A reverse polarity red light LED chip and its manufacturing method
Through the design of a new electrode structure and GaAs ohmic contact ring, combined with the specific structure of AlCu alloy material and silver mirror layer, the problems of improving the brightness and reliability of reverse polarity red LED chips and high cost are solved, achieving high brightness and stability High performance and low cost LED chips.
Patent Information
- Application Number
- CN202410910141.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-09
AI Technical Summary
There is a need to improve the brightness and reliability of reverse polarity red LED chips. At the same time, the production cost is high. It is necessary to design an LED chip with high brightness, reliable and stable performance and low cost.
A new electrode structure is used with a GaAs ohmic contact ring design. The inner layer of the electrode is made of AlCu alloy material, and through a layer-by-layer coating structure and a specific silver mirror layer design, the light emitting rate and electrode stability are increased. At the same time, by setting up in the through hole Smaller ohmic contact blocks increase the contact area of the silver mirror layer and reduce production costs.
It improves the light emission rate and electrode stability of the LED chip, reduces production costs, meets the requirements for high brightness and reliability, and avoids the problems of electrode absorption of light and bonding wire impact.
Smart Images

Figure CN118472142B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of LEDs, and in particular to a reverse polarity red light LED chip and a manufacturing method thereof. Background Art
[0002] The materials and processes of reverse polarity red LED chips are different from those of traditional red LED chips. Reverse polarity red LED chips have higher luminous efficiency than traditional polarity chips and are widely used in lighting and outdoor display fields.
[0003] With the continuous expansion of application scenarios and the fierce market competition, new requirements have been put forward for the brightness and reliability of reverse polarity LEDs in order to meet the growing consumer demand. In addition, in the chip production process, precious metals account for half of the cost. Therefore, designing an LED chip with high brightness, reliable and stable performance, and reduced production costs has become an urgent problem to be solved. Summary of the invention
[0004] The object of the present invention is to provide a reverse polarity red light LED chip and a manufacturing method thereof, which has the advantages of high brightness, stable performance and low production cost.
[0005] In order to solve the above problems, the technical solution provided by the present invention is:
[0006] The first aspect of the present invention is to provide a reverse polarity red light LED chip, comprising a P electrode, a Si substrate, a first bonding layer, a second bonding layer, a barrier layer, a silver mirror layer, a dielectric film layer, a GaP window layer, a P-type semiconductor layer, a light-emitting layer, an N-type semiconductor layer and an N-electrode arranged in sequence from bottom to top; the N-type semiconductor layer comprises an N-type limiting layer, a current spreading layer, a roughening layer arranged in sequence from bottom to top, and a GaAs ohmic contact ring arranged on the upper surface of the roughening layer;
[0007] The N electrode comprises an electrode mirror layer, an electrode inner layer and an electrode outer layer;
[0008] The electrode mirror layer is adapted to the shape of the GaAs ohmic contact ring, and the electrode mirror layer is completely embedded in the GaAs ohmic contact ring, and the lower surface of the electrode mirror layer is in contact with the upper surface of the roughening layer;
[0009] The electrode inner layer covers the outer surface of the GaAs ohmic contact ring embedded with the electrode mirror layer, and the electrode inner layer adopts a multi-layer structure, wherein a core layer is made of AlCu;
[0010] The electrode outer layer is covered on the outer surface of the electrode inner layer.
[0011] Further, the preparation material of the inner layer of the electrode includes Au, AuGe, Ti, AlCu and Al which are sequentially evaporated, and the thicknesses thereof are 200 angstroms, 1000 angstroms, 100 angstroms, 3.5 microns and 0.5 microns respectively;
[0012] The mass percentage of Cu in the AlCu material is 2% to 5%.
[0013] Further, the preparation material of the outer layer of the electrode includes Ti and Au evaporated in sequence, and the thicknesses thereof are 100 angstroms and 3000 angstroms respectively;
[0014] The preparation material of the electrode mirror layer includes Ag and TiW which are evaporated in sequence, and the thicknesses thereof are 3000 angstroms and 200 angstroms respectively.
[0015] Further, the GaAs ohmic contact ring is in the shape of a square ring, a circular ring or an elliptical ring;
[0016] The ring width of the GaAs ohmic contact ring is 5 to 7 microns;
[0017] The upper surface of the electrode mirror layer is flush with the upper surface of the GaAs ohmic contact ring.
[0018] Furthermore, the dielectric film layer has a plurality of through holes, and ohmic contact blocks are arranged in the through holes;
[0019] The silver mirror layer has a plurality of bumps, the bumps are adapted to the shape of the through holes and embedded in the through holes, the tops of the bumps have grooves, the shape of the ohmic contact blocks is adapted to the grooves, and the ohmic contact blocks are embedded in the grooves;
[0020] The upper surface of the ohmic contact block contacts the lower surface of the GaP window layer.
[0021] Further, the size of the through hole is 10 microns to 12 microns; the size of the ohmic contact block is 1 / 4 to 1 / 2 of the size of the through hole;
[0022] The thickness of the ohmic contact block is 0.3 micrometers;
[0023] The thickness of the dielectric film layer is 5000 angstroms.
[0024] Further, the thickness of the silver mirror layer is 3000 angstroms;
[0025] The barrier layer is prepared from materials including Ti, Pt, Au, Ti and Ni which are sequentially evaporated, and the thicknesses thereof are 200 angstroms, 200 angstroms, 2000 angstroms, 100 angstroms and 1000 angstroms respectively.
[0026] Further, the preparation material of the first bonding layer includes Ti, Pt and Au deposited in sequence, and the thicknesses thereof are 200 angstroms, 200 angstroms and 2000 angstroms respectively;
[0027] The second bonding layer is made of In, and has a thickness of 3 micrometers.
[0028] Furthermore, the chip sidewall has a cutting path etched from the chip upper surface to the GaP window layer, and the surface of the cutting path is covered with a passivation layer;
[0029] The passivation layer is made of silicon nitride or silicon oxide.
[0030] Another aspect of the present invention is to provide a method for manufacturing the above-mentioned reverse polarity red LED chip, the manufacturing method comprising:
[0031] S1, providing a GaAs substrate as a growth substrate for a reverse polarity red light epitaxial structure;
[0032] S2, sequentially growing an N-type semiconductor layer, a light-emitting layer, a P-type semiconductor layer and a GaP window layer on a GaAs substrate;
[0033] S3, using PECVD to deposit silicon dioxide on the surface of the GaP window layer to prepare a dielectric film layer;
[0034] S4. Use a negative resist mask to produce a patterned conductive hole pattern, the size of which is 4 to 6 microns. Use a fluorine-containing solution to etch away the dielectric film material in the conductive hole, and perform water flushing and high spin. Use electron beam evaporation cold plating to evaporate ohmic contact blocks in the conductive hole, and use a negative resist stripping process to complete the ohmic contact block production;
[0035] S5, using positive resist to make a patterned through-hole pattern, the through-hole pattern is aligned with the conductive hole pattern, the through-hole size is 10 microns to 12 microns, and a fluorine-containing solution is used to etch away the dielectric film material in the through-hole by wet etching;
[0036] S6, sputtering a silver mirror layer on the surface by sputtering, and then plating a barrier layer;
[0037] S7, evaporating a second bonding layer on the surface by electron beam evaporation;
[0038] S8, performing electron beam evaporation on the prepared Si substrate to form a first bonding layer;
[0039] S9, attaching the second bonding layer and the first bonding layer of the epitaxial wafer together to complete the bonding between the two;
[0040] S10, placing the bonded source into a mixed solution of ammonia and hydrogen peroxide, removing the GaAs substrate by chemical etching to expose the N-type semiconductor layer;
[0041] S11, using a negative resist mask, a patterned GaAs ohmic contact ring pattern is produced, and the GaAs ohmic contact layer is etched by a mixture of phosphoric acid, hydrogen peroxide and water, and then rinsed and high-spinned; using a sputtering method, an electrode mirror layer is prepared, and a negative resist stripping process is used to complete the production of the electrode mirror layer;
[0042] S12, using a negative resist mask to produce a patterned electrode inner layer pattern, the size of the electrode inner layer pattern is larger than the size of the GaAs ohmic contact ring pattern, using electron beam evaporation to evaporate the electrode inner layer, and completing the electrode inner layer production through a negative resist stripping process;
[0043] S13, using a negative resist mask to produce a patterned electrode outer layer pattern, the size of the electrode outer layer pattern is larger than the size of the electrode inner layer pattern, using electron beam evaporation to evaporate the electrode outer layer, and completing the electrode outer layer production through a negative resist stripping process;
[0044] S14, using positive resist to make cutting path patterns, and using dry etching to etch the cutting paths;
[0045] S15, using positive resist to make a roughening layer protection pattern, and performing surface roughening by wet etching;
[0046] S16, depositing a passivation layer by PECVD, patterning the passivation layer by positive resist, and completing the passivation layer fabrication by wet etching;
[0047] S17. The LED chip is manufactured by thinning the Si substrate, making the P electrode, and laser cutting.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] 1. The reverse polarity red LED chip provided by the present application adopts a new electrode structure with a GaAs ohmic contact ring structure design. On the one hand, the GaAs ohmic contact ring can guide the current to diffuse from the bottom of the N electrode to the surrounding area, reducing the current from the bottom of the N electrode to the light-emitting layer to emit light; the electrode mirror layer embedded in the GaAs ohmic contact ring has a flat surface, so that the light emitted by the light-emitting layer and directed to the N electrode can be effectively reflected back to avoid electrode absorption and increase the probability of light emission. On the other hand, the AlCu alloy material added to the inner layer of the electrode and the GaAs ohmic contact ring arranged around the electrode mirror layer can provide protection for the electrode mirror layer, effectively resist the impact force of the wire welding process, stabilize the structure of the electrode mirror layer, and avoid the impact force of the wire welding process or external impact force causing damage to the electrode mirror layer.
[0050] 2. The N electrode adopts a structure that is coated layer by layer with an electrode outer layer, an electrode inner layer and an electrode mirror layer. The electrode inner layer is preset first. The electrode inner layer adopts Au, AuGe, Ti, AlCu and Al which are evaporated in sequence, and is mainly made of AlCu material, which is low in cost. The thickness of the electrode inner layer can be set very thick, which can effectively resist the impact force of the wire welding process and maintain the original shape of the electrode. The electrode outer layer is set on the periphery. The electrode outer layer is mainly made of thinner Au, which can ensure solderability (the gold layer can be effectively fused with the solder ball) on the one hand, and effectively protect the stability of the material of the electrode inner layer on the other hand.
[0051] 3. In the present application, a smaller ohmic contact block is arranged in a larger through hole, and the ohmic contact block is embedded in the groove on the top of the bump, so that the silver mirror material can cover the surrounding and lower surface of the ohmic contact block at the same time, significantly increasing the contact area between the ohmic contact block and the silver mirror layer, and ensuring the effective electrical connection between the silver mirror layer and the ohmic contact block; at the same time, the structural design does not need to increase the size of the ohmic contact block, so it will not cause a large area of epitaxial material to be rough, and can provide a relatively flat substrate for the preparation of the silver mirror layer, thereby ensuring that the prepared silver mirror layer has a good optical reflection effect.
[0052] 4. When the patterned GaAs ohmic contact layer is produced, the electrode mirror layer is produced by negative photoresist stripping. The preparation method is simple and easy to operate, and the prepared electrode mirror layer has a stable structure. The inner electrode is mainly made of low-cost metal, and the inner electrode and the outer electrode are produced separately, so that the outer electrode can fully cover the inner electrode, reducing the influence of external temperature, water vapor and chemical substances on the inner electrode, thereby reducing the production cost while ensuring stable performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0054] Figure 1 This is a schematic diagram of the structure of a reverse polarity red LED chip shown in some embodiments of the present application;
[0055] Figure 2 for Figure 1 A partial enlarged view of the middle A area;
[0056] Figure 3 This is a schematic diagram of the epitaxial structure of a reverse polarity red LED shown in some embodiments of the present application;
[0057] Figure 4This is a schematic diagram of a structure in which a dielectric film layer and a conductive hole are formed on a reverse polarity red light LED epitaxial structure as shown in some embodiments of the present application;
[0058] Figure 5 A schematic diagram of a structure for forming a through hole in a reverse polarity red LED epitaxial structure shown in some embodiments of the present application;
[0059] Figure 6 A schematic structural diagram showing another perspective of a through hole formed in a reverse polarity red LED epitaxial structure according to some embodiments of the present application;
[0060] Figure 7 A schematic diagram of a structure for forming a second bonding layer for a reverse polarity red LED epitaxial structure shown in some embodiments of the present application;
[0061] Figure 8 A schematic diagram of the structure of forming a GaAs ohmic contact ring and an electrode mirror layer in a reverse polarity red LED epitaxial structure shown in some embodiments of the present application;
[0062] Fig. 9 A schematic structural diagram of another perspective of forming a GaAs ohmic contact ring and an electrode mirror layer in a reverse polarity red LED epitaxial structure shown in some embodiments of the present application;
[0063] Fig.10 A schematic diagram of a structure for forming an N electrode in a reverse polarity red LED epitaxial structure as shown in some embodiments of the present application;
[0064] Description of the drawings: 1. GaAs substrate; 2. N-type semiconductor layer; 3. Light-emitting layer; 4. P-type semiconductor layer; 5. GaP window layer; 6. Dielectric film layer; 7. Ohmic contact block; 8. Silver mirror layer; 9. Barrier layer; 10. First bonding layer; 11. Si substrate; 12. Second bonding layer; 13. N-electrode; 14. Electrode mirror layer; 15. Electrode inner layer; 16. Electrode outer layer; 17. Passivation layer; 18. P-electrode; 19. N-type limiting layer; 20. Current spreading layer; 21. Roughening layer; 22. GaAs ohmic contact layer; 23. GaAs ohmic contact ring; 24. Through hole; 25. Bump; 27. Conductive hole. DETAILED DESCRIPTION
[0065] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application or use. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0066] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values of the parts and steps set forth in these embodiments do not limit the scope of the present application. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so that once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.
[0067] In the description of the present application, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present application.
[0068] In the description of the present application, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present application and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction, and therefore cannot be understood as limiting the scope of protection of the present application; the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.
[0069] The present application is further described in detail below with reference to specific embodiments:
[0070] Example 1
[0071] The reverse polarity red LED chip provided in this embodiment, Figure 1 This is a schematic diagram of the structure of a reverse polarity red LED chip shown in some embodiments of the present application; Figure 2 for Figure 1 Specifically, the structure provided by this application is as follows, please refer to Figure 1 and Figure 2, a reverse polarity red light LED chip, comprising a P electrode 18, a Si substrate 11, a first bonding layer 10, a second bonding layer 12, a barrier layer 9, a silver mirror layer 8, a dielectric film layer 6, a GaP window layer 5, a P-type semiconductor layer 4, a light-emitting layer 3, an N-type semiconductor layer 2 and an N-electrode 13 arranged in sequence from bottom to top; the N-type semiconductor layer 2 comprises an N-type limiting layer 19, a current spreading layer 20, a roughening layer 21 arranged in sequence from bottom to top, and a GaAs ohmic contact ring 23 arranged on the upper surface of the roughening layer 21; the N-electrode 13 comprises an electrode mirror layer 14, an electrode The inner layer 15 and the electrode outer layer 16; the electrode mirror layer 14 is adapted to the shape of the GaAs ohmic contact ring 23, and the electrode mirror layer 14 is completely embedded in the GaAs ohmic contact ring 23, and the lower surface of the electrode mirror layer 14 is in contact with the upper surface of the roughened layer 21; the electrode inner layer 15 covers the outer surface of the GaAs ohmic contact ring 23 embedded with the electrode mirror layer 14; the electrode inner layer 15 adopts a multi-layer structure, in which a core layer is made of AlCu, and the electrode outer layer 16 covers the outer surface of the electrode inner layer 15.
[0072] The present application adopts a novel electrode structure in combination with a GaAs ohmic contact ring 23 structural design. On the one hand, the GaAs ohmic contact ring 23 can guide the current to diffuse from directly below the N electrode 13 to the surrounding area, reduce the current from directly below the N electrode 13 to enter the light-emitting layer 3 to emit light, and prepare the electrode mirror layer 14 in an embedded manner in the GaAs ohmic contact ring 23, so that a flat electrode mirror layer 14 can be obtained, thereby effectively reflecting the light emitted by the light-emitting layer 3 and directed to the N electrode 13, avoiding electrode absorption, and increasing the probability of light emission. On the other hand, the AlCu alloy material added to the electrode inner layer 15 (Cu has a higher hardness than the traditional electrode material Au) and the GaAs ohmic contact ring 23 arranged around the electrode mirror layer 14 can provide protection for the electrode mirror layer 14, effectively resist the impact force of the wire welding process, stabilize the structure of the electrode mirror layer 14, and avoid the impact force of the wire welding process or external impact force causing damage to the electrode mirror layer 14.
[0073] The shape and arrangement position of the N electrode 13 of the present application can be set according to the existing reverse polarity red light LED, and its shape can be, for example, circular, elliptical, positive direction, rectangular, etc., preferably circular. Correspondingly, the electrode mirror layer 14, the electrode inner layer 15 and the electrode outer layer 16 are all circular, and the sizes of the electrode mirror layer 14, the electrode inner layer 15 and the electrode outer layer 16 increase successively.
[0074] According to some preferred embodiments, the preparation material of the electrode inner layer 15 includes Au, AuGe, Ti, AlCu and Al evaporated in sequence, and the thicknesses thereof are 200 angstroms, 1000 angstroms, 100 angstroms, 3.5 microns and 0.5 microns respectively; the mass percentage of Cu in the AlCu material is 2% to 5%, the preparation material of the electrode outer layer 16 includes Ti and Au evaporated in sequence, and the thicknesses thereof are 100 angstroms and 3000 angstroms respectively; the preparation material of the electrode mirror layer 14 includes Ag and TiW evaporated in sequence, and the thicknesses thereof are 3000 angstroms and 200 angstroms respectively. The N electrode 13 of the present application adopts a structure in which an electrode outer layer 16, an electrode inner layer 15 and an electrode mirror layer 14 are coated layer by layer. By adjusting the electrode structure, the electrode inner layer 15 is preset first. The electrode inner layer 15 adopts Au, AuGe, Ti, AlCu and Al evaporated in sequence, and is mainly made of AlCu material, which is low in cost. The thickness of the electrode inner layer 15 can be set to be very thick, which can effectively resist the impact force of the wire welding process and maintain the original shape of the electrode. The electrode outer layer 16 is arranged on the periphery. The electrode outer layer 16 is mainly made of thinner Au, which on the one hand ensures solderability (the gold layer can be effectively fused with the solder ball), and on the other hand can effectively protect the stability of the material of the electrode inner layer 15.
[0075] In the present application, the shape of the GaAs ohmic contact ring 23 is adapted to the shape of the N electrode 13. According to some preferred embodiments, the shape of the GaAs ohmic contact ring 23 is a square ring, a circular ring or an elliptical ring; the ring width of the GaAs ohmic contact ring 23 is 5 microns to 7 microns, and the upper surface of the electrode mirror layer 14 is flush with the upper surface of the GaAs ohmic contact ring 23.
[0076] According to some preferred embodiments, the dielectric film layer 6 has a plurality of through holes 24, and an ohmic contact block 7 is arranged in the through hole 24; the silver mirror layer 8 has a plurality of bumps 25, and the bumps 25 are adapted to the shape of the through holes 24 and embedded in the through holes 24, and the top of the bump 25 has a groove, and the shape of the ohmic contact block 7 is adapted to the groove, and the ohmic contact block 7 is embedded in the groove; the upper surface of the ohmic contact block 7 is in contact with the lower surface of the GaP window layer 5.
[0077] The ohmic contact blocks 7 are regularly arranged on the dielectric film layer 6 except for the area directly below the N-electrode 13, so as to avoid the current gathering directly below the N-electrode 13, thereby making the current evenly distributed around and making the chip brightness more uniform.
[0078] The size of the through hole 24 is 10 microns to 12 microns; the size of the ohmic contact block 7 is 1 / 4 to 1 / 2 of the size of the through hole 24, and the center of the ohmic contact block 7 coincides with the center of the through hole 24; the thickness of the ohmic contact block 7 is 0.3 microns; the thickness of the dielectric film layer 6 is 5000 angstroms.
[0079] Ohmic contact materials can cause the surface of epitaxial materials to be rough, so the through holes 24 and ohmic contact blocks 7 on the dielectric film layer 6 are usually made relatively small, which can cause the ohmic contact material deposited in the through holes 24 to be suspended or have poor contact with the silver mirror layer 8. The present application sets a smaller ohmic contact block 7 in a larger through hole 24, and embeds the ohmic contact block 7 into the groove at the top of the bump 25, so that the silver mirror material can cover the surroundings and the lower surface of the ohmic contact block 7 at the same time, significantly increasing the contact area between the ohmic contact block 7 and the silver mirror layer 8, and ensuring the effective electrical connection between the silver mirror layer 8 and the ohmic contact block 7; at the same time, the structural design does not need to enlarge the size of the ohmic contact block 7, will not cause a large area of epitaxial material to be rough, and can provide a relatively flat substrate for the preparation of the silver mirror layer 8, thereby ensuring that the prepared silver mirror layer 8 has a good optical reflection effect.
[0080] According to some preferred embodiments, the thickness of the silver mirror layer 8 is 3000 angstroms;
[0081] The barrier layer 9 can ensure the stability of the silver mirror layer 8. According to some preferred embodiments, the barrier layer 9 is made of materials including Ti, Pt, Au, Ti and Ni evaporated in sequence, with thicknesses of 200 angstroms, 200 angstroms, 2000 angstroms, 100 angstroms and 1000 angstroms, respectively.
[0082] According to some preferred embodiments, the preparation material of the first bonding layer 10 includes Ti, Pt and Au evaporated in sequence, and the thicknesses thereof are 200 angstroms, 200 angstroms and 2000 angstroms respectively; the preparation material of the second bonding layer 12 is In, and the thickness of the second bonding layer 12 is 3 microns.
[0083] According to some preferred embodiments, the chip sidewall has a cutting path etched from the chip upper surface to the GaP window layer 5, and the surface of the cutting path is covered with a passivation layer 17; the passivation layer 17 is made of silicon nitride or silicon oxide.
[0084] From the above, it can be seen that the reverse polarity red LED chip provided in the embodiment of the present application has the following advantages:
[0085] 1. The reverse polarity red LED chip provided by the present application adopts a new electrode structure with a GaAs ohmic contact ring structure design. On the one hand, the GaAs ohmic contact ring can guide the current to diffuse from the N electrode directly below to the surrounding area, reducing the current from the N electrode directly below to the light-emitting layer 3 to emit light. The electrode mirror layer embedded in the GaAs ohmic contact ring can prepare a flat electrode mirror layer, so that the light emitted by the light-emitting layer and directed to the N electrode can be effectively reflected back to avoid electrode absorption and increase the probability of light emission. On the other hand, the AlCu alloy material with a higher hardness added to the inner layer of the electrode and the GaAs ohmic contact ring arranged around the electrode mirror layer can provide protection for the electrode mirror layer, which can effectively resist the impact force of the wire bonding process, stabilize the electrode mirror layer structure, and avoid the impact force of the wire bonding process or external impact force causing damage to the electrode mirror layer.
[0086] 2. The N electrode of the present application adopts a structure in which an electrode outer layer, an electrode inner layer and an electrode mirror layer are coated layer by layer. By adjusting the electrode structure, the electrode inner layer is preset first. The electrode inner layer adopts Au, AuGe, Ti, AlCu and Al which are sequentially evaporated, and is mainly made of AlCu material, which is low in cost. The thickness of the electrode inner layer can be set very thick, which can effectively resist the impact force of the wire welding process and maintain the original shape of the electrode. The electrode outer layer is arranged on the periphery, and the electrode outer layer is mainly made of thinner Au. On the one hand, it ensures solderability (the gold layer can be effectively fused with the solder ball), and on the other hand, it can effectively protect the stability of the material of the electrode inner layer.
[0087] 3. In the present application, a smaller ohmic contact block is arranged in a larger through hole, and the ohmic contact block is embedded in the groove on the top of the bump, so that the silver mirror material can cover the surrounding and lower surface of the ohmic contact block at the same time, thereby significantly increasing the contact area between the ohmic contact block and the silver mirror layer, and ensuring the effective electrical connection between the silver mirror layer and the ohmic contact block; at the same time, the structural design does not need to increase the size of the ohmic contact block, so it will not cause a large area of epitaxial material to be rough, and can provide a relatively flat substrate for the preparation of the silver mirror layer, thereby ensuring that the prepared silver mirror layer has a good optical reflection effect.
[0088] Example 2
[0089] Please combine Figures 1 to 10 This embodiment provides a method for manufacturing a reverse polarity red LED chip, the manufacturing method comprising:
[0090] Step 1: Please combine Figure 3 , Figure 3The figure shows a schematic diagram of the epitaxial structure of a reverse polarity red light LED chip; a GaAs substrate 1 is provided as a growth substrate for the reverse polarity red light epitaxial structure, a program is set on a MOCVD machine, and an N-type semiconductor layer 2, a light-emitting layer 3, a P-type semiconductor layer 4 and a GaP window layer 5 are sequentially grown on the GaAs substrate 1; the N-type semiconductor layer 2 includes a GaAs ohmic contact layer 22, a roughening layer 21, a current spreading layer 20 and an N-type limiting layer 19;
[0091] As a preferred embodiment, the thickness of the GaP window layer 5 is 0.5 microns to 1.5 microns;
[0092] Step 2: Please combine Figure 4 , Figure 4 The schematic diagram of the structure of forming a dielectric film layer and a conductive hole on the reverse polarity red light LED epitaxial structure shown in some embodiments of the present application; the epitaxial wafer is cleaned with an acid-base solution, and silicon dioxide is deposited on the surface of the GaP window layer 5 on the surface of the epitaxial wafer by PECVD to prepare a dielectric film layer 6; a patterned conductive hole 27 pattern is produced by using a negative resist mask, and the size of the conductive hole 27 is 4 microns to 6 microns, and the dielectric film material in the conductive hole 27 is etched away by a fluorine-containing solution, and water flushing and high spin are performed, and further an ohmic contact block 7 is evaporated in the conductive hole 27 by electron beam evaporation cold plating, and the ohmic contact block 7 is completed by a negative resist stripping process;
[0093] As a preferred embodiment, the thickness of the dielectric film layer 6 is 5000 angstroms, the material of the ohmic contact block 7 is Au, AuZn (or AuBe) and Au deposited in sequence, and the thickness of the ohmic contact block 7 is 0.3 microns;
[0094] Step 3: Please combine Figure 5 and Figure 6 , Figure 5 This is a schematic diagram of a structure in which a through hole is formed in an epitaxial structure of a reverse polarity red light LED as shown in some embodiments of the present application. Figure 6 Another perspective structural diagram of the through hole formed in the reverse polarity red LED epitaxial structure shown in some embodiments of the present application; the patterned through hole 24 pattern is made by positive resist lithography, the through hole 24 pattern is aligned with the conductive hole 27 pattern, the through hole 24 size is 10 microns to 12 microns, and the dielectric film material in the through hole 24 is further etched away by wet etching using a fluorine-containing solution;
[0095] Step 4: Please combine Figure 7 , Figure 7 A schematic diagram of a structure for forming a second bonding layer for a reverse polarity red LED epitaxial structure shown in some embodiments of the present application; the surface is cleaned with an organic solution, a silver mirror layer 8 is sputtered on the surface by sputtering, and a barrier layer 9 is further plated; the surface is cleaned with an organic solution, and a second bonding layer 12 is evaporated on the surface by electron beam evaporation;
[0096] As a preferred embodiment, the barrier layer 9 is made of materials including Ti, Pt, Au, Ti and Ni which are sequentially evaporated, and the thicknesses thereof are 200 angstroms, 200 angstroms, 2000 angstroms, 100 angstroms and 1000 angstroms respectively.
[0097] As a preferred embodiment, the second bonding layer 12 is made of In, and the thickness of the second bonding layer 12 is 3 micrometers.
[0098] Please combine the following steps 5 to 8 Figure 8 and Fig. 9 , Figure 8 A schematic diagram of the structure of forming a GaAs ohmic contact ring and an electrode mirror layer in a reverse polarity red LED epitaxial structure shown in some embodiments of the present application; Fig. 9 A schematic structural diagram of another perspective of forming a GaAs ohmic contact ring and an electrode mirror layer in a reverse polarity red LED epitaxial structure shown in some embodiments of the present application;
[0099] Step 5: The prepared Si substrate 11 is subjected to electron beam evaporation to complete the evaporation of the first bonding layer 10;
[0100] As a preferred embodiment, the preparation material of the first bonding layer 10 includes Ti, Pt and Au deposited in sequence, and the thicknesses thereof are 200 angstroms, 200 angstroms and 2000 angstroms respectively;
[0101] Step 6: Paste the second bonding layer 12 and the first bonding layer 10 of the epitaxial wafer together, place them in a special bonding fixture, put them into a bonding machine, and complete the bonding of the two by low temperature and low pressure;
[0102] As a preferred embodiment, the bonding of the two is completed at a low temperature of 200°C and a low pressure of 2000kgf;
[0103] Step 7: Place the bonded source into a mixed solution of ammonia and hydrogen peroxide, remove the GaAs substrate 1 by chemical etching, and expose the N-type semiconductor layer 2;
[0104] Step 8: A patterned GaAs ohmic contact ring 23 is produced by using a negative resist mask, and the GaAs ohmic contact layer 22 is etched by using a mixture of phosphoric acid, hydrogen peroxide and water, and then subjected to water high spin washing; further, the electrode mirror layer 14 is sputtered and evaporated by using a sputtering method, and the electrode mirror layer 14 is produced by using a negative resist stripping process;
[0105] As a preferred embodiment, the electrode mirror layer 14 is made of materials including Ag and TiW which are sequentially evaporated, and the thicknesses thereof are 3000 angstroms and 200 angstroms respectively.
[0106] Please combine the following steps nine to ten Fig.10 , Fig.10 This is a schematic diagram of a structure in which an N electrode is formed in a reverse polarity red LED epitaxial structure as shown in some embodiments of the present application;
[0107] Step nine, a patterned electrode inner layer 15 pattern is produced by using a negative resist mask, the pattern size of the electrode inner layer 15 pattern is larger than the pattern size of the GaAs ohmic contact ring 23, the electrode inner layer 15 is evaporated by electron beam evaporation, and the electrode inner layer 15 is produced by a negative resist stripping process, and high-temperature fusion is performed at 280° C. to 320° C.;
[0108] As a preferred embodiment, the preparation material of the electrode inner layer 15 includes Au, AuGe, Ti, AlCu and Al evaporated in sequence, and the thicknesses thereof are 200 angstroms, 1000 angstroms, 100 angstroms, 3.5 microns and 0.5 microns respectively; the mass percentage of Cu in the AlCu material is 2% to 5%.
[0109] Step 10: Using a negative resist mask, a patterned electrode outer layer 16 is produced. The size of the electrode outer layer 16 is larger than that of the electrode inner layer 15. The electrode outer layer 16 is deposited by electron beam evaporation, and the negative resist stripping process is used to complete the production of the electrode outer layer 16.
[0110] As a preferred embodiment, the preparation material of the electrode outer layer 16 includes Ti and Au deposited in sequence, and the thicknesses thereof are 100 angstroms and 3000 angstroms respectively;
[0111] Please combine the following steps 11 to 14 Figure 1 and Figure 2 , Figure 1 This is a schematic diagram of the structure of a reverse polarity red LED chip shown in some embodiments of the present application; Figure 2 for Figure 1 A partial enlarged view of the middle A area;
[0112] Step 11: Use positive resist to make cutting path patterns, and use dry etching to etch the cutting paths until 5000 angstroms remain on the GaP window layer 5;
[0113] Step 12: Use positive resist to make a roughening layer 21 to protect the pattern, and perform surface roughening by wet etching;
[0114] Step 13: clean the wafer organically, deposit the passivation layer 17 by PECVD, pattern the passivation layer 17 by positive resist, and complete the passivation layer 17 by wet etching;
[0115] Step 14: Thin the Si substrate 11, make the P electrode 18, and complete the LED chip manufacturing by laser cutting.
[0116] From the above, it can be seen that the method for manufacturing the reverse polarity red LED chip provided in the embodiment of the present application has the following advantages:
[0117] 1. The preparation method provided in the present application is to complete the ohmic contact block production by evaporation stripping after the first conductive hole pattern is etched; the second dielectric film through-hole pattern is aligned with the first one to etch a larger through-hole; the first smaller conductive hole forms an ohmic contact block with a smaller pattern, so that the ohmic contact metal and the GaP window layer have a smaller contact area (ohmic contact will make the surface rough, which is not conducive to the production of a flat Ag mirror surface); the second through-hole is etched larger to allow an effective connection between the Ag mirror surface and the ohmic contact metal, avoiding the problem of suspended contact or breakage at the step due to the through-hole size being too small, thereby ensuring the optical effect while also ensuring the electrical characteristics.
[0118] 2. When the patterned GaAs ohmic contact layer is produced, the electrode mirror layer is produced by negative photoresist stripping. The preparation method is simple and easy to operate, and the prepared electrode mirror layer has a stable structure. The inner electrode is mainly made of low-cost metal, and by producing the inner electrode and the outer electrode separately, the outer electrode can fully cover the inner electrode, reducing the influence of external temperature, water vapor and chemical substances on the inner electrode, thereby reducing the production cost while ensuring stable performance.
[0119] Since the method for manufacturing the reverse polarity red LED chip provided in the embodiment of the present application obtains the reverse polarity red LED chip in the above embodiment 1, it also has the advantages of the reverse polarity red LED chip in the above embodiment 1, which will not be elaborated here.
[0120] For content not described in this embodiment, please refer to the relevant description in the rest of this application.
[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application and not to limit it. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present application can still be modified or some technical features can be replaced by equivalents, which should all be included in the scope of the technical solution requested for protection in this application.
Claims
1. A reverse polarity red LED chip, characterized in that: The invention comprises a P electrode, a Si substrate, a first bonding layer, a second bonding layer, a barrier layer, a silver mirror layer, a dielectric film layer, a GaP window layer, a P-type semiconductor layer, a light-emitting layer, an N-type semiconductor layer and an N-electrode which are sequentially arranged from bottom to top; the N-type semiconductor layer comprises an N-type limiting layer, a current spreading layer, a roughening layer which are sequentially arranged from bottom to top, and a GaAs ohmic contact ring which is arranged on the upper surface of the roughening layer; The N electrode comprises an electrode mirror layer, an electrode inner layer and an electrode outer layer; The electrode mirror layer is adapted to the shape of the GaAs ohmic contact ring, and the electrode mirror layer is completely embedded in the GaAs ohmic contact ring, and the lower surface of the electrode mirror layer is in contact with the upper surface of the roughening layer; the preparation material of the electrode mirror layer includes Ag and TiW evaporated in sequence; The electrode inner layer covers the outer surface of the GaAs ohmic contact ring embedded with the electrode mirror layer, and the electrode inner layer adopts a multilayer structure, wherein a core layer is made of AlCu; The electrode outer layer covers the outer surface of the electrode inner layer; The dielectric film layer has a plurality of through holes, and ohmic contact blocks are arranged in the through holes; The silver mirror layer has a plurality of bumps, the bumps are adapted to the shape of the through holes and embedded in the through holes, the tops of the bumps have grooves, the shape of the ohmic contact blocks is adapted to the grooves, and the ohmic contact blocks are embedded in the grooves; The upper surface of the ohmic contact block contacts the lower surface of the GaP window layer.
2. The reverse polarity red LED chip according to claim 1, characterized in that: The preparation material of the inner layer of the electrode includes Au, AuGe, Ti, AlCu and Al which are sequentially evaporated, and the thicknesses thereof are 200 angstroms, 1000 angstroms, 100 angstroms, 3.5 microns and 0.5 microns respectively; The mass percentage of Cu in the AlCu material is 2% to 5%.
3. The reverse polarity red LED chip according to claim 1, characterized in that: The preparation material of the outer layer of the electrode includes Ti and Au which are sequentially evaporated, and the thicknesses thereof are 100 angstroms and 3000 angstroms respectively; The preparation material of the electrode mirror layer includes Ag and TiW which are evaporated in sequence, and the thicknesses thereof are 3000 angstroms and 200 angstroms respectively.
4. The reverse polarity red LED chip according to claim 1, characterized in that: The GaAs ohmic contact ring is in the shape of a square ring, a circular ring or an elliptical ring; The ring width of the GaAs ohmic contact ring is 5 to 7 microns; The upper surface of the electrode mirror layer is flush with the upper surface of the GaAs ohmic contact ring.
5. The reverse polarity red LED chip according to claim 1, characterized in that: The size of the through hole is 10 microns to 12 microns; the size of the ohmic contact block is 1 / 4 to 1 / 2 of the size of the through hole; The thickness of the ohmic contact block is 0.3 micrometers; The thickness of the dielectric film layer is 5000 angstroms.
6. The reverse polarity red LED chip according to claim 1, characterized in that: The thickness of the silver mirror layer is 3000 angstroms; The barrier layer is prepared from materials including Ti, Pt, Au, Ti and Ni which are sequentially evaporated, and the thicknesses thereof are 200 angstroms, 200 angstroms, 2000 angstroms, 100 angstroms and 1000 angstroms respectively.
7. The reverse polarity red LED chip according to claim 1, characterized in that: The preparation material of the first bonding layer includes Ti, Pt and Au deposited in sequence, and the thicknesses thereof are 200 angstroms, 200 angstroms and 2000 angstroms respectively; The second bonding layer is made of In, and has a thickness of 3 micrometers.
8. The reverse polarity red LED chip according to claim 1, characterized in that: The chip sidewall has a cutting path etched from the chip upper surface to the GaP window layer, and the surface of the cutting path is covered with a passivation layer; The passivation layer is made of silicon nitride or silicon oxide.
9. A method for manufacturing a reverse polarity red LED chip as claimed in any one of claims 1 to 8, characterized in that: The production method comprises: S1, providing a GaAs substrate as a growth substrate for a reverse polarity red light epitaxial structure; S2, sequentially growing an N-type semiconductor layer, a light-emitting layer, a P-type semiconductor layer and a GaP window layer on a GaAs substrate; S3, using PECVD to deposit silicon dioxide on the surface of the GaP window layer to prepare a dielectric film layer; S4. Use a negative resist mask to produce a patterned conductive hole pattern, the size of which is 4 to 6 microns. Use a fluorine-containing solution to etch away the dielectric film material in the conductive hole, and perform water flushing and high spin. Use electron beam evaporation cold plating to evaporate ohmic contact blocks in the conductive hole, and use a negative resist stripping process to complete the ohmic contact block production; S5, using positive resist to make a patterned through-hole pattern, the through-hole pattern is aligned with the conductive hole pattern, the through-hole size is 10 microns to 12 microns, and a fluorine-containing solution is used to etch away the dielectric film material in the through-hole by wet etching; S6, sputtering a silver mirror layer on the surface by sputtering, and then plating a barrier layer; S7, evaporating a second bonding layer on the surface by electron beam evaporation; S8, performing electron beam evaporation on the prepared Si substrate to form a first bonding layer; S9, attaching the second bonding layer and the first bonding layer of the epitaxial wafer together to complete the bonding between the two; S10, placing the bonded source into a mixed solution of ammonia and hydrogen peroxide, removing the GaAs substrate by chemical etching to expose the N-type semiconductor layer; S11, using a negative resist mask, a patterned GaAs ohmic contact ring pattern is produced, and the GaAs ohmic contact layer is etched by a mixture of phosphoric acid, hydrogen peroxide and water, and then rinsed and high-spinned; using a sputtering method, an electrode mirror layer is prepared, and a negative resist stripping process is used to complete the production of the electrode mirror layer; S12, using a negative resist mask to produce a patterned electrode inner layer pattern, the size of the electrode inner layer pattern is larger than the size of the GaAs ohmic contact ring pattern, using electron beam evaporation to evaporate the electrode inner layer, and completing the electrode inner layer production through a negative resist stripping process; S13, using a negative resist mask to produce a patterned electrode outer layer pattern, the size of the electrode outer layer pattern is larger than the size of the electrode inner layer pattern, using electron beam evaporation to evaporate the electrode outer layer, and completing the electrode outer layer production through a negative resist stripping process; S14, using positive resist to make cutting path patterns, and using dry etching to etch the cutting paths; S15, using positive resist to make a roughening layer protection pattern, and performing surface roughening by wet etching; S16, depositing a passivation layer by PECVD, patterning the passivation layer by positive resist, and completing the passivation layer fabrication by wet etching; S17. The LED chip is manufactured by thinning the Si substrate, making the P electrode, and laser cutting.
Citation Information
Patent Citations
Semiconductor light emitting element
CN101901862A
Full coverage type one-time smooth electrode light emitting diode and manufacturing method thereof
CN107248545A