A titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts

By using a combination of a small molecular weight polyether amine-based penetrating stripper and hydrogen peroxide on titanium alloy aluminum alloy bimetal structural parts, the problems of high wastewater treatment cost and insufficient cleanliness of the titanium removal membrane method in the existing technology are solved, and the problem is achieved. It achieves efficient and environmentally friendly titanium film stripping effect.

CN118461008BActive Publication Date: 2024-10-25DONGGUAN CHENGJUN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410668715.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-10-25
Estimated Expiration
2044-05-28

AI Technical Summary

Technical Problem

The existing methods for removing titanium films include the use of strong acids and alkalis, which results in high wastewater treatment costs, corrosion of aluminum alloy anodes, sandblasting methods that require pre-shielding of components and high costs, and the treatment is not clean enough.

Method used

A titanium film deplating agent for titanium alloy aluminum alloy bimetal structural parts is used, including a penetrating stripper, hydrogen peroxide, chelating agent, corrosion inhibitor and accelerator, by preparing a small molecular weight polyether amine-based penetrating stripper and The combination of hydrogen oxide uses peroxyl radicals and thioether structure to achieve local strong oxidative deplating of the titanium film and improve cleanliness.

Benefits of technology

It realizes water-based chemical stripping without strong acid, strong alkali, toxic and harmful substances, reduces the processing cost, improves the cleanliness and efficiency of stripping, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118461008B_ABST
    Figure CN118461008B_ABST
Patent Text Reader

Abstract

The present invention relates to a titanium film stripping agent for a titanium alloy aluminum alloy bimetallic structural part, and belongs to the technical field of electroplating. The titanium film stripping agent includes the following components by mass fraction: 12-18% of a penetrating stripping agent, 3.2-4.4% of hydrogen peroxide, 6-9% of a chelating agent, 2.5-3.5% of a corrosion inhibitor, and 4-6% of a promoter, and the balance is water; the penetrating stripping agent has a polyether segment as the main chain, has good water dispersibility and permeability, and the sulfur, nitrogen, and oxygen structures at the ends of its molecules form a chelation effect and adhere to the surface of the titanium film, and the peroxy free radicals generated by hydrogen peroxide attack the carbonyl in the acetylated structure, and peracetic acid is generated in situ on the surface of the titanium film, forming local strong oxidizing properties on the surface of the titanium film, accelerating the stripping of the titanium film, and the small-grained titanium film of the stripping is chelated and captured by the penetrating stripping agent, which is a small molecular weight polymer, and has a large resistance in the stripping solution, and is easier to peel off and bring out the small-grained titanium film of the stripping stripping, so that the stripping cleanliness is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating, and in particular relates to a titanium film stripping agent for a titanium alloy and aluminum alloy bimetallic structural part. Background Art

[0002] Aluminum alloy has the advantages of small specific gravity, high ductility, excellent electrical and thermal conductivity, and easy processing. Titanium alloy has high strength, good corrosion resistance, and high heat resistance, and is widely used in aerospace, electronics, architectural decoration and other fields. In particular, the current new generation of mobile phone frames widely use titanium alloy as the frame, and the middle plate is a bimetallic structural part of aluminum alloy, which can not only reflect the lightweight, corrosion-resistant and wear-resistant performance of titanium alloy as the frame, but also show the advantage of aluminum alloy as the middle plate to be easy to form and reduce the overall price. In the process of making titanium alloy and aluminum alloy bimetal as aluminum alloy anode, a layer of colorful irregular titanium film will also be generated on the surface of titanium alloy. The subsequent processing process needs to remove the colorful irregular titanium film on the surface of titanium alloy. Among them, the chemical properties of aluminum alloy are active and it is easy to react with acid and alkali to corrode. The aluminum alloy anode film will also react with acid and alkali, and the corrosion will cause the film layer to be discolored and fall off.

[0003] In the prior art, there are two main methods for stripping titanium film: chemical method and sandblasting method. The chemical method uses strong alkali or strong acid and adds hydrogen peroxide, which has high wastewater treatment cost, and strong acids and strong alkalis can easily corrode aluminum alloy and aluminum alloy anode film. The sandblasting method has high cleanliness and no wastewater is generated. However, it is usually necessary to pre-shield other components except titanium alloy. After sandblasting, the size of titanium alloy is greatly affected, and the processing cost is high. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts comprises the following components in mass fractions: 12-18% of a penetrating stripping agent, 3.2-4.4% of hydrogen peroxide, 6-9% of a chelating agent, 2.5-3.5% of a corrosion inhibitor, 4-6% of an accelerator, and the balance is water.

[0007] The penetrating stripper is prepared by the following method:

[0008] Step A1: premix polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to no higher than 20°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.2-1.5h, then raise the temperature to 35-45°C, add triethylamine and continue stirring and reacting for 20-30min. After the reaction is completed, vacuum dry and remove tetrahydrofuran to obtain intermediate compound a;

[0009] Furthermore, the ratio of the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran is 0.1 mol: 0.11-0.13 mol: 4.5-6 mL: 65-100 mL, and the allyl glycidyl ether having a monoepoxy structure is ring-opened with the active amino group of the polyetheramine;

[0010] Furthermore, the polyetheramine is a low molecular weight difunctional polyetheramine, and the average molecular weight is not higher than 1000.

[0011] Step A2: Mix the intermediate compound a, mercaptoethanol, dimethyl benzoate and ethanol, raise the temperature to 65-75°C, and use UVA ultraviolet light at 240-360W / m 2 The mixture was irradiated with high intensity and stirred for reaction for 2.2-3.5 hours. After the reaction was completed, ethanol was removed by rotary evaporation to obtain intermediate compound b;

[0012] Furthermore, the dosage ratio of the intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol is 0.1 mol: 0.2 mol: 0.1-0.15 g: 150-280 mL. Under the promotion of ultraviolet irradiation, the active thiol group of mercaptoethanol and the double bond introduced by the intermediate compound a undergo click addition.

[0013] Step A3: Mix the intermediate compound b and toluene, introduce dry nitrogen for protection, control the water bath temperature at 40-50°C, slowly add acetic anhydride, and control the total reaction time to be 1.2-1.5h. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent;

[0014] Furthermore, the usage ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.14-0.16 mol: 6-8 g: 120-180 mL, and the acetic anhydride reacts with the alcohol in the molecular structure of the intermediate compound b for acetylation.

[0015] Furthermore, the chelating agent is one or a combination of two or more of potassium sodium tartrate, sodium citrate, EDTA-4Na and sodium gluconate.

[0016] Furthermore, the corrosion inhibitor is one or a combination of two or more of sodium silicate, potassium silicate, sodium metasilicate and potassium metasilicate.

[0017] Furthermore, the promoter is one or both of polyferric sulfate and polyaluminium ferric sulfate.

[0018] Beneficial effects of the present invention:

[0019] The invention discloses a water-based chemical stripping agent, which does not contain toxic and harmful substances such as strong acid and strong alkali, cyanide, nitrate, etc., has simple post-treatment, is more environmentally friendly, and has clean stripping and moderate stripping time, so as to facilitate industrial stripping treatment. The invention benefits from the coordinated effect of the penetrating stripping agent and hydrogen peroxide in the components. The penetrating stripping agent uses a small molecular weight polyetheramine as a raw material, and is prepared by ring-opening allyl glycidyl ether and its amino group to introduce an alkenyl ether structure, and then by click addition of mercaptoethanol and the introduced alkenyl group to introduce a thioether structure and a primary alcohol hydroxyl group, and finally by acetic anhydride and the primary alcohol hydroxyl group to carry out acetylation reaction. The prepared penetrating stripping agent has a polyether segment as the main chain and is compatible with the aqueous agent. It has good dispersibility and permeability. The sulfide structure at the end of its molecule forms a chelate with the nitrogen and oxygen structures in the chain, and adheres to the surface of the titanium film during the stripping process. The peroxy free radicals generated by hydrogen peroxide attack the carbonyl group in the acetylated structure, and generate peracetic acid in situ on the surface of the titanium film, forming local strong oxidizing properties on the surface of the titanium film, accelerating the stripping of the titanium film, and the small-grained titanium film being stripped is chelated and captured by the penetrating stripper. It is a small molecular weight polymer. Compared with small molecule chelating agents, it has greater resistance in the stripping solution and generates greater stripping force in the dynamic state of the stripping solution, making it easier to peel off and remove the small-grained titanium film that is being stripped, making the stripping cleanliness higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 The stripping test results of Example 1 of the present invention and the comparative example are shown;

[0022] Figure 2 The stripping test results of Example 2 of the present invention and the comparative example are shown;

[0023] Figure 3 The stripping test results of Example 3 of the present invention and the comparative example are shown;

[0024] Figure 4 The stripping test results of Example 4 of the present invention and the comparative example are shown. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1, preparing a titanium film stripping agent, the specific implementation process is as follows:

[0027] (1) Preparation of penetrating stripping agent

[0028] Step A1: Take polyetheramine, CAD-230 difunctional polyetheramine produced by Yangzhou Chenhua New Materials Co., Ltd., with an average molecular weight of about 230, premix the polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to 5°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.2h, then raise the temperature to 35°C, add triethylamine and continue stirring and reacting for 20min, wherein the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran are used in a ratio of 0.1mol:0.11mol:4.5mL:65mL. After the reaction is completed, vacuum drying is performed to remove tetrahydrofuran to obtain intermediate compound a.

[0029] Step A2: Mix the intermediate compound a, mercaptoethanol, dimethyl benzoate and ethanol, raise the temperature to 65°C, and use UVA with an intensity of 240 W / m 2 The mixture was irradiated with ultraviolet light and stirred for reaction for 2.2 hours, wherein the usage ratio of intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol was 0.1 mol: 0.2 mol: 0.1 g: 150 mL. After the reaction, ethanol was removed by rotary evaporation to obtain intermediate compound b.

[0030] Step A3: Take the intermediate compound b and toluene, mix them, pass dry nitrogen for protection, control the temperature of the water bath to 40°C, and then slowly add acetic anhydride for 30 minutes. After complete addition, continue to stir the reaction at a constant temperature. The total reaction time of the addition of acetic anhydride is controlled to be 1.2 hours, wherein the amount ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.14 mol: 6 g: 120 mL. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent.

[0031] (2) Configuration of titanium film stripping agent

[0032] Step S1, ingredients: raw materials are taken according to mass fraction, 12% of penetration stripping agent, which is self-made in this embodiment; 3.2% of hydrogen peroxide, which is an industrial grade raw material; 9% of chelating agent, which is selected from potassium sodium tartrate; 3.5% of corrosion inhibitor, which is selected from sodium silicate; 6% of accelerator, which is selected from polyferric sulfate; 66.3% of water;

[0033] Step S2, liquid preparation: premix the penetrating stripping agent, chelating agent, corrosion inhibitor, accelerator and water evenly, then add hydrogen peroxide and mix to obtain a titanium film stripping agent.

[0034] Example 2, preparing a titanium film stripping agent, the specific implementation process is as follows:

[0035] (1) Preparation of penetrating stripping agent

[0036] Step A1: Take polyetheramine, CAED-900 difunctional polyetheramine produced by Yangzhou Chenhua New Materials Co., Ltd., with an average molecular weight of about 900, premix the polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to 20°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.5h, then raise the temperature to 45°C, add triethylamine and continue stirring and reacting for 30min, wherein the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran are used in a ratio of 0.1mol:0.13mol:6mL:100mL. After the reaction is completed, vacuum drying is performed to remove tetrahydrofuran to obtain intermediate compound a.

[0037] Step A2: Mix the intermediate compound a, mercaptoethanol, dimethyl benzoate and ethanol, raise the temperature to 75°C, and use UVA with an intensity of 360W / m 2 The mixture was irradiated with ultraviolet light and stirred for 3.5 hours, wherein the amount ratio of intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol was 0.1 mol: 0.2 mol: 0.15 g: 280 mL. After the reaction, ethanol was removed by rotary evaporation to obtain intermediate compound b.

[0038] Step A3: Take the intermediate compound b and toluene, mix them, pass dry nitrogen for protection, control the temperature of the water bath to 50°C, and then slowly add acetic anhydride for 30 minutes. After complete addition, continue to stir the reaction at a constant temperature. The total reaction time of acetic anhydride is controlled to be 1.5 hours, wherein the amount ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.16 mol: 8 g: 180 mL. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent.

[0039] (2) Configuration of titanium film stripping agent

[0040] Step S1, ingredients: raw materials are taken according to mass fraction, 18% of penetration stripping agent, which is self-made in this embodiment; 4.4% of hydrogen peroxide, which is an industrial grade raw material; 6% of chelating agent, which is selected from EDTA-4Na; 2.5% of corrosion inhibitor, which is selected from potassium silicate; 4% of accelerator, which is selected from polyferric sulfate; 65.1% of water;

[0041] Step S2, liquid preparation: premix the penetrating stripping agent, chelating agent, corrosion inhibitor, accelerator and water evenly, then add hydrogen peroxide and mix to obtain a titanium film stripping agent.

[0042] Example 3, preparing a titanium film stripping agent, the specific implementation process is as follows:

[0043] (1) Preparation of penetrating stripping agent

[0044] Step A1: Take polyetheramine, CAED-600 difunctional polyetheramine produced by Yangzhou Chenhua New Materials Co., Ltd., with an average molecular weight of about 600, premix the polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to 15°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.3h, then raise the temperature to 40°C, add triethylamine and continue stirring and reacting for 30min, wherein the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran are used in a ratio of 0.1mol:0.12mol:5.5mL:90mL. After the reaction is completed, vacuum drying is performed to remove tetrahydrofuran to obtain intermediate compound a.

[0045] Step A2: Mix the intermediate compound a, mercaptoethanol, dimethyl benzoate and ethanol, raise the temperature to 72°C, and use UVA with an intensity of 300W / m 2 The mixture was irradiated with ultraviolet light and stirred for 3 hours, wherein the dosage ratio of intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol was 0.1 mol: 0.2 mol: 0.12 g: 220 mL. After the reaction, ethanol was removed by rotary evaporation to obtain intermediate compound b.

[0046] Step A3: Take the intermediate compound b and toluene, mix them, pass dry nitrogen for protection, control the temperature of the water bath to 45°C, and then slowly add acetic anhydride for 30 minutes. After complete addition, continue to stir the reaction at a constant temperature. The total reaction time of acetic anhydride is controlled to be 1.4 hours, wherein the amount ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.15 mol: 7 g: 150 mL. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent.

[0047] (2) Configuration of titanium film stripping agent

[0048] Step S1, ingredients: raw materials are taken according to mass fraction, 14% of penetration stripping agent, which is self-made in this embodiment; 3.8% of hydrogen peroxide, which is an industrial-grade raw material; 7.2% of chelating agent, which is compounded by potassium sodium tartrate, sodium citrate and sodium gluconate in a mass ratio of 1:1:1; 3.2% of corrosion inhibitor, which is compounded by sodium silicate, sodium metasilicate and potassium metasilicate in a mass ratio of 1:1:1; 5.5% of accelerator, which is selected from polyaluminium ferric sulfate; 66.3% of water;

[0049] Step S2, liquid preparation: premix the penetrating stripping agent, chelating agent, corrosion inhibitor, accelerator and water evenly, then add hydrogen peroxide and mix to obtain a titanium film stripping agent.

[0050] Example 4, preparing a titanium film stripping agent, the specific implementation process is as follows:

[0051] (1) Preparation of penetrating stripping agent

[0052] Step A1: Take polyetheramine, CAED-600 difunctional polyetheramine produced by Yangzhou Chenhua New Materials Co., Ltd., with an average molecular weight of about 600, premix the polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to 10°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.4 hours, then raise the temperature to 42°C, add triethylamine and continue stirring and reacting for 30 minutes, wherein the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran are used in a ratio of 0.1 mol: 0.12 mol: 5.5 mL: 85 mL, and after the reaction is completed, vacuum drying is performed to remove tetrahydrofuran to obtain intermediate compound a.

[0053] Step A2: Mix the intermediate compound a, mercaptoethanol, dimethyl benzoate and ethanol, raise the temperature to 75°C, and use UVA with an intensity of 280 W / m 2 The mixture was irradiated with ultraviolet light and stirred for 2.8 hours, wherein the amount ratio of intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol was 0.1 mol: 0.2 mol: 0.12 g: 250 mL. After the reaction, ethanol was removed by rotary evaporation to obtain intermediate compound b.

[0054] Step A3: Take the intermediate compound b and toluene, mix them, pass dry nitrogen for protection, control the temperature of the water bath to 40°C, and then slowly add acetic anhydride for 30 minutes. After complete addition, continue to stir the reaction at a constant temperature. The total reaction time of the addition of acetic anhydride is controlled to be 1.4 hours, wherein the amount ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.14 mol: 7 g: 160 mL. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent.

[0055] (2) Configuration of titanium film stripping agent

[0056] Step S1, ingredients: raw materials are taken according to mass fraction, 15% of the penetration stripping agent is prepared in this embodiment; 4.1% of hydrogen peroxide is an industrial-grade raw material; 7.8% of the chelating agent is prepared by mixing sodium citrate, EDTA-4Na and sodium gluconate in a mass ratio of 1:1:1; 3% of the corrosion inhibitor is prepared by mixing potassium silicate, sodium metasilicate and potassium metasilicate in a mass ratio of 1:1:1; 5% of the accelerator is selected from polyaluminium ferric sulfate; 65.1% of water;

[0057] Step S2, liquid preparation: premix the penetrating stripping agent, chelating agent, corrosion inhibitor, accelerator and water evenly, then add hydrogen peroxide and mix to obtain a titanium film stripping agent.

[0058] Comparative Example: An acidic stripping agent is prepared with reference to the prior art, and the specific implementation process is as follows:

[0059] The raw materials are taken according to mass fraction, namely, 20% sulfuric acid, 8% oxalic acid, 7% sodium citrate, 3.5% sodium silicate, 4.5% polyferric sulfate and 57% water; the raw materials are added and mixed to obtain an acidic stripping agent.

[0060] Take the titanium alloy-aluminum alloy workpieces to be stripped from the same batch, randomly select 10 pieces, use sandblasting to polish the titanium film for stripping, and use the weighing method to detect the average value of the mass loss before and after sandblasting as the complete stripping amount M0;

[0061] The titanium film stripping agent prepared above was diluted 10 times with water to prepare a stripping solution, the workpiece to be stripped was clamped in a stripping tank, the stripping solution temperature was controlled to be 35±2°C, the workpiece was taken out after stripping, rinsed with water, and dried, and the experimental stripping amount M1 was detected by weighing method, the detection frequency was 1min / time, and the stripping rate was calculated as M1 / M0×100%, and the stripping data of Examples 1 to 4 were compared with the comparative examples, respectively, as shown in detail. Figure 1-Figure 4 shown.

[0062] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0063] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts, characterized in that: The composition comprises the following components by mass fraction: 12-18% of a penetrating stripping agent, 3.2-4.4% of hydrogen peroxide, 6-9% of a chelating agent, 2.5-3.5% of a corrosion inhibitor, 4-6% of an accelerator, and the balance being water; The penetrating stripper is prepared by the following method: Step A1: premix polyetheramine and tetrahydrofuran, introduce nitrogen protection, adjust the temperature of the reaction system to no higher than 20°C in an ice-water bath, add allyl glycidyl ether, stir and react for 1.2-1.5h, then raise the temperature to 35-45°C, add triethylamine and continue stirring and reacting for 20-30min. After the reaction is completed, vacuum dry and remove tetrahydrofuran to obtain intermediate compound a; Step A2: Mix the intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol, raise the temperature to 65-75°C, and use UVA ultraviolet light at 240-360W / m 2 High intensity irradiation, stirring and reacting for 2.2-3.5 hours, after the reaction is completed, ethanol is removed by rotary evaporation to obtain intermediate compound b; Step A3: Mix the intermediate compound b and toluene, introduce dry nitrogen for protection, control the water bath temperature at 40-50°C, slowly add acetic anhydride, and control the total reaction time to be 1.2-1.5h. After the reaction is completed, add ammonium carbonate and evaporate under reduced pressure to remove toluene to obtain a penetrating stripping agent; The chelating agent is one or more combinations of potassium sodium tartrate, sodium citrate, EDTA-4Na and sodium gluconate; The corrosion inhibitor is one or more combinations of sodium silicate, potassium silicate, sodium metasilicate and potassium metasilicate; The accelerator is one or both of polyferric sulfate and polyaluminium ferric sulfate.

2. The titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts according to claim 1, characterized in that: The usage ratio of the amino content of the polyetheramine, allyl glycidyl ether, triethylamine and tetrahydrofuran is 0.1 mol: 0.11-0.13 mol: 4.5-6 mL: 65-100 mL.

3. A titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts according to claim 2, characterized in that: The polyetheramine is a small molecular weight difunctional polyetheramine with an average molecular weight of no more than 1000.

4. The titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts according to claim 3, characterized in that: The usage ratio of the intermediate compound a, mercaptoethanol, benzoin dimethyl ether and ethanol is 0.1 mol: 0.2 mol: 0.1-0.15 g: 150-280 mL.

5. The titanium film stripping agent for titanium alloy and aluminum alloy bimetallic structural parts according to claim 4, characterized in that: The usage ratio of the intermediate compound b, acetic anhydride, ammonium carbonate and toluene is 0.1 mol: 0.14-0.16 mol: 6-8 g: 120-180 mL.