A polylactic acid-polyhydroxyalkanoate-based degradable composite material and preparation method thereof
By combining the ternary flame retardant with lignin and graft polymerization with vegetable oil, the problem of insufficient heat resistance and toughness of the polylactic acid material is solved, its flame retardant performance and compatibility are improved, the production cost is reduced, and the Improve the comprehensive performance of polylactic acid-polyhydroxyalkanoate based degradable composite materials.
Patent Information
- Application Number
- CN202410911580.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Polylactic acid materials have poor heat resistance, insufficient toughness, and poor compatibility after blending with polyhydroxyalkanoate, resulting in reduced mechanical properties, increased production costs, and limiting its application.
The ternary flame retardant is combined with lignin to form a composite material, and is grafted and polymerized with vegetable oil to improve the mechanical properties and compatibility of polylactic acid and reduce production costs. A twin-screw extruder is used for melt blending to prepare polylactic acid. -Polyhydroxyalkanoate based degradable composite material.
It improves the flame retardant performance, toughness, UV resistance and mechanical properties of polylactic acid, reduces production costs, expands the scope of application, and enhances the overall performance of the material.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biodegradable materials, and in particular, relates to a polylactic acid-polyhydroxyalkanoate-based degradable composite material and a preparation method thereof. Background Art
[0002] With the improvement of people's environmental awareness, biodegradable polymer materials have attracted more and more attention. Biodegradable polymer materials are polymers whose physical and chemical properties decrease and form carbon dioxide, water, methane and other small molecular weight compounds under the action of microorganisms and plants and animals under aerobic and anaerobic conditions. Polylactic acid is one of the biodegradable materials. It has good mechanical properties and processability. However, the disadvantages of polylactic acid are also prominent. It has poor heat resistance, insufficient toughness, and easy to become brittle after crystallization. These disadvantages limit the application of polylactic acid materials. Polyhydroxyalkanoates are intracellular polyesters synthesized by many bacteria. They exist in organisms mainly as storage substances for carbon sources and energy. They have physicochemical properties similar to those of synthetic plastics and excellent properties such as biodegradability, biocompatibility, optical activity, piezoelectricity, and gas barrier properties that synthetic plastics do not have.
[0003] Polylactic acid has the disadvantages of low elongation at break, poor toughness, and brittle and easy to break. After being blended with polyhydroxyalkanoates, not only the performance of the polyhydroxyalkanoates themselves can be improved, but also the mechanical properties of polylactic acid can be improved. However, a large amount of polyhydroxyalkanoates usually needs to be added, which increases the production cost of the material. In addition, the compatibility between polyhydroxyalkanoates and polylactic acid is not very good. Simple blending will lead to a decrease in the mechanical properties of the product, so it is limited in practical applications. Summary of the invention
[0004] The object of the present invention is to provide a polylactic acid-polyhydroxyalkanoate-based degradable composite material and a preparation method thereof. A ternary flame retardant is combined with lignin to obtain a composite material. The ternary flame retardant composed of hexachlorocyclotriphosphazene and aminosilane contains nitrogen, phosphorus and silicon elements, has a good flame retardant effect, and can improve the flame retardant performance of polylactic acid. Combining lignin with the ternary flame retardant can not only enhance the toughness of polylactic acid, but also improve the mechanical properties and UV resistance of polylactic acid, and provide reaction sites for subsequent grafting reactions. The composite material is combined with vegetable oil to obtain a reinforcing modifier. The lignin in the composite material can be in a mixture containing calcium chloride and peroxide. The polylactic acid-polyhydroxyalkanoate-based biodegradable composite material is obtained by grafting the polylactic acid-polyhydroxyalkanoate-based biodegradable composite material with the vegetable oil in a hydrogen initiation system, and the vegetable oil improves the compatibility between the composite material and polylactic acid and polyhydroxyalkanoate, and improves the plasticity and toughness of the polylactic acid; the polylactic acid, polyhydroxyalkanoate, a reinforcing modifier, an antioxidant and a lubricant are mixed, added into a twin-screw extruder, melt-blended and then extruded to obtain a polylactic acid-polyhydroxyalkanoate-based biodegradable composite material, the reinforcing modifier enhances the interface compatibility between the reinforcing modifier and the polylactic acid and polyhydroxyalkanoate, improves the mechanical properties, toughness and biodegradability of the polylactic acid-polyhydroxyalkanoate biodegradable composite material, improves its comprehensive performance, and reduces its production cost at the same time.
[0005] Technical problem to be solved by the present invention: Polylactic acid has the disadvantages of low elongation at break, poor toughness, and brittle and easy to break. By blending with polyhydroxyalkanoates, not only the performance of the polyhydroxyalkanoates themselves can be improved, but also the mechanical properties of polylactic acid can be improved. However, a large amount of polyhydroxyalkanoates usually needs to be added, which increases the production cost of the material. In addition, the compatibility between polyhydroxyalkanoates and polylactic acid is not very good. Simple blending will lead to a decrease in the mechanical properties of the product, so it is limited in practical applications.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material comprises the following steps:
[0008] S1: A composite material is obtained by combining a ternary flame retardant with lignin;
[0009] S2: combining the composite material with vegetable oil to obtain a reinforcing modifier;
[0010] S3: polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant are blended and added into a twin-screw extruder, melt blended and then extruded, pelletized and dried to obtain a polylactic acid-polyhydroxyalkanoate based biodegradable composite material.
[0011] Further, in step S1, the composite material comprises the following steps to be prepared:
[0012] A1: dissolving hexachlorocyclotriphosphazene to obtain reaction solution A, dissolving aminosilane and NaOH in deionized water to obtain reaction solution B, adding reaction solution B to reaction solution A for the first time, and reacting at 0-5°C for 2-4h, raising the temperature of the reaction system to 45-55°C, adding reaction solution B to reaction solution A for the second time, continuing the reaction for 2-4h, and then adding reaction solution B to reaction solution A for the third time, and then storing the mixture at 80-90°C for 10-12h, cooling to room temperature, and finally washing and drying under reduced pressure to obtain a ternary flame retardant, wherein the mass ratio of reaction solution A to total reaction solution B is 208-229:306-372;
[0013] A2: The ternary flame retardant is dissolved in an ethanol aqueous solution (the volume ratio of ethanol to water is 1:9), and stirred at 65-75°C for 3-5 hours to obtain component A, lignin is dissolved in dimethyl sulfoxide, and stirred at room temperature for 1-3 hours to obtain component B, component A is added to component B, and stirred for 22-24 hours, the mixture is washed with deionized water, and then filtered to precipitate lignin, and then dried at 55-65°C to obtain a composite material, wherein the mass ratio of the ternary flame retardant, the ethanol aqueous solution, the lignin and the dimethyl sulfoxide is 1.5-2.5:16-20:9.5-10.5:100-120.
[0014] In the above reaction process, hexachlorocyclotriphosphazene has chlorine atoms, and aminosilane has amino groups. The amino groups on the aminosilane can combine with the chlorine atoms in the hexachlorocyclotriphosphazene, and the aminosilane is grafted on the hexachlorocyclotriphosphazene to obtain a ternary flame retardant. The aminosilane has silanol groups after hydrolysis, and lignin has a large number of hydroxyl groups. The hydroxyl groups on the lignin can combine with the silanol groups on the aminosilane. The lignin and the aminosilane are combined together to finally obtain a composite material.
[0015] Furthermore, the aminosilane is KH550.
[0016] Further, in step S2, the reinforcing modifier comprises the following steps to prepare:
[0017] Calcium chloride is added to dimethyl sulfoxide and stirred for 8-12 minutes until it is completely dissolved, and then the composite material is added and stirred for 15-25 minutes, and then vegetable oil and hydrogen peroxide solution are added, and stirring is continued for 3-7 minutes, and then the system temperature is increased to 45-55°C, and 4-methoxyphenol is added to terminate the reaction. After the reaction is completed, the obtained solution is added to a dilute hydrochloric acid solution, and the precipitate is filtered, washed with deionized water, and vacuum dried at 55-65°C for 24 hours to obtain a reinforcing modifier, wherein the mass ratio of calcium chloride, dimethyl sulfoxide, composite material, vegetable oil, hydrogen peroxide solution, 4-methoxyphenol and dilute hydrochloric acid solution is 0.5-1.5:15-25:0.5-1.5:7.5-8.5:1-2:0.01-0.03:20-30.
[0018] In the above reaction process, the composite material contains lignin, and in the initiation system containing calcium chloride and hydrogen peroxide, a synergistic reaction can occur to form a peroxide-chloride ion complex, which can extract hydrogen from the lignin to form lignin macromolecular free radicals. The high concentration of benzyl sites in the lignin makes them more easily extracted by hydrogen, thereby supporting active grafting sites. In addition, the formed hydroxyl radicals can react quickly with chlorine to form chlorine atoms without homopolymerization. The formed chlorine atoms can also extract hydrogen from the lignin to form lignin macromolecular free radicals. The lignin macromolecular free radicals can trigger a polymerization reaction of carbon-carbon double bonds in the vegetable oil, graft the vegetable oil onto the composite material, and finally obtain a reinforcing modifier.
[0019] Furthermore, the vegetable oil is castor oil or olive oil.
[0020] Furthermore, in step S3, the polylactic acid-polyhydroxyalkanoate-based degradable composite material is prepared by the following steps:
[0021] The polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant are mixed, stirred at a speed of 30-40rpm for 30-40min and mixed evenly, then added into a twin-screw extruder, melt blended and extruded, the melting temperature is 180-190℃, the screw speed is 200-450r / min, pelletized by water cooling, and then dried to obtain a polylactic acid-polyhydroxyalkanoate degradable composite material, wherein the mass ratio of polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant is 60-80:20-30:10-15:0.1-1:0.1-1.
[0022] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0023] Furthermore, the lubricant is pentaerythritol stearate.
[0024] Beneficial effects of the present invention:
[0025] (1) In the technical scheme of the present invention, a composite material is obtained by combining a ternary flame retardant with lignin. The ternary flame retardant is composed of hexachlorocyclotriphosphazene and aminosilane. Hexachlorocyclotriphosphazene contains nitrogen and phosphorus elements, and aminosilane contains silicon elements. The ternary flame retardant formed by combining aminosilane with hexachlorocyclotriphosphazene has a good flame retardant effect, which can further improve the flame retardant properties of polylactic acid and polyhydroxyalkanoate. The silanol group generated after the hydrolysis of aminosilane can also provide reaction sites for the subsequent grafting reaction, thereby increasing the binding force between the ternary flame retardant and lignin. The aminosilane can also increase The dispersibility of hexachlorocyclotriphosphazene; lignin is cheap, abundant, green and biodegradable. Combining lignin with a ternary flame retardant can not only toughen polylactic acid, but also improve the mechanical properties of polylactic acid. At the same time, the combination of lignin and the ternary flame retardant consumes hydroxyl groups, enhances the hydrophobicity and dispersibility of lignin, and improves the compatibility between lignin and polylactic acid. Lignin can also enhance the UV resistance, ductility and heat resistance of polylactic acid. In addition, the use of lignin also provides reaction sites for subsequent grafting reactions, increasing the binding between lignin and vegetable oil.
[0026] (2) In the technical solution of the present invention, the composite material is combined with vegetable oil to obtain a reinforcing modifier. The lignin in the composite material can be grafted with the vegetable oil in an initiation system containing calcium chloride and hydrogen peroxide. The vegetable oil is grafted onto the composite material to improve the thermal stability of the lignin. The vegetable oil can not only serve as a compatibilizer to improve the compatibility between the composite material and polylactic acid and polyhydroxyalkanoate, but also as a plasticizer to improve the plasticity and toughness of polylactic acid. The hydroxyl groups contained in the vegetable oil can also be further combined with the carboxyl groups in polylactic acid to improve the compatibility between the reinforcing modifier and polylactic acid. Polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant are mixed and added to a twin-screw extruder. After melt blending, extrusion is performed to obtain a polylactic acid-polyhydroxyalkanoate-based degradable composite material. By adding the reinforcing modifier, not only the interfacial compatibility between it and polylactic acid and polyhydroxyalkanoate is enhanced, but also the mechanical properties, toughness, thermal stability and degradability of the polylactic acid-polyhydroxyalkanoate degradable composite material are improved.
[0027] (3) In the technical scheme of the present invention, the ternary flame retardant is combined with lignin and then with vegetable oil to obtain a reinforcing modifier, which is then mixed with polylactic acid, polyhydroxyalkanoate, an antioxidant and a lubricant, extruded after melt blending, pelletized after water cooling, and dried to finally obtain a polylactic acid-polyhydroxyalkanoate-based biodegradable composite material. The reinforcing modifier not only improves the compatibility between polylactic acid and polyhydroxyalkanoate, but also improves the toughness and mechanical properties of the polylactic acid-polyhydroxyalkanoate biodegradable composite material, showing good elongation at break and tensile strength, thereby improving its overall comprehensive performance, reducing pollution to the environment, reducing the production cost of the material, and expanding its application range. DETAILED DESCRIPTION
[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The specific parameters of the raw materials used in the present invention are as follows:
[0030] The molecular weight of polylactic acid is 50,000-700,000, the melting point is 165-175°C, the melt flow index is 15-30 g / 10 min, and the glass transition temperature is 55-60°C; the melting point of polyhydroxyalkanoate is 140-160°C, and the melt flow index is 5-7 g / 10 min; lignin was recovered from corncob biorefining residues by dissolving alkali and acid precipitation, and was purchased from Shandong Longli Biotechnology Co., Ltd., China.
[0031] Example 1
[0032] The composite material comprises the following steps to prepare:
[0033] A1: Hexachlorocyclotriphosphazene was dissolved in 1,4-dioxane at a mass ratio of 18:190 to obtain a reaction solution A, and aminosilane and NaOH were dissolved in deionized water at a mass ratio of 8.5:3.5:90 to obtain a reaction solution B. The reaction solution B was added to the reaction solution A for the first time, and reacted at 0°C for 2 hours. The temperature of the reaction system was raised to 45°C, and the reaction solution B was added to the reaction solution A for the second time. After continuing to react for 2 hours, the reaction solution B was added to the reaction solution A for the third time. The mixture was then stored at 80°C for 10 hours, cooled to room temperature, and finally washed with deionized water. It was dried under reduced pressure at 75°C for 12 hours to obtain a ternary flame retardant. The mass of the reaction solution B added three times was controlled to be equal, wherein the mass ratio of the reaction solution A to the total reaction solution B was 208:306;
[0034] A2: The ternary flame retardant is dissolved in an ethanol aqueous solution (the volume ratio of ethanol to water is 1:9), and stirred at 65°C for 3 hours to obtain component A. Lignin is dissolved in dimethyl sulfoxide and stirred at room temperature for 1 hour to obtain component B. Component A is added to component B and stirred for 22 hours. The mixture is washed with deionized water, filtered to precipitate lignin, and then dried at 55°C to obtain a composite material, wherein the mass ratio of the ternary flame retardant, the ethanol aqueous solution, the lignin, the dimethyl sulfoxide and the deionized water is 1.5:16:9.5:100:40.
[0035] The reinforcing modifier comprises the following steps to prepare:
[0036] Calcium chloride was added to dimethyl sulfoxide and stirred for 8 minutes until it was completely dissolved, and then the composite material was added and stirred for 15 minutes, and then olive oil and 3wt% hydrogen peroxide solution were added, and stirring was continued for 3 minutes, and then the system temperature was increased to 45°C, and 4-methoxyphenol was added to terminate the reaction. After the reaction was completed, the obtained solution was added to a dilute hydrochloric acid solution with a mass concentration of 0.1 mol / L, and the precipitate was filtered, washed with deionized water, and vacuum dried at 55°C for 24 hours to obtain a reinforcing modifier, wherein the mass ratio of calcium chloride, dimethyl sulfoxide, composite material, olive oil, hydrogen peroxide solution, 4-methoxyphenol, dilute hydrochloric acid solution and deionized water was 0.5:15:0.5:7.5:1:0.01:20:40.
[0037] The polylactic acid-polyhydroxyalkanoate-based degradable composite material comprises the following steps:
[0038] Polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 1010 and pentaerythritol stearate are mixed, stirred at a speed of 30 rpm for 30 minutes and mixed evenly, then added into a twin-screw extruder, melt blended and extruded, the melting temperature is 180°C, the screw speed is 200 r / min, pelletized by water cooling, and then dried at 70°C to obtain a polylactic acid-polyhydroxyalkanoate degradable composite material, wherein the mass ratio of polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 1010 and pentaerythritol stearate is 60:20:10:0.1:0.1.
[0039] Example 2
[0040] The composite material comprises the following steps to prepare:
[0041] A1: Hexachlorocyclotriphosphazene was dissolved in 1,4-dioxane at a mass ratio of 18.5:200 to obtain a reaction solution A, and aminosilane and NaOH were dissolved in deionized water at a mass ratio of 9:4:100 to obtain a reaction solution B. The reaction solution B was added to the reaction solution A for the first time, and reacted at 3°C for 3 hours. The temperature of the reaction system was raised to 50°C, and the reaction solution B was added to the reaction solution A for the second time. After continuing to react for 3 hours, the reaction solution B was added to the reaction solution A for the third time, and the mixture was stored at 85°C for 11 hours, cooled to room temperature, and finally washed with deionized water, and dried under reduced pressure at 80°C for 12 hours to obtain a ternary flame retardant. The mass of the reaction solution B added three times was controlled to be equal, wherein the mass ratio of the reaction solution A to the total reaction solution B was 218.5:339;
[0042] A2: The ternary flame retardant is dissolved in an ethanol aqueous solution (the volume ratio of ethanol to water is 1:9), and stirred at 70°C for 4 hours to obtain component A. Lignin is dissolved in dimethyl sulfoxide and stirred at room temperature for 2 hours to obtain component B. Component A is added to component B and stirred for 23 hours. The mixture is washed with deionized water, filtered to precipitate lignin, and then dried at 60°C to obtain a composite material, wherein the mass ratio of the ternary flame retardant, the ethanol aqueous solution, the lignin, the dimethyl sulfoxide and the deionized water is 2:18:10:110:50.
[0043] The reinforcing modifier comprises the following steps to prepare:
[0044] Calcium chloride was added to dimethyl sulfoxide and stirred for 10 minutes until it was completely dissolved, and then the composite material was added and stirred for 20 minutes, and then castor oil and 3wt% hydrogen peroxide solution were added, and stirring was continued for 5 minutes, and then the system temperature was increased to 50°C, and 4-methoxyphenol was added to terminate the reaction. After the reaction was completed, the obtained solution was added to a dilute hydrochloric acid solution with a mass concentration of 0.1 mol / L, and the precipitate was filtered, washed with deionized water, and vacuum dried at 60°C for 24 hours to obtain a reinforcing modifier, wherein the mass ratio of calcium chloride, dimethyl sulfoxide, composite material, castor oil, hydrogen peroxide solution, 4-methoxyphenol, dilute hydrochloric acid solution and deionized water was 1:20:1:8:1.5:0.02:25:50.
[0045] The polylactic acid-polyhydroxyalkanoate-based degradable composite material comprises the following steps:
[0046] Polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 1076 and pentaerythritol stearate are mixed, stirred at a speed of 35 rpm for 35 minutes and mixed evenly, then added into a twin-screw extruder, melt blended and extruded, the melting temperature is 185°C, the screw speed is 300 r / min, pelletized by water cooling, and then dried at 75°C to obtain a polylactic acid-polyhydroxyalkanoate degradable composite material, wherein the mass ratio of polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 1076 and pentaerythritol stearate is 70:25:13:0.5:0.5.
[0047] Example 3
[0048] The composite material comprises the following steps to prepare:
[0049] A1: Hexachlorocyclotriphosphazene was dissolved in 1,4-dioxane at a mass ratio of 19:210 to obtain a reaction solution A, and aminosilane and NaOH were dissolved in deionized water at a mass ratio of 9.5:4.5:110 to obtain a reaction solution B. The reaction solution B was added to the reaction solution A for the first time, and reacted at 5°C for 4 hours. The temperature of the reaction system was raised to 55°C, and the reaction solution B was added to the reaction solution A for the second time. After continuing to react for 4 hours, the reaction solution B was added to the reaction solution A for the third time. The mixture was then stored at 90°C for 12 hours, cooled to room temperature, and finally washed with deionized water. It was dried under reduced pressure at 85°C for 12 hours to obtain a ternary flame retardant. The mass of the reaction solution B added three times was controlled to be equal, wherein the mass ratio of the reaction solution A to the total reaction solution B was 229:372;
[0050] A2: The ternary flame retardant is dissolved in an ethanol aqueous solution (the volume ratio of ethanol to water is 1:9), and stirred at 75°C for 5 hours to obtain component A. Lignin is dissolved in dimethyl sulfoxide and stirred at room temperature for 3 hours to obtain component B. Component A is added to component B and stirred for 24 hours. The mixture is washed with deionized water, filtered to precipitate lignin, and then dried at 65°C to obtain a composite material, wherein the mass ratio of the ternary flame retardant, the ethanol aqueous solution, the lignin, the dimethyl sulfoxide and the deionized water is 2.5:20:10.5:120:60.
[0051] The reinforcing modifier comprises the following steps to prepare:
[0052] Calcium chloride was added to dimethyl sulfoxide and stirred for 12 minutes until it was completely dissolved, and then the composite material was added and stirred for 25 minutes, and then olive oil and 3wt% hydrogen peroxide solution were added, and stirring was continued for 7 minutes, and then the system temperature was increased to 55°C, and 4-methoxyphenol was added to terminate the reaction. After the reaction was completed, the obtained solution was added to a dilute hydrochloric acid solution with a mass concentration of 0.1 mol / L, and the precipitate was filtered, washed with deionized water, and vacuum dried at 65°C for 24 hours to obtain a reinforcing modifier, wherein the mass ratio of calcium chloride, dimethyl sulfoxide, composite material, olive oil, hydrogen peroxide solution, 4-methoxyphenol, dilute hydrochloric acid solution and deionized water was 1.5:25:1.5:8.5:2:0.03:30:60.
[0053] The polylactic acid-polyhydroxyalkanoate-based degradable composite material comprises the following steps:
[0054] Polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 168 and pentaerythritol stearate are mixed, stirred at a speed of 40 rpm for 40 minutes and mixed evenly, then added into a twin-screw extruder, melt blended and extruded, the melting temperature is 190°C, the screw speed is 450 r / min, pelletized by water cooling, and then dried at 80°C to obtain a polylactic acid-polyhydroxyalkanoate degradable composite material, wherein the mass ratio of polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant 168 and pentaerythritol stearate is 80:30:15:1:1.
[0055] Comparative Example 1
[0056] The difference between this comparative example and Example 3 is that KH550 is replaced by KH570, and the remaining steps and raw materials are the same as Example 3.
[0057] Comparative Example 2
[0058] The difference between this comparative example and Example 3 is that the ternary flame retardant is prepared by the following steps:
[0059] Hexachlorocyclotriphosphazene was dissolved in 1,4-dioxane at a mass ratio of 19:210 to obtain a reaction solution A, and aminosilane and NaOH were dissolved in deionized water at a mass ratio of 28.5:13.5:330 to obtain a reaction solution B. The reaction solution B was added to the reaction solution A, and the reaction was carried out at 5°C for 4 hours. The temperature of the reaction system was raised to 55°C, and the reaction was continued for 4 hours. The system was then heated to 90°C and stored for 12 hours, cooled to room temperature, and finally washed with deionized water, and dried under reduced pressure at 85°C for 12 hours to obtain a ternary flame retardant, wherein the mass ratio of the reaction solution A to the reaction solution B was 229:372, and the remaining steps and raw materials were synchronized with Example 3.
[0060] Comparative Example 3
[0061] The difference between this comparative example and Example 3 is that when preparing the reinforcing modifier, the composite material is replaced by a ternary flame retardant, and the remaining steps and raw materials are the same as those of Example 3.
[0062] Comparative Example 4
[0063] The difference between this comparative example and Example 3 is that the reinforcing modifier is directly prepared by uniformly mixing the composite material and olive oil in a mass ratio of 1.5:8.5.
[0064] Comparative Example 5
[0065] The difference between this comparative example and Example 3 is that when preparing the reinforcing modifier, the mass of olive oil is replaced by soybean oil, and the remaining steps and raw materials are synchronized with Example 3.
[0066] The polylactic acid-polyhydroxyalkanoate-based degradable composite materials prepared in Examples 1-3 and Comparative Examples 1-5 are now tested for tensile strength, elongation at break, Vicat softening temperature, biodegradation rate and flame retardancy, wherein the tensile strength and elongation at break are measured using the GB / T 1040.3-2006 standard; the Vicat softening temperature is measured using the GB / T 1633-2000 standard; the biodegradation rate is measured using the GB / T 19277-2011 standard, and the final carbon dioxide release of the polylactic acid-polyhydroxyalkanoate-based degradable composite materials prepared in Examples 1-3 and Comparative Examples 1-6 after degradation for 60 days is measured, and the biodegradation rate (%) of the material is expressed by the ratio of the actual carbon dioxide release to its theoretical maximum release; and the flame retardancy is measured using the UL 94 standard. The test results are shown in Table 1:
[0067] Table 1 Performance parameters of the composite materials prepared in Examples 1-3 and Comparative Examples 1-5
[0068]
[0069] It can be seen from the data in Table 1 above that, by comparing Comparative Examples 1-2 with Example 3, it can be seen that the test results of the ternary flame retardant prepared by combining KH570 with hexachlorocyclotriphosphazene or adding KH550 to hexachlorocyclotriphosphazene at one time to prepare the ternary flame retardant are worse than those of Example 3, indicating that the ternary flame retardant prepared by combining hexachlorocyclotriphosphazene with KH550 and adding KH550 to hexachlorocyclotriphosphazene three times not only has a good flame retardant effect, but also can enhance the binding force between the ternary flame retardant and lignin, and further improve the toughness, mechanical properties, heat resistance, flame retardancy and biodegradability of the polylactic acid-polyhydroxyalkanoate-based degradable composite material;
[0070] From the comparison between Comparative Example 3 and Example 3, it can be seen that the test result of the reinforcing modifier prepared by directly combining the ternary flame retardant with the vegetable oil is worse than that of Example 3, indicating that the ternary flame retardant is first combined with lignin to obtain a composite material, and then the composite material is combined with the vegetable oil to obtain a reinforcing modifier, which can increase the interfacial compatibility between the composite material and polylactic acid, and at the same time improve the toughness, mechanical properties and heat resistance of the polylactic acid-polyhydroxyalkanoate-based degradable composite material;
[0071] By comparing Comparative Examples 4-5 with Example 3, it can be seen that the reinforcing modifier prepared by uniformly stirring the composite material and olive oil or by combining soybean oil with the composite material to prepare the reinforcing modifier has a test result that is worse than that of Example 3, indicating that the reinforcing modifier prepared by grafting the composite material with vegetable oil in an initiation system containing calcium chloride and hydrogen peroxide can enhance the binding force between the composite material and the vegetable oil, further increase the compatibility between the composite material and polylactic acid and polyhydroxyalkanoate, and improve the toughness, mechanical properties, heat resistance, flame retardancy and biodegradability of the polylactic acid-polyhydroxyalkanoate-based degradable composite material.
[0072] As can be seen from Table 1 above, the polylactic acid-polyhydroxyalkanoate-based degradable composite materials prepared in Examples 1-3 are compared with Comparative Examples 1-5. The ternary flame retardant is combined with lignin, and then combined with vegetable oil to obtain a reinforcing modifier, and finally mixed with polylactic acid, polyhydroxyalkanoate, antioxidant and lubricant, and melt blended and extruded to obtain a polylactic acid-polyhydroxyalkanoate-based degradable composite material, which improves its toughness, mechanical properties, heat resistance and biodegradability as a whole, and meets the test performance requirements. The polylactic acid-polyhydroxyalkanoate-based degradable composite materials prepared in Comparative Examples 1-5 did not meet the performance requirements. The polylactic acid-polyhydroxyalkanoate-based degradable composite materials prepared by the present invention not only have good biodegradability, but also have good toughness, mechanical properties, heat resistance and flame retardancy, greatly improve the comprehensive performance, reduce pollution to the environment, and reduce production costs.
[0073] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0074] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material, characterized in that: The following steps are involved: S1: A composite material is obtained by combining a ternary flame retardant with lignin; S2: combining the composite material with vegetable oil to obtain a reinforcing modifier; S3: mixing polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant, adding them into a twin-screw extruder, extruding after melt blending, pelletizing after water cooling, and drying to obtain a polylactic acid-polyhydroxyalkanoate based biodegradable composite material; Step S1 is specifically as follows: A1: dissolving hexachlorocyclotriphosphazene to obtain reaction solution A, dissolving aminosilane and NaOH in deionized water to obtain reaction solution B, adding reaction solution B to reaction solution A for the first time, and reacting at 0-5°C for 2-4h, raising the temperature of the reaction system to 45-55°C, adding reaction solution B to reaction solution A for the second time, continuing the reaction for 2-4h, and then adding reaction solution B to reaction solution A for the third time, and then storing the mixture at 80-90°C for 10-12h, cooling to room temperature, and finally washing and drying under reduced pressure to obtain a ternary flame retardant; A2: The ternary flame retardant is dissolved in an ethanol aqueous solution and stirred at 65-75°C for 3-5 hours to obtain component A, lignin is dissolved in dimethyl sulfoxide and stirred at room temperature for 1-3 hours to obtain component B, component A is added to component B and stirred for 22-24 hours, the mixture is washed with deionized water, filtered, and then dried to obtain a composite material; Step S2 is specifically as follows: Calcium chloride is added to dimethyl sulfoxide and stirred for 8-12 minutes, then the composite material is added and stirred for 15-25 minutes, then vegetable oil and hydrogen peroxide solution are added, stirring is continued for 3-7 minutes, the system temperature is increased to 45-55° C., 4-methoxyphenol is added to terminate the reaction, the obtained solution is added to a dilute hydrochloric acid solution, filtered, washed with deionized water, and vacuum dried to obtain a reinforcing modifier; The vegetable oil is castor oil or olive oil.
2. The method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material according to claim 1, characterized in that: In step A1, the mass ratio of reaction liquid A to total reaction liquid B is 208-229:306-372; in step A2, the mass ratio of ternary flame retardant, ethanol aqueous solution, lignin and dimethyl sulfoxide is 1.5-2.5:16-20:9.5-10.5:100-120.
3. The method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material according to claim 1, characterized in that: The mass ratio of calcium chloride, dimethyl sulfoxide, composite material, vegetable oil, hydrogen peroxide solution, 4-methoxyphenol and dilute hydrochloric acid solution is 0.5-1.5:15-25:0.5-1.5:7.5-8.5:1-2:0.01-0.03:20-30.
4. The method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material according to claim 1, characterized in that: Step S3 is specifically as follows: The polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant are mixed, stirred at a speed of 30-40 rpm for 30-40 minutes and mixed evenly, then added into a twin-screw extruder, melt blended and extruded, the melt temperature is 180-190° C., the screw speed is 200-450 r / min, pelletized by water cooling, and then dried to obtain a polylactic acid-polyhydroxyalkanoate degradable composite material.
5. The method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material according to claim 4, characterized in that: The mass ratio of polylactic acid, polyhydroxyalkanoate, reinforcing modifier, antioxidant and lubricant is 60-80:20-30:10-15:0.1-1:0.1-1.
6. The method for preparing a polylactic acid-polyhydroxyalkanoate-based degradable composite material according to claim 4, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 1076, and antioxidant 168.
7. A polylactic acid-polyhydroxyalkanoate-based degradable composite material obtained by the preparation method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Organic-inorganic hybridized nanometer compound with chain extension-flame retardant synergistic effect, and preparation method and flame retardant polylactic acid thereof
CN106928490A
Antiflaming lignin / polylactic acid composite material and preparation method thereof
CN108410148A
Cited By
Degradable low-smoke halogen-free flame-retardant cable
CN224036117U