A method for preparing a circuit board substrate and a circuit board substrate
By laminating, electroplating, grooving and heat-treating the circuit board substrate material, a pillar structure is formed, which solves the problem of insufficient heat dissipation and mechanical properties of the existing circuit board substrate, achieves more efficient heat dissipation and processing performance, and is suitable for High power density circuits.
Patent Information
- Application Number
- CN202410931010.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The heat dissipation performance and mechanical processing performance of existing circuit board substrates are insufficient, making it difficult to meet the needs of high power density circuits.
By laminating the base material, copper foil and insulation layer of the circuit board to form the original copper substrate, electroplating and grooving are performed to form a pillar structure, followed by heat treatment and cutting to form a structure with good heat dissipation performance and mechanical properties. Processing performance circuit board substrate.
The heat dissipation performance and mechanical processing performance of the circuit board substrate are improved, which can meet the needs of high power density circuits and extend its service life.
Smart Images

Figure CN118475017B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of circuit boards, and also to a method for preparing a circuit board substrate and the circuit board substrate. Background Art
[0002] With the continuous development of electronic equipment, high-power and high-current electronic equipment are increasingly widely used. With the continuous development of electronic technology, the requirements for circuit boards as carriers of electronic components are getting higher and higher. One of the important points is the requirement for their heat dissipation effect. Therefore, as the most important part of manufacturing circuit boards, the heat dissipation of the substrate is also crucial. At present, the circuit board substrates on the market mainly adopt the traditional manufacturing method, that is, directly bonding the insulating layer on the copper foil, and then cutting and processing. Although this method is simple, it has problems such as poor heat dissipation performance and weak mechanical processing performance, and it is difficult to meet the needs of high power density circuits. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for preparing a circuit board substrate and a circuit board substrate, so as to improve the heat dissipation performance of the circuit board.
[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0005] A first aspect of the present invention provides a method for preparing a circuit board substrate, comprising:
[0006] Provide substrate materials, copper foil and insulation layer for circuit boards;
[0007] The substrate material of the circuit board, the copper foil and the insulating layer are pressed together to obtain an original copper substrate;
[0008] Electroplating the original copper substrate to obtain a copper substrate with a copper-based boss;
[0009] Performing a groove process on the copper substrate with the copper-based boss to obtain a copper substrate with a pillar-type structure;
[0010] Performing heat treatment on the copper substrate of the pillar structure to obtain a heat-treated copper substrate;
[0011] The heat-treated copper substrate is cut according to preset cutting conditions to obtain a circuit board substrate.
[0012] Optionally, laminating the substrate material of the circuit board, the copper foil and the insulating layer to obtain an original copper substrate comprises:
[0013] Pre-treating the substrate material of the circuit board, the copper foil and the insulating layer to obtain the pre-treated substrate material of the circuit board, the pre-treated copper foil and the pre-treated insulating layer;
[0014] The pretreated substrate material of the circuit board, the pretreated copper foil and the pretreated insulating layer are stacked in a preset order, and placed in a laminating machine for laminating according to preset laminating parameters to obtain an original copper substrate.
[0015] Optionally, the original copper substrate is electroplated to obtain a copper substrate with a copper-based boss, comprising:
[0016] Sputtering the original copper substrate to obtain a copper substrate with a copper film;
[0017] Performing photolithography on the copper substrate with the copper film according to a preset pattern to obtain a copper substrate with a photoresist layer;
[0018] Placing the copper substrate with the photoresist layer into an electroplating tank and performing electroplating according to preset electroplating parameters to obtain a copper substrate with copper pillars;
[0019] Immersing the copper substrate with the copper pillars in a cleaning solution for cleaning to obtain the copper substrate with the photoresist layer removed;
[0020] The copper substrate with the photoresist layer removed is subjected to shaping treatment to obtain a copper substrate with a copper-based boss.
[0021] Optionally, the copper substrate with the copper-based boss is grooved to obtain a copper substrate with a pillar structure, comprising:
[0022] Determining a slotting position according to the copper substrate with the copper-based boss;
[0023] A depth-controlled gong machine is used to gong a depth-controlled blind groove at the grooving position to obtain a copper substrate with a pillar-type structure.
[0024] Optionally, heat-treating the copper substrate of the pillar structure to obtain the heat-treated copper substrate includes:
[0025] Performing a first treatment on the copper substrate of the pillar structure according to a preset first treatment condition to obtain a copper substrate after the first treatment;
[0026] Performing annealing treatment on the copper substrate after the first treatment according to preset annealing treatment conditions to obtain an annealed copper substrate;
[0027] The annealed copper substrate is quenched according to preset quenching conditions to obtain a heat-treated copper substrate.
[0028] Optionally, performing a first treatment on the copper substrate of the pillar structure according to a preset first treatment condition to obtain the copper substrate after the first treatment includes:
[0029] Obtaining a preset first processing condition; the preset first processing condition includes: a holding temperature of 800° C. to 900° C., and a holding time of 1 hour to 4 hours;
[0030] According to the preset first processing condition, placing the copper substrate of the pillar structure into a resistance furnace for heat preservation treatment to obtain the copper substrate after heat preservation treatment;
[0031] The copper substrate after the heat preservation treatment is subjected to cooling treatment to obtain the copper substrate after the first treatment.
[0032] Optionally, annealing the copper substrate after the first treatment according to preset annealing conditions to obtain the annealed copper substrate includes:
[0033] Obtaining preset annealing conditions; the preset annealing conditions include: an annealing temperature of any one of 780°C, 650°C to 675°C, and 600°C, and a holding time of 1 hour to 2 hours;
[0034] The copper substrate after the first treatment is placed in an annealing furnace for annealing according to the preset annealing conditions to obtain the annealed copper substrate.
[0035] Optionally, quenching the annealed copper substrate according to preset quenching conditions to obtain a heat-treated copper substrate includes:
[0036] Preheating the annealed copper substrate to obtain a preheated copper substrate;
[0037] Obtaining preset quenching conditions; the preset quenching conditions include: a quenching temperature of 900° C. to 950° C., and a quenching time of 5 seconds to 15 seconds;
[0038] Performing quenching treatment on the preheated copper substrate according to the preset quenching treatment conditions to obtain a quenched copper substrate;
[0039] The quenched copper substrate is repaired to obtain a heat-treated copper substrate.
[0040] Optionally, the heat-treated copper substrate is cut according to preset cutting conditions to obtain a circuit board substrate, including:
[0041] Cleaning the heat-treated copper substrate to obtain a cleaned copper substrate;
[0042] Performing quality inspection on the cleaned copper substrate to obtain a qualified copper substrate;
[0043] The qualified copper substrate is cut according to preset cutting conditions to obtain a circuit board substrate.
[0044] A second aspect of the present invention provides a circuit board substrate, which is prepared by any of the above-mentioned methods for preparing a circuit board substrate.
[0045] The above solution of the present invention includes at least the following beneficial effects:
[0046] The above scheme of the present invention obtains an original copper substrate by laminating the substrate material, copper foil and insulating layer of the circuit board, electroplating and grooving the original copper substrate, forming a pillar structure for heat dissipation on the original copper substrate, and then heat treating and cutting the copper substrate with the pillar structure. The obtained circuit board substrate has the advantages of good heat dissipation performance and strong mechanical processing performance, and can meet the needs of high power density circuits. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 is a schematic flow chart of a method for preparing a circuit board substrate in an embodiment of the present invention;
[0048] Figure 2 It is a schematic structural diagram of a circuit board substrate in an embodiment of the present invention.
[0049] Explanation of the reference numerals: 1-substrate material layer, 2-copper foil layer, 3-insulating layer, 4-copper-based boss, 5-blind groove, 6-component. DETAILED DESCRIPTION
[0050] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0051] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing a circuit board substrate, comprising the following steps:
[0052] Step 101, providing a substrate material, copper foil and an insulating layer of a circuit board;
[0053] Step 102, laminating the substrate material of the circuit board, the copper foil and the insulating layer to obtain an original copper substrate;
[0054] Step 103, electroplating the original copper substrate to obtain a copper substrate with copper-based bosses;
[0055] Step 104, performing a grooving process on the copper substrate with the copper-based bosses to obtain a copper substrate with a pillar-type structure;
[0056] Step 105, heat-treating the copper substrate of the pillar structure to obtain a heat-treated copper substrate;
[0057] Step 106, cutting the heat-treated copper substrate according to preset cutting conditions to obtain a circuit board substrate.
[0058] The preparation method of the circuit board substrate proposed in the embodiment of the present invention comprises the following steps: laminating the substrate material, copper foil and insulating layer of the circuit board to obtain an original copper substrate, electroplating and slotting the original copper substrate, forming a pillar structure for heat dissipation on the original copper substrate, and then heat treating and cutting the copper substrate with the pillar structure. The obtained circuit board substrate has the advantages of good heat dissipation performance and strong mechanical processing performance, can meet the requirements of high power density circuits, improve the quality and stability of the circuit board substrate, and extend its service life.
[0059] In an optional embodiment of the present invention, in step 101, the substrate material of the circuit board can be selected from a FR4 (a composite material of epoxy resin and glass fiber cloth) metal substrate. Other suitable substrate materials for the circuit board can be selected according to the purpose and performance of the circuit board. Copper foil is the conductive layer of the circuit board. The thickness of the copper foil will affect the resistance and current carrying capacity of the circuit board circuit. Therefore, the thickness of the copper foil is generally 35 Up to 280 The insulating layer is used to isolate the copper foil layer to prevent electrical connection between different layers. The insulating layer is usually made of materials such as polyimide (PI) and polyester (PET).
[0060] In an optional embodiment of the present invention, step 102 includes:
[0061] Step 1021, pre-treating the substrate material of the circuit board, the copper foil and the insulating layer to obtain the pre-treated substrate material of the circuit board, the pre-treated copper foil and the pre-treated insulating layer;
[0062] Specifically, before lamination, the substrate material, copper foil and insulating layer of the circuit board need to be cleaned and flattened to ensure the cleanliness and flatness of the surface; the copper foil can also be roughened to improve the adhesion between the copper foil layer and the insulating layer or substrate material; the designed circuit diagram is transferred to the copper foil through photolithography or laser cutting technology to form the required circuit pattern.
[0063] Step 1022, stacking the pretreated circuit board substrate material, the pretreated copper foil and the pretreated insulation layer in a preset order, and placing them in a laminating machine for laminating according to preset laminating parameters to obtain an original copper substrate.
[0064] Specifically, in accordance with the order of preset requirements, the pre-treated substrate material, pre-treated copper foil and pre-treated insulating layer of the circuit board are stacked in a certain order, and then placed in a laminating machine, first preheated to soften the insulating layer and drive out the gas and moisture therein; then, under the preset laminating parameters, the stacked substrate material, copper foil and insulating layer are laminated to ensure the tight bonding between the substrate material, copper foil and insulating layer. Among them, the preset laminating parameters include laminating temperature and pressure parameters, which are adjusted and set according to the material type and thickness of the substrate material, copper foil and insulating layer. In a specific embodiment, in order to fully solidify the material and increase the stability between the layers of the circuit board, the temperature of each laminating usually needs to reach 175°C and be maintained for more than 70 minutes to achieve the standard laminating environment of the application base layer, plus the waiting time for the heating and cooling process, the single laminating time is generally more than 4 hours.
[0065] In an optional embodiment of the present invention, step 103 includes:
[0066] Step 1031, performing sputtering treatment on the original copper substrate to obtain a copper substrate with a copper film;
[0067] Specifically, the surface of the original copper substrate is cleaned to remove impurities such as oil, dust, etc. to ensure the quality of subsequent processes; then, a sputtering process is used to cover the cleaned surface of the copper substrate with a uniform copper film. This layer of copper film will provide a conductive basis for the subsequent electroplated copper pillars and ensure the close bonding between the electroplated copper layer and the circuit board.
[0068] Step 1032, performing photolithography on the copper substrate with the copper film according to a preset pattern to obtain a copper substrate with a photoresist layer;
[0069] Specifically, a protective photoresist layer with a preset pattern can be formed on the copper film layer by using a photolithography process, and the protective photoresist layer covers the area that does not need electroplating to ensure that the electroplated copper pillars are only formed at designated positions.
[0070] Step 1033, placing the copper substrate with the photoresist layer into an electroplating tank and performing electroplating according to preset electroplating parameters to obtain a copper substrate with copper pillars;
[0071] Specifically, the preset electroplating parameters include current density, electroplating time (such as 2 hours) and electroplating solution components (generally including metal salts, acids or alkalis, etc.). The current density can be calculated using the formula J=I / S, where J is the current density ( ), I is the current intensity (A), S is the cross-sectional area of the copper substrate with the photoresist layer ( ). The copper substrate with the photoresist layer is placed in an electroplating tank, and a copper layer is deposited on the exposed copper film layer according to preset electroplating parameters through an electroplating process to form the required copper pillars.
[0072] Step 1034, immersing the copper substrate with the copper pillars in a cleaning solution for cleaning to obtain the copper substrate with the photoresist layer removed;
[0073] Specifically, the cleaning liquid can be a cupric chloride cleaning liquid, which mainly includes cupric chloride, hydrochloric acid, water, inhibitors, brighteners, etc. Other alkaline cleaning liquids or a mixture of sulfuric acid and hydrogen peroxide can also be selected according to the substrate material. The copper substrate with copper pillars is immersed in the cleaning liquid for cleaning, and the photoresist layer on the copper substrate can be removed.
[0074] Step 1035 , shaping the copper substrate with the photoresist layer removed to obtain a copper substrate with copper-based bosses.
[0075] Specifically, solder paste can be applied to the copper pillar and preheated, then heated to the welding temperature to melt the solder paste, and the copper substrate is cooled after welding. These operations are to plasticize the copper substrate with the photoresist layer removed to improve the strength and stability of the copper pillar and make the copper pillar more closely bonded to the substrate surface.
[0076] In an optional embodiment of the present invention, step 104 includes:
[0077] Step 1041, determining a slotting position according to the copper substrate with the copper-based boss;
[0078] Specifically, the position where the blind groove needs to be formed on the copper substrate can be determined according to the preset groove requirements.
[0079] Step 1042, using a depth-controlled gong machine to gong a depth-controlled blind groove at the grooving position to obtain a copper substrate with a pillar-type structure.
[0080] Specifically, the working parameters of the depth-controlled gong machine can be set in advance, such as controlling the depth at 0.16±0.025mm. According to the working parameters, the depth-controlled gong machine gongs a controlled-depth blind groove at the groove opening position of the copper substrate. It should be noted that the depth-controlled gong machine needs to ensure that the bottom surface of the blind groove is inside the copper substrate to form a pillar structure.
[0081] In an optional embodiment of the present invention, step 105 includes:
[0082] Step 1051, performing a first treatment on the copper substrate of the pillar structure according to a preset first treatment condition to obtain a copper substrate after the first treatment;
[0083] Step 1052, annealing the copper substrate after the first treatment according to preset annealing conditions to obtain an annealed copper substrate;
[0084] Step 1053 , quenching the annealed copper substrate according to preset quenching conditions to obtain a heat-treated copper substrate.
[0085] Specifically, by performing the first treatment, annealing treatment and quenching treatment on the copper substrate, the substrate can have good mechanical processing performance, which facilitates the subsequent processing of the circuit board and prolongs the service life of the circuit board.
[0086] In an optional embodiment of the present invention, step 1051 includes:
[0087] Step 10511, obtaining a preset first processing condition; the preset first processing condition includes: a holding temperature of 800° C. to 900° C., and a holding time of 1 hour to 4 hours;
[0088] Step 10512, placing the copper substrate of the pillar structure into a resistance furnace for heat preservation treatment according to the preset first treatment condition, to obtain the copper substrate after heat preservation treatment;
[0089] It should be noted that the copper substrate with a pillar structure is placed in a resistance furnace and heated to 800°C to 900°C and then kept warm for 1 to 4 hours, so that the alloy elements inside the copper are fully dissolved into the copper matrix to form a uniform solid solution, thereby improving the mechanical properties and corrosion resistance of the copper substrate.
[0090] Step 10513, cooling the copper substrate after the heat preservation treatment to obtain the copper substrate after the first treatment.
[0091] Specifically, the copper substrate after the heat preservation treatment can be cooled by air cooling or oil cooling to reduce the residual stress.
[0092] In an optional embodiment of the present invention, step 1052 includes:
[0093] Step 10521, obtaining preset annealing conditions; the preset annealing conditions include: annealing temperature is any one of 780° C., 650° C. to 675° C., and 600° C., and holding time is 1 hour to 2 hours;
[0094] Step 10522: placing the copper substrate after the first treatment into an annealing furnace for annealing according to the preset annealing conditions to obtain the copper substrate after annealing.
[0095] Specifically, the copper substrate after the first treatment is placed in an annealing furnace and heated to the annealing temperature in the preset annealing treatment conditions, then kept warm for 1 to 2 hours, and then slowly cooled, which can eliminate the residual stress generated in the preparation process of the copper substrate and improve plasticity and toughness.
[0096] In an optional embodiment of the present invention, step 1053 includes:
[0097] Step 10531, preheating the annealed copper substrate to obtain a preheated copper substrate;
[0098] Specifically, the copper substrate after annealing can be thoroughly cleaned first to remove oil, scale and other impurities on the surface of the copper substrate. After cleaning, the copper substrate can be dried to ensure that the surface of the copper substrate after cleaning is dry and free of water stains. Preheating the copper substrate after annealing can reduce the thermal stress of the copper substrate during the quenching process and make the temperature inside and outside the copper substrate more uniform.
[0099] Step 10532, obtaining preset quenching conditions; the preset quenching conditions include: a quenching temperature of 900° C. to 950° C., and a quenching time of 5 seconds to 15 seconds;
[0100] Specifically, the quenching temperature and quenching time can be set according to the substrate material, thickness and required performance. The preset quenching treatment conditions in this embodiment are only used as examples.
[0101] Step 10533, quenching the preheated copper substrate according to the preset quenching conditions to obtain a quenched copper substrate;
[0102] Specifically, the preheated copper substrate can be quenched by oil quenching or water quenching. Oil quenching is to quickly immerse the copper substrate heated to 900°C to 950°C in preheated quenching oil for cooling. The oil quenching temperature is moderate and is suitable for copper substrates with low quenching sensitivity. The quenching oil should have good thermal stability and oxidation resistance. Water quenching is to put the copper substrate heated to 900°C to 950°C into water, heat it red hot, and then put it into water, and repeat it to the preset number of water quenching times. The water quenching cooling speed is fast, and higher hardness and wear resistance can be obtained.
[0103] Step 10534, repairing the quenched copper substrate to obtain a heat-treated copper substrate.
[0104] Specifically, the copper substrate after quenching may have problems such as deformation, cracking or uneven hardness. Therefore, it is necessary to repair the copper substrate after quenching to improve its performance. The repair treatment method can be:
[0105] Tempering: Tempering can reduce the hardness of the copper substrate and improve its toughness and plasticity. The specific tempering treatment method can be to place the copper substrate in the air and heat it to the tempering temperature (generally between 350-650℃); observe the color change of the copper substrate, wait until the color becomes darker (the judgment condition can be that the color of the copper substrate meets the preset color range) and keep it for a certain period of time, then start cooling; gradually cool down to room temperature, and the tempering treatment is completed.
[0106] Straightening: For the copper substrate that is deformed after quenching, straightening treatment can be used to restore its straightness. Specifically, the copper substrate can be straightened using a straightening machine.
[0107] Surface treatment: In order to improve the appearance and performance of the copper substrate, its surface can be treated, such as polishing, sandblasting, etc.
[0108] In an optional embodiment of the present invention, step 106 includes:
[0109] Step 1061, cleaning the heat-treated copper substrate to obtain a cleaned copper substrate;
[0110] Specifically, concentrated alkaline chemicals (such as a mixture of sodium hydroxide and water) can be used to clean the heat-treated copper substrate at a temperature range of 60-70°C for 20-30 minutes; or steam formed by chlorofluorocarbons reaching the boiling point can be used to clean the heat-treated copper substrate. After that, an acidic solution (such as a mixture of aminosulfonic acid and water) can be used to remove oxides and rust on the surface of the copper substrate; then the copper substrate can be soaked and rinsed with clean water to ensure that the detergent is completely removed; finally, the copper substrate can be dried by hot air drying or vacuum drying.
[0111] Step 1062, performing quality inspection on the cleaned copper substrate to obtain a qualified copper substrate;
[0112] Specifically, ultrasonic testing can be used to detect defects inside the copper substrate, X-ray testing can be used to detect the internal structure of the copper substrate, visual testing can be used to detect whether there is oil, scratches, oxidation, etc. on the surface of the copper substrate, and mechanical properties such as tensile strength and strength testing can be evaluated. The cleaned copper substrate can be inspected for quality, and the copper substrate that meets the inspection conditions can be used as a qualified copper substrate for subsequent processing. Inspection conditions may include: there are no cavities, bubbles, impurities, cracks, etc. inside the copper substrate (applicable to ultrasonic testing); the internal structure of the copper substrate presents a uniform grayscale distribution (applicable to X-ray testing); there is no oil, scratches, oxidation, etc. on the surface of the copper substrate (applicable to visual testing); the tensile strength meets the preset standard (such as the tensile strength of the copper substrate is at least 7 pounds per inch).
[0113] Step 1063, cutting the qualified copper substrate according to preset cutting conditions to obtain a circuit board substrate.
[0114] Specifically, the qualified copper substrate can be cut according to a preset size or a preset shape to meet user needs. In a specific embodiment, the preset size may include: a width of 50 mm, 75 mm, or 100 mm, a length of 50 mm, 75 mm, or 100 mm, and a thickness of 0.4 mm or 0.8 mm. Specifically, the preset size may also include a minimum aperture, a minimum line width, a minimum line spacing, a pad diameter, a pad spacing, etc. The preset shape may be a square, a rectangle, a circle, etc., and a suitable shape may be selected according to user needs.
[0115] A specific implementation of the above method of the present invention is as follows:
[0116] Step 111, providing a substrate material, copper foil and an insulating layer of a circuit board. In this embodiment, the substrate material is a FR4 metal substrate, and the thickness of the copper foil is 35 , the material of the insulating layer is polyimide.
[0117] Step 112, clean and dry the substrate material, copper foil and insulating layer of the circuit board. Taking three layers as an example, stack the copper foil, insulating layer and substrate material in order from top to bottom, and put them into a pressing machine for pressing at 175°C for 2 hours to tightly combine the substrate material, copper foil and insulating layer into a copper substrate.
[0118] Step 113, placing the copper substrate and the target material in the corresponding positions of the vacuum sputtering machine, and evacuating the vacuum through the vacuum pump system to make the vacuum degree in the vacuum sputtering machine less than Pa, start the vacuum sputtering machine to cover the surface of the copper substrate with a uniform copper film. Then use the photolithography process to form a photoresist layer on the copper film, and put the copper substrate into the electroplating tank for 2 hours to form a copper pillar.
[0119] Step 114, using a depth-controlled gong machine to gong a blind groove at a preset position of the copper substrate, and the bottom of the blind groove is connected to the substrate material of the circuit board.
[0120] Step 115, after cleaning the surface of the copper substrate to remove impurities such as oil, oxides, etc., the copper substrate is heat treated. The heat treatment method may include solution treatment, aging treatment, annealing treatment and quenching treatment, etc., to increase the hardness of the copper substrate, improve the conductivity of the copper substrate, and eliminate residual stress.
[0121] Step 116, cleaning the copper substrate after the heat treatment, and then using ultrasound, X-rays, etc. to perform quality inspection on the copper substrate. Only the copper substrate that meets the preset inspection conditions is regarded as a qualified copper substrate for subsequent processing.
[0122] Step 117, cutting the qualified copper substrate according to the size (such as length, width, height, thickness, etc.) or shape (such as square, rectangle, circle, etc.) required by the customer, and mechanical cutting or laser cutting can be used to ensure the cutting accuracy and flatness, and the cut copper substrate is packaged as a circuit board substrate. The substrate material, copper foil and insulating layer of the circuit board are pressed together to obtain the original copper substrate, and the original copper substrate is electroplated and slotted to form a pillar structure for heat dissipation on the original copper substrate, and then the copper substrate of the pillar structure is heat-treated and cut. The obtained circuit board substrate has the advantages of good heat dissipation performance and strong mechanical processing performance, which can meet the needs of high power density circuits, improve the quality and stability of the circuit board substrate, and extend its service life.
[0123] The above method of the embodiment of the present invention forms a pillar structure for heat dissipation on the original copper substrate by electroplating and grooving the original copper substrate, so that the circuit board substrate has good heat dissipation performance; in addition, by heat treating the copper substrate, the effect of improving the mechanical processing performance of the circuit board substrate is achieved, so that the circuit board substrate is suitable for high power density circuits and has the advantages of high quality, good stability and long service life.
[0124] An embodiment of the present invention further provides a circuit board substrate, which is prepared by the method for preparing the circuit board substrate described in any one of the above embodiments.
[0125] like Figure 2 The figure is a schematic diagram of the structure of a circuit board substrate in a specific embodiment. The circuit board substrate comprises a substrate material layer 1, a copper foil layer 2, an insulating layer 3 and a copper-based boss 4, wherein the insulating layer 3 is located between the copper foil layer 2 and the substrate material layer 1, the copper foil layer 2 is arranged above the insulating layer 3, the substrate material layer 1 is arranged below the insulating layer 3, a blind groove 5 is arranged in the substrate material layer 1, the copper-based boss 4 passes through the copper foil layer 2 and the insulating layer 3, and the bottom of the copper-based boss 4 is connected to the substrate material layer 1, and a component 6 is arranged on the copper foil layer 2.
[0126] Among them, blind grooves 5 are formed on the substrate material layer 1, and the blind grooves 5 are filled with insulating resin, so that the substrate material layer 1 is divided into multiple separate networks, and then the circuits on the copper foil layer 2 are connected to the multiple networks on the substrate material layer 1 through components 6, which can meet the needs of large current passing through the substrate material layer and conduct away heat, greatly improving the heat dissipation effect.
[0127] The circuit board substrate provided in the embodiment of the present invention has a pillar structure, which can improve the mechanical strength and heat dissipation effect of the circuit board substrate, and has good mechanical processing performance, and is suitable for circuits with high power density.
[0128] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a circuit board substrate, characterized in that: include: Providing a substrate material, a copper foil and an insulating layer of a circuit board; the thickness of the copper foil is 35 microns to 280 microns; The substrate material of the circuit board, the copper foil and the insulating layer are pressed together to obtain an original copper substrate; Electroplating the original copper substrate to obtain a copper substrate with a copper-based boss; Performing a grooving process on the copper substrate with the copper-based bosses to obtain a copper substrate with a pillar-type structure; Performing heat treatment on the copper substrate of the pillar structure to obtain a heat-treated copper substrate; Cutting the heat-treated copper substrate according to preset cutting conditions to obtain a circuit board substrate; The substrate material of the circuit board, the copper foil and the insulating layer are pressed together to obtain an original copper substrate, including: Pre-treating the substrate material of the circuit board, the copper foil and the insulating layer to obtain the pre-treated substrate material of the circuit board, the pre-treated copper foil and the pre-treated insulating layer; specifically, cleaning and flattening the substrate material of the circuit board, the copper foil and the insulating layer; and then roughening the copper foil; The pretreated substrate material of the circuit board, the pretreated copper foil and the pretreated insulating layer are stacked in a preset order, placed in a laminating machine for preheating, and pressed according to preset pressing parameters to obtain an original copper substrate; the preset pressing parameters include a pressing temperature of 175° C.; The original copper substrate is electroplated to obtain a copper substrate with a copper-based boss, comprising: Sputtering the original copper substrate to obtain a copper substrate with a copper film; Performing photolithography on the copper substrate with the copper film according to a preset pattern to obtain a copper substrate with a photoresist layer; Placing the copper substrate with the photoresist layer into an electroplating tank and performing electroplating according to preset electroplating parameters to obtain a copper substrate with copper pillars; the preset electroplating parameters include current density, which is calculated by the formula J=I / S, where J is current density, I is current intensity, and S is the cross-sectional area of the copper substrate with the photoresist layer; Immersing the copper substrate with the copper pillars in a cleaning solution for cleaning to obtain the copper substrate with the photoresist layer removed; Performing shaping treatment on the copper substrate with the photoresist layer removed to obtain a copper substrate with a copper-based boss; The copper substrate with the copper-based boss is grooved to obtain a copper substrate with a pillar structure, comprising: Determining a slotting position according to the copper substrate with the copper-based boss; A depth-controlled gong machine is used to gong a depth-controlled blind groove at the grooving position to obtain a copper substrate with a pillar-type structure; The step of heat-treating the copper substrate of the pillar structure to obtain the heat-treated copper substrate comprises: Performing a first treatment on the copper substrate of the pillar structure according to a preset first treatment condition to obtain a copper substrate after the first treatment; Performing annealing treatment on the copper substrate after the first treatment according to preset annealing treatment conditions to obtain the annealed copper substrate; Performing quenching treatment on the annealed copper substrate according to preset quenching treatment conditions to obtain a heat-treated copper substrate; The copper substrate with the pillar structure is subjected to a first treatment according to a preset first treatment condition to obtain the copper substrate after the first treatment, comprising: Obtaining a preset first processing condition; the preset first processing condition includes: a holding temperature of 800° C. to 900° C., and a holding time of 1 hour to 4 hours; According to the preset first processing condition, placing the copper substrate of the pillar structure into a resistance furnace for heat preservation treatment to obtain the copper substrate after heat preservation treatment; Cooling the copper substrate after the heat preservation treatment to obtain the copper substrate after the first treatment; Wherein, annealing the copper substrate after the first treatment according to preset annealing conditions to obtain the annealed copper substrate includes: Obtaining preset annealing conditions; the preset annealing conditions include: an annealing temperature of any one of 780° C., 650° C. to 675° C., and 600° C., and a holding time of 1 hour to 2 hours; placing the copper substrate after the first treatment into an annealing furnace for annealing according to the preset annealing conditions to obtain the copper substrate after annealing; The quenching treatment is performed on the annealed copper substrate according to preset quenching treatment conditions to obtain a heat-treated copper substrate, including: Preheating the annealed copper substrate to obtain a preheated copper substrate; Obtaining preset quenching conditions; the preset quenching conditions include: a quenching temperature of 900° C. to 950° C., and a quenching time of 5 seconds to 15 seconds; Performing quenching treatment on the preheated copper substrate according to the preset quenching treatment conditions to obtain a quenched copper substrate; The quenched copper substrate is repaired to obtain a heat-treated copper substrate.
2. The method for preparing a circuit board substrate according to claim 1, characterized in that: The heat-treated copper substrate is cut according to preset cutting conditions to obtain a circuit board substrate, including: Cleaning the heat-treated copper substrate to obtain a cleaned copper substrate; Performing quality inspection on the cleaned copper substrate to obtain a qualified copper substrate; The qualified copper substrate is cut according to preset cutting conditions to obtain a circuit board substrate.