigh epoxy resin, silane coupling agent KH550, triethylenetetramine, silicone resin, butyl acetate in the raw materials and nano titanium dioxide, nano silicon dioxide, silane coupling agent KH550, 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride, N,N-dimethylacetamide and aluminum sol in the composite filler;
[0052] Step 2: Add 4,4′-diaminodiphenyl ether to N,N-dimethylacetamide, and stir the mixture under magnetic stirring for 15 minutes. Then, add pyromellitic anhydride, silane coupling agent KH550 and aluminum sol, and perform ultrasonic treatment for 15 minutes. Then, stir the mixture under magnetic stirring for 5 hours to obtain a composite filler.
[0053] Step 3: adding the epoxy resin in step 1 to butyl acetate and treating it in a constant temperature water bath for 30 minutes, then adding silane coupling agent KH550, silicone resin, triethylenetetramine, and the composite filler in step 2 for blending, stirring for 60 minutes, and obtaining a halogen-free low expansion epoxy resin for copper clad laminate;
[0054] In step two, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step three, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 900 r / min, the stirring speed in the second stage is 600 r / min, and the stirring speed in the third stage is 300 r / min.
[0055] The halogen-free low expansion epoxy resin for copper clad laminate in the comparative example and the embodiment of the present invention was tested and treated, and the electronic glass fiber cloth was immersed in the halogen-free low expansion epoxy resin for copper clad laminate in the comparative example and the embodiment for 30 minutes, respectively, and cured at a temperature of 180°C for 6 hours, and cooled to room temperature after curing to obtain a prepreg; the prepreg was subjected to thermal expansion coefficient, flame retardancy, and temperature resistance thermogravimetric testing; thermal expansion coefficient: TMA method; flame retardancy: UL94 flame retardancy grade test; temperature resistance thermogravimetric test: a thermogravimetric analyzer was used to measure the mass change process of the sample with temperature when heated, the sample mass was 5-10 mg, the test temperature was 30-800°C, the heating rate was 20°C / min, the gas flow rate was 100 mL / min, the test atmosphere was nitrogen, and the temperature at which the prepreg was thermally decomposed by 5% was detected; the test results are shown in Table 1:
[0056] Table 1:
[0057]
[0058] It can be seen from the above table that when the halogen-free low expansion epoxy resin for copper clad laminate of the present invention is used in the copper clad laminate, the high temperature resistance of the prepreg in the copper clad laminate can be effectively improved, the flame retardant performance of the prepreg in the copper clad laminate can be effectively guaranteed, the thermal weight loss temperature of the prepreg in the copper clad laminate can be effectively increased, the thermal weight loss loss is smaller under the same temperature conditions, and the safety performance of the copper clad laminate can be effectively improved.
[0059] The silane coupling agent KH550 in the present invention can be used to perform silanization treatment on epoxy resin. The silane coupling agent KH550 and epoxy resin undergo polycondensation reaction to generate silanized epoxy resin. Then, the epoxy resin is modified by physical copolymerization of organic silicone resin and silanized epoxy resin, which can effectively improve the heat resistance, adhesion and corrosion resistance of epoxy resin. The composite filler is added to the epoxy resin for supplementary treatment, which can further improve the heat resistance and thermal weight loss temperature of the epoxy resin material. The 4,4′-diaminodiphenyl ether in the composite filler is a diamine monomer, the pyromellitic anhydride is an acid anhydride monomer, the silane coupling agent KH550 is a coupling agent, the diamine and the acid anhydride monomers are polymerized to form a polyamic acid solution, and the polyamic acid solution is formed through dehydration and cyclization. Imine, aluminum isopropoxide in aluminum sol is the aluminum source. After heat treatment, aluminum sol finally exists in the form of AlO(OH). Aluminum isopropoxide gradually forms a macromolecular chain similar to organic polymers during the hydrolysis process. There are a large number of hydroxyl groups (-OH) on its surface. -OH can react with silane coupling agent KH550 to form Si-O-Al bonds. The amino group (-NH2) at the other end can form hydrogen bonds with macromolecular polyamic acid. The intermolecular hydrogen bonds can improve the thermal stability of the material. When added to epoxy resin, it can effectively improve the thermal stability and heat resistance of epoxy resin materials. The combination of nano titanium dioxide and nano silicon dioxide in the composite filler can be added to epoxy resin materials to further improve the heat resistance of epoxy resin materials. Titanium oxide particles are much smaller than ordinary titanium dioxide and have better thermal stability, while the microstructure of nano-silicon dioxide is spherical and the branch structure is a three-dimensional chain structure, which can form a spatial network structure together with the polymer compound, and can greatly improve the mechanical properties, temperature resistance and corrosion resistance of the composite material; in step 2, 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride are polymerized in an organic solvent to form a polyamic acid solution; in step 3, silane coupling agent KH550 and aluminum sol are blended with the polyamic acid solution, which can effectively ensure that the polyamic acid solution continues to react, and the aluminum sol is hydrolyzed and compounded inside the polyimide, which can effectively strengthen the polymerization contact blending of AlO(OH) and polyimide Treatment effect: ultrasonically blending nano titanium dioxide and nano silicon dioxide in the composite filler can effectively enhance the dispersion uniformity and stability of nano titanium dioxide and nano silicon dioxide in the composite filler, thereby improving the distribution uniformity of nano titanium dioxide and nano silicon dioxide in the epoxy resin material; in step 4, reacting the epoxy resin with the silane coupling agent KH550 in an organic solvent can effectively ensure the silanization treatment of the epoxy resin and ensure the subsequent copolymerization and bonding effect of the silanized epoxy resin and the silicone resin; in step 5, the silicone resin, the curing agent, the composite filler, and the material B are blended and stirred, which can effectively ensure the rapid blending reaction treatment of the above raw materials to obtain a halogen-free low-expansion epoxy resin for copper clad laminates.
[0060] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A halogen-free low expansion epoxy resin for copper clad laminates, Features: The raw materials include, by weight percentage, 28-32% of epoxy resin, 2.5-3.5% of silane coupling agent KH550, 2.1-2.9% of curing agent, 18-22% of silicone resin, 11-13% of composite filler, and the rest is organic solvent; the raw materials of the composite filler include, by weight percentage, 8.5-9.5% of nano titanium dioxide, 8.5-9.5% of nano silicon dioxide, 9.6-10.6% of aluminum sol, 3.5-4.5% of silane coupling agent KH550, 3.7-4.7% of 4,4'-diaminodiphenyl ether, 4.5-5.5% of pyromellitic anhydride, and the rest is organic solvent; the curing agent is one of ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, and diethylaminopropylamine.
2. The halogen-free low expansion epoxy resin for copper clad laminate according to claim 1, Features: The organic solvent is one of butyl acetate, N,N-dimethylacetamide, methyl acetate and ethyl acetate.
3. The halogen-free low expansion epoxy resin for copper clad laminate according to claim 1, Features: The raw materials include, by weight percentage, 29-31% of epoxy resin, 2.8-3.2% of silane coupling agent KH550, 2.3-2.7% of curing agent, 19-21% of silicone resin, 11.5-12.5% of composite filler, and the rest is organic solvent; the raw materials of the composite filler include, by weight percentage, 8.8-9.2% of nano titanium dioxide, 8.8-9.2% of nano silicon dioxide, 9.9-10.3% of aluminum sol, 3.8-4.2% of silane coupling agent KH550, 3.9-4.5% of 4,4'-diaminodiphenyl ether, 4.8-5.2% of pyromellitic anhydride, and the rest is organic solvent.
4. The halogen-free low expansion epoxy resin for copper clad laminate according to claim 1, Features: The raw materials include, by weight percentage, 30% of epoxy resin, 3.0% of silane coupling agent KH550, 2.5% of curing agent, 20% of silicone resin, 12% of composite filler, and the rest is organic solvent; the raw materials of the composite filler include, by weight percentage, 9.0% of nano titanium dioxide, 9.0% of nano silicon dioxide, 10.1% of aluminum sol, 4.0% of silane coupling agent KH550, 4.2% of 4,4'-diaminodiphenyl ether, 5.0% of pyromellitic anhydride, and the rest is organic solvent.
5. The method for preparing a halogen-free low expansion epoxy resin for copper clad laminate according to claim 1, Features: The specific preparation steps are as follows: Step 1: weighing epoxy resin, silane coupling agent KH550, curing agent, silicone resin, organic solvent in the raw materials and nano titanium dioxide, nano silicon dioxide, silane coupling agent KH550, 4,4'-diaminodiphenyl ether, pyromellitic acid dianhydride, organic solvent and aluminum sol in the composite filler; Step 2: adding 4,4′-diaminodiphenyl ether to the organic solvent of the composite filler, magnetically stirring for 10 to 20 minutes, then adding pyromellitic dianhydride, ultrasonically treating for 10 to 20 minutes, and then magnetically stirring for 4 to 6 hours to obtain material A; Step 3: adding the silane coupling agent KH550 and aluminum sol in the composite filler to the material A in step 2, magnetically stirring for 4 to 6 hours, and then adding nano titanium dioxide and nano silicon dioxide for ultrasonic treatment for 40 to 60 minutes to obtain a composite filler; Step 4: Add the epoxy resin in step 1 to an organic solvent and treat it in a constant temperature water bath for 20 to 40 minutes, then add the silane coupling agent KH550, and then stir it in a constant temperature water bath for 2 to 4 hours to obtain material B; Step 5: Blend the silicone resin, curing agent, the composite filler in step 3 and material B in step 4, and stir for 50 to 70 minutes to obtain a halogen-free low expansion epoxy resin for copper clad laminates.
6. A method for preparing a halogen-free low expansion epoxy resin for copper clad laminate according to claim 5, Features: In step 2, the magnetic stirring speed is 800-1000 r / min, the ultrasonic frequency is 1.3-1.5 MHz, and the ultrasonic power is 400-500 W; in step 3, the magnetic stirring speed is 800-1000 r / min, the ultrasonic frequency is 1.3-1.5 MHz, and the ultrasonic power is 400-500 W; in step 4, the constant temperature water bath temperature is 38-42° C., and the stirring speed is 800-1000 r / min; in step 5, the stirring process is divided into three stages, and the time of each stage is the same, the stirring speed of the first stage is 800-1000 r / min, the stirring speed of the second stage is 500-700 r / min, and the stirring speed of the third stage is 200-400 r / min.
7. A method for preparing a halogen-free low expansion epoxy resin for copper clad laminate according to claim 6, Features: In step 2, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 3, the magnetic stirring speed is 900 r / min, the ultrasonic frequency is 1.4 MHz, and the ultrasonic power is 450 W; in step 4, the constant temperature water bath temperature is 40°C, and the stirring speed is 900 r / min; in step 5, the stirring process is divided into three stages, each stage has the same time, the stirring speed in the first stage is 900 r / min, the stirring speed in the second stage is 600 r / min, and the stirring speed in the third stage is 300 r / min.
8. The method for preparing a halogen-free low expansion epoxy resin for copper clad laminate according to claim 5, Features: The preparation steps of the aluminum sol are as follows: adding aluminum isopropoxide to deionized water, performing water bath ultrasonic treatment until the pH value no longer changes, adding nitric acid solution to adjust the pH to 1.8-2.2, and performing reflux reaction treatment in a water bath for 1-2 hours to obtain the aluminum sol.
9. The method for preparing a halogen-free low expansion epoxy resin for copper clad laminate according to claim 8, Features: The weight ratio of the aluminum isopropoxide to deionized water is 1:30-40, the concentration of the nitric acid solution is 1.5-2.5 mol / L, and the water bath temperature is 55-65°C.