Preparation process of cement-based composite mortar for repairing cracks in marine concrete structures

The repair mortar that combines emulsified asphalt, graphene oxide, strong alkali, etc. solves the crack and leakage problems of offshore concrete structures in high-salt and high-humidity environments, and achieves high adhesion and waterproof and anti-permeability properties. The repair effect is improved and industrial solid waste is used to solve the problem of easy falling off of repair materials in the existing technology.

CN118495884BActive Publication Date: 2024-10-18YANTAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410640439.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-10-18
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Marine concrete structures are prone to cracks and leakage problems in high-salt and high-humidity environments. Existing cement-based repair materials are not tightly integrated with the concrete structure, resulting in poor repair results, and the repair materials are easy to fall off, affecting the mechanical properties of the bridge. and security.

Method used

Emulsified asphalt is used as a component of the repair material. It is combined with graphene oxide, strong alkali liquid, steel slag fine aggregate and polycarboxylate water-reducing agent to form modified fine aggregate, and is combined with Portland cement and activated coal. Gangue, fly ash and silica fume are mixed to form a repair mortar with high adhesion and waterproof and impermeability properties.

Benefits of technology

It significantly improves the bonding performance and waterproof and impermeability performance of the repair mortar and the concrete structure, enhances the repair effect, has secondary repair capabilities, and uses industrial solid waste to improve the mechanical properties and resource utilization of the repair mortar.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118495884B_ABST
    Figure CN118495884B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of concrete, and specifically discloses a preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures. The process comprises the following steps: (1) dispersing GO in a strong alkaline solution to form an alkaline suspension. (2) mixing steel slag fine aggregate with an aqueous solution of a polycarboxylate water reducer to form a wet material, then spraying the alkaline suspension while stirring, and then heating the obtained mixture in a closed environment for reaction. After completion, the obtained product is dried to obtain a modified fine aggregate. (3) The following raw materials are taken: silicate cement, modified fine aggregate, fly ash, silica ash, and emulsified asphalt. First, silicate cement, modified fine aggregate, activated coal gangue, fly ash and silica ash are uniformly mixed, and then the emulsified asphalt and water are added and mixed to obtain the repair mortar. The repair mortar containing emulsified asphalt of the present invention not only has a strong bonding ability with the concrete structure, but also has good waterproof and anti-seepage properties, thereby improving the repair effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete, and in particular to a preparation process of a cement-based composite mortar for repairing cracks in marine engineering concrete structures. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] A cross-sea bridge is a bridge that crosses a bay, strait, deep sea, estuary or other marine waters. As the cross-sea bridge is deep in the marine environment, it faces complex and harsh natural conditions. Concrete is the main building material for the construction of cross-sea bridges. Cross-sea bridges are in a high-salt, high-humidity environment for a long time. Once moisture and salt enter through cracks and other damaged parts, it will cause accelerated corrosion of the steel bars in the bridge structure. In particular, the entry of chloride ions will destroy the passivation film on the surface of the steel bars, accelerate the corrosion rate of the steel bars, affect the mechanical properties of the bridge, and cause a decrease in safety. In addition, other concrete structures in the marine environment also face similar problems. Therefore, it is very necessary to repair the damaged parts of such marine concrete structures in a timely manner.

[0004] The use of cement-based repair materials to repair cracks and other damaged parts on marine concrete structures is currently a common method. However, due to the obvious interface between the repair material and the concrete structure, and the phenomenon of insufficient bonding, leakage still exists in the repaired part. With the increase of service time, the steel bars inside the concrete structure will still show accelerated corrosion. In addition, after a certain period of seawater erosion and scouring, the repair material is easy to fall off the concrete structure. Therefore, the use of repair materials that can be tightly bonded to the concrete structure and have good anti-seepage performance is the key to ensuring the repair effect. Summary of the invention

[0005] In view of the above problems, the present invention provides a preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures. The repair mortar containing emulsified asphalt of the present invention not only has a strong bonding ability with the concrete structure, but also has good waterproof and anti-seepage properties, thereby improving the repair effect. Specifically, the technical solution of the present invention is as follows.

[0006] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0007] (1) Disperse graphene oxide (GO) in a strong alkaline solution to form an alkaline suspension for later use.

[0008] (2) Mix the steel slag fine aggregate and the aqueous solution of the polycarboxylate water-reducing agent to form a wet material, then spray the alkaline suspension while stirring, and then heat the obtained mixture in a closed environment for reaction. After completion, dry the obtained product to obtain the modified fine aggregate for standby use.

[0009] (3) Take the following raw materials: 300-400 parts by weight of silicate cement, 410-462 parts by weight of the modified fine aggregate, 70-90 parts by weight of activated coal gangue, 90-120 parts by weight of fly ash, 35-50 parts by weight of silica fume, and 100-150 parts by weight of emulsified asphalt. First, mix the silicate cement, modified fine aggregate, activated coal gangue, fly ash and silica fume evenly, then add the emulsified asphalt and water and mix evenly to obtain the repair mortar.

[0010] Furthermore, in step (1), the ratio of graphene oxide to strong alkaline solution is 1 g: 30-40 ml. Optionally, the concentration of the strong alkaline solution is 2-4 mol / L.

[0011] Furthermore, in step (1), the strong alkaline solution includes any one of sodium hydroxide solution, potassium hydroxide solution, etc.

[0012] Furthermore, in step (2), the ratio of the steel slag fine aggregate to the aqueous solution of the polycarboxylate water-reducing agent is 1 g: 1-2 ml. Optionally, the mass fraction of the aqueous solution of the polycarboxylate water-reducing agent is 3-7%.

[0013] Furthermore, in step (2), the ratio of the steel slag fine aggregate to the alkaline suspension is 1 g: 0.8-1.2 ml. Optionally, the particle size of the steel slag fine aggregate is 0.2-0.5 mm.

[0014] Furthermore, in step (2), the heating temperature is 70-90° C. and the reaction time is 40-55 min.

[0015] Furthermore, in step (2), the drying temperature is 50-60° C. and the drying time is 1.5-2 h.

[0016] Furthermore, in step (3), the solid content of the emulsified asphalt is 50-65%.

[0017] Furthermore, in step (3), the water is added according to a water-cement ratio of 0.28 to 0.33. The "ash" includes silicate cement, fly ash and silica fume.

[0018] Furthermore, the activated coal gangue is prepared by the following method: coal gangue particles and sodium hydroxide solid powder are mixed and then heat treated, and after completion, the obtained product is cooled, and then mechanically ground and sieved to obtain the activated coal gangue.

[0019] Furthermore, the mass ratio of the coal gangue particles to the sodium hydroxide solid powder is 1:0.13-0.17.

[0020] Furthermore, the heat treatment temperature is 500-600° C., and the treatment time is 20-30 min.

[0021] Furthermore, the particle size of the activated coal gangue is between 0.1 and 0.2 mm.

[0022] The present invention has the following beneficial technical effects: the cement-based composite mortar of the present invention is a composite of cement cementitious materials and emulsified asphalt, and the emulsified asphalt can not only enhance the bonding performance between the repair mortar and the concrete structure. At the same time, the emulsified asphalt can also effectively improve the waterproof and impermeability of the protective layer formed by the repair mortar as a whole. In addition, the emulsified asphalt also enables the repair mortar of the present invention to have a secondary repair effect. When microcracks occur in the repair material, the microcracks can be repaired by heating to melt the asphalt to ensure the repair effect of the damaged part. In addition, the repair mortar of the present invention makes extensive use of coal gangue, steel slag, fly ash and silica fume, which is not only conducive to the resource utilization of these industrial solid wastes, but also improves the mechanical properties of the repair mortar. However, due to the insufficient volume stability of steel slag, cracks are easily generated in the repair mortar, resulting in a decrease in the repair effect. Therefore, the present invention first applies an aqueous solution of a polycarboxylic acid water reducer on the steel slag fine aggregate, thereby loading the water reducer on the steel slag. When the alkaline suspension formed by graphene oxide and strong alkali solution is further applied and heated for reaction, on the one hand, calcium oxide, the main factor of poor volume stability in the steel slag, reacts with water, effectively improving the volume stability of the steel slag. On the other hand, the hydroxide ions provided by the alkaline suspension can attack the silicon-calcium and silicon-aluminum inert mineral phase structures on the surface of the steel slag, causing these mineral phase structures to depolymerize and form [SiO4] 4- and [AlO4] 5- Tetrahedron. During the hydration stage of the mortar material, these tetrahedral structures react under the action of calcium ions produced by cement hydration to form cementitious materials such as hydrated calcium silicate and hydrated calcium aluminate, which not only makes the bonding force between the steel slag fine aggregate and the repair mortar matrix stronger, but also increases the amount of cementitious materials, thereby improving the mechanical strength of the repair mortar. At the same time, the present invention utilizes the abundant carboxyl groups carried by the water reducer and the alkaline environment provided by the alkaline suspension to dehydrate and condense the hydroxyl groups on the graphene oxide with the carboxyl groups under the catalysis of the alkaline solution, connect the graphene oxide with the water reducer, and thus accurately graft the graphene oxide onto the steel slag fine aggregate, thereby improving the bonding force and density between the fine aggregate and the repair material matrix, and improving the mechanical properties of the repair material.

[0023] In addition, coal gangue is a solid waste generated in the process of coal mining, with a huge output. The accumulation of a large amount of coal gangue in the open air has brought many environmental problems. Due to the presence of carbonaceous components in coal gangue, after entering the repair material of the present invention, it is easy to absorb water under the action of moisture provided by seawater during service, resulting in a series of reactions, causing the coal gangue particles to expand, pulverize, and other problems, and then causing the repair material itself to crack. For this reason, the present invention treats coal gangue and sodium hydroxide solid powder at high temperature. At this time, the coal gangue itself can play a certain role as fuel. While removing the carbonaceous material, sodium hydroxide is also used to activate the coal gangue at high temperature to improve the gelling activity of the coal gangue. At the same time, after the activated coal gangue enters the repair material, the residual sodium hydroxide loaded on the activated coal gangue dissolves in water to form an alkaline solution, which can also stimulate the fly ash and silica ash, thereby improving the gelling activity of the fly ash and silica ash, and allowing the coal gangue, fly ash and silica ash to utilize the calcium hydroxide produced by cement hydration for secondary hydration to form more cementitious substances, thereby improving the mechanical properties and anti-seepage properties of the repair material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0025] Figure 1 The following is a sample diagram of a test piece prepared for compressive strength testing in Example 1.

[0026] Figure 2 This is a test graph of chloride ion diffusion coefficient of the following Example 1. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0028] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meaning as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. Now, the technical solution of the present invention is further described in conjunction with specific embodiments.

[0029] Example 1

[0030] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0031] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm and an aqueous solution of polycarboxylate superplasticizer (mass fraction 5%) were mixed to form a wet material in a ratio of 1 g:1.5 ml.

[0032] (2) Graphene oxide and 3 mol / L sodium hydroxide solution were mixed in a ratio of 1 g:40 ml and then ultrasonically treated for 10 min to form an alkaline suspension. Then, the alkaline suspension was sprayed into the wet material while stirring the wet material in a ratio of 1 g:1 ml of the steel slag fine aggregate and the alkaline suspension.

[0033] (3) The mixture obtained in (2) is heated to 80°C in a sealed reactor and kept at this temperature for 45 minutes. After completion, the obtained product is placed in an oven and dried at 60°C for 2 hours to obtain the modified fine aggregate, which is then used for later use.

[0034] (4) The coal gangue particles and sodium hydroxide solid powder were mixed in a mass ratio of 1:0.14 and stirred evenly, and then heated to 570°C in a furnace for 20 minutes. After completion, the obtained product was cooled to room temperature, and then mechanically ground and sieved to obtain activated coal gangue with a particle size distribution between 0.1 and 0.15 mm.

[0035] (5) Take the following raw materials: 330 parts by weight of 42.5 ordinary Portland cement, 440 parts by weight of the modified fine aggregate of this embodiment, 76 parts by weight of activated coal gangue of this embodiment, 100 parts by weight of Class I fly ash, 45 parts by weight of silica fume, and 120 parts by weight of emulsified asphalt with a solid content of 50% (produced by Wuxi Senjinglin Building Materials Co., Ltd.). First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder at a water-cement ratio of 0.3, stir them evenly, and obtain the repair mortar.

[0036] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box (temperature 20±2°C, humidity>95%) for curing for 7 days. Then, the test piece (such as Figure 1 In addition, the chloride ion diffusion coefficient (as shown in Figure 2) of the repair mortar prepared in this embodiment was tested according to the Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete (GBT50082-2009). Figure 2 The results are as follows: 7d compressive strength = 59.24 MPa. Chloride ion diffusion coefficient = 1.36×10 −12 m 2 s −1.

[0037] Example 2

[0038] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0039] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm and an aqueous solution of polycarboxylate water-reducing agent (mass fraction 3%) were mixed to form a wet material in a ratio of 1 g:2 ml.

[0040] (2) Graphene oxide and 4 mol / L sodium hydroxide solution were mixed in a ratio of 1 g:30 ml and then ultrasonically treated for 8 minutes to form an alkaline suspension. Then, the alkaline suspension was sprayed into the wet material while stirring the wet material in a ratio of 1 g:1.2 ml of the steel slag fine aggregate and the alkaline suspension.

[0041] (3) The mixture obtained in (2) is heated to 70°C in a sealed reactor and kept at this temperature for 55 min. After completion, the obtained product is placed in an oven and dried at 50°C for 2 h to obtain the modified fine aggregate, which is then used for later use.

[0042] (4) The coal gangue particles and sodium hydroxide solid powder were mixed in a mass ratio of 1:0.13 and stirred evenly, and then heated to 500°C in a Ma furnace for 30 minutes. After completion, the obtained product was cooled to room temperature, and then mechanically ground and sieved to obtain activated coal gangue with a particle size distribution between 0.15 and 0.2 mm.

[0043] (5) Take the following raw materials: 400 parts by weight of 42.5 ordinary Portland cement, 462 parts by weight of the modified fine aggregate of this embodiment, 90 parts by weight of activated coal gangue of this embodiment, 120 parts by weight of Class I fly ash, 50 parts by weight of silica fume, and 150 parts by weight of emulsified asphalt with a solid content of 50%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder according to a water-cement ratio of 0.33, stir evenly, and obtain the repair mortar.

[0044] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 61.07 MPa. Chloride ion diffusion coefficient = 1.12×10 −12 m 2 s−1 .

[0045] Example 3

[0046] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0047] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm was mixed with an aqueous solution of polycarboxylate superplasticizer (mass fraction 7%) to form a wet material in a ratio of 1 g:1 ml.

[0048] (2) Graphene oxide and 2 mol / L potassium hydroxide solution were mixed in a ratio of 1 g:35 ml and then ultrasonically treated for 10 min to form an alkaline suspension. Then, the alkaline suspension was sprayed into the wet material while stirring the wet material in a ratio of 1 g:0.8 ml of the steel slag fine aggregate and the alkaline suspension.

[0049] (3) The mixture obtained in (2) is heated to 90°C in a sealed reactor and kept at this temperature for 40 minutes. After completion, the obtained product is placed in an oven and dried at 60°C for 1.5 hours to obtain the modified fine aggregate, which is then used for later use.

[0050] (4) The coal gangue particles and sodium hydroxide solid powder were mixed in a mass ratio of 1:0.17 and stirred evenly, and then heated to 600°C in a Ma furnace for 20 minutes. After completion, the obtained product was cooled to room temperature, and then mechanically ground and sieved to obtain activated coal gangue with a particle size distribution between 0.1 and 0.15 mm.

[0051] (5) Take the following raw materials: 300 parts by weight of 42.5 ordinary Portland cement, 410 parts by weight of the modified fine aggregate of this embodiment, 70 parts by weight of activated coal gangue of this embodiment, 90 parts by weight of Class I fly ash, 35 parts by weight of silica fume, and 100 parts by weight of emulsified asphalt with a solid content of 55%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder at a water-cement ratio of 0.28, stir evenly, and obtain the repair mortar.

[0052] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 58.33 MPa. Chloride ion diffusion coefficient = 1.58×10 −12 m2 s −1 .

[0053] Example 4

[0054] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps: taking the following raw materials: 400 parts by weight of 42.5 ordinary Portland cement, 462 parts by weight of steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm, 90 parts by weight of activated coal gangue of Example 2, 120 parts by weight of Class I fly ash, 50 parts by weight of silica fume, and 150 parts by weight of emulsified asphalt with a solid content of 50%. First, the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume are mixed and stirred evenly, and then the emulsified asphalt and water are added to the obtained dry powder according to a water-cement ratio of 0.33, and the repair mortar is obtained after stirring evenly.

[0055] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The results are: 7d compressive strength = 40.54 MPa. Chloride ion diffusion coefficient = 4.03×10 −12 m 2 s −1 .

[0056] Example 5

[0057] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0058] (1) Mix steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm with deionized water in a ratio of 1 g: 1.5 ml and stir evenly to form a wet material for later use.

[0059] (2) Graphene oxide and 3 mol / L sodium hydroxide solution were mixed in a ratio of 1 g:40 ml and then ultrasonically treated for 10 min to form an alkaline suspension. Then, the alkaline suspension was sprayed into the wet material while stirring the wet material in a ratio of 1 g:1 ml of the steel slag fine aggregate and the alkaline suspension.

[0060] (3) The mixture obtained in (2) is heated to 80°C in a sealed reactor and kept at this temperature for 45 minutes. After completion, the obtained product is placed in an oven and dried at 60°C for 2 hours to obtain the modified fine aggregate, which is then used for later use.

[0061] (4) Take the following raw materials: 330 parts by weight of 42.5 ordinary Portland cement, 440 parts by weight of the modified fine aggregate of this embodiment, 76 parts by weight of the activated coal gangue of Example 1, 100 parts by weight of Class I fly ash, 45 parts by weight of silica fume, and 120 parts by weight of emulsified asphalt with a solid content of 50%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder at a water-cement ratio of 0.3, stir them evenly, and obtain the repair mortar.

[0062] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 54.02 MPa. Chloride ion diffusion coefficient = 1.96×10 −12 m 2 s −1 .

[0063] Example 6

[0064] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0065] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm and an aqueous solution of polycarboxylate water-reducing agent (mass fraction 3%) were mixed to form a wet material in a ratio of 1 g:2 ml.

[0066] (2) Graphene oxide and deionized water were mixed in a ratio of 1 g:30 ml and then ultrasonically treated for 8 minutes to form a graphene suspension. Then, the graphene suspension was sprayed into the wet material while stirring the wet material in a ratio of 1 g:1.2 ml of the steel slag fine aggregate and the graphene suspension.

[0067] (3) The mixture obtained in (2) is heated to 70°C in a sealed reactor and kept at this temperature for 55 min. After completion, the obtained product is placed in an oven and dried at 50°C for 2 h to obtain the modified fine aggregate, which is then used for later use.

[0068] (4) Take the following raw materials: 400 parts by weight of 42.5 ordinary Portland cement, 462 parts by weight of the modified fine aggregate of this embodiment, 90 parts by weight of the activated coal gangue of Example 2, 120 parts by weight of Class I fly ash, 50 parts by weight of silica fume, and 150 parts by weight of emulsified asphalt with a solid content of 50%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder according to a water-cement ratio of 0.33, stir evenly, and obtain the repair mortar.

[0069] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 49.19MPa. Chloride ion diffusion coefficient = 2.52×10 −12 m 2 s −1 .

[0070] Example 7

[0071] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0072] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm was mixed with an aqueous solution of polycarboxylate superplasticizer (mass fraction 7%) to form a wet material in a ratio of 1 g:1 ml.

[0073] (2) According to the material-liquid ratio of 1g:0.8ml, 2mol / L potassium hydroxide solution is sprayed into the wet material while stirring. Then the obtained mixture is heated to 90℃ in a closed reactor for 40min. After completion, the obtained product is placed in an oven at 60℃ and dried for 1.5h to obtain modified fine aggregate for standby use.

[0074] (3) Take the following raw materials: 300 parts by weight of 42.5 ordinary Portland cement, 410 parts by weight of the modified fine aggregate of this embodiment, 70 parts by weight of the activated coal gangue of Example 3, 90 parts by weight of Class I fly ash, 35 parts by weight of silica fume, and 100 parts by weight of emulsified asphalt with a solid content of 55%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder at a water-cement ratio of 0.28, stir evenly, and obtain the repair mortar.

[0075] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 55.63 MPa. Chloride ion diffusion coefficient = 2.14×10 −12 m 2 s −1 .

[0076] Example 8

[0077] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps:

[0078] (1) Steel slag fine aggregate with a particle size distribution between 0.2 and 0.5 mm and an aqueous solution of polycarboxylate superplasticizer (mass fraction 5%) were mixed to form a wet material in a ratio of 1 g:1.5 ml.

[0079] (2) Graphene oxide and 3 mol / L sodium hydroxide solution were mixed in a ratio of 1 g:40 ml and then ultrasonically treated for 10 min to form an alkaline suspension. Then, the alkaline suspension was sprayed into the wet material while stirring the steel slag fine aggregate in a ratio of 1 g:1 ml. The obtained mixture was then placed in an oven and dried at 60°C for 2 h to obtain a modified fine aggregate.

[0080] (3) Take the following raw materials: 330 parts by weight of 42.5 ordinary Portland cement, 440 parts by weight of the modified fine aggregate of this embodiment, 76 parts by weight of the activated coal gangue of Example 1, 100 parts by weight of Class I fly ash, 45 parts by weight of silica fume, and 120 parts by weight of emulsified asphalt with a solid content of 50%. First, mix the cement, modified fine aggregate, activated coal gangue, fly ash and silica fume and stir them evenly. Then, add the emulsified asphalt and water to the obtained dry powder according to a water-cement ratio of 0.3, stir evenly, and obtain the repair mortar.

[0081] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The result is: 7d compressive strength = 52.81 MPa. Chloride ion diffusion coefficient = 3.22×10−12 m 2 s −1 .

[0082] Example 9

[0083] A preparation process of a cement-based composite mortar for repairing cracks in marine concrete structures, comprising the following steps: taking the following raw materials: 300 parts by weight of 42.5 ordinary Portland cement, 410 parts by weight of modified fine aggregate of Example 3, 70 parts by weight of coal gangue with a particle size distribution between 0.1 and 0.15 mm, 90 parts by weight of Class I fly ash, 35 parts by weight of silica fume, and 100 parts by weight of emulsified asphalt with a solid content of 55%. First, the cement, modified fine aggregate, coal gangue, fly ash and silica fume are mixed and stirred evenly, and then the emulsified asphalt and water are added to the obtained dry powder according to a water-cement ratio of 0.28, and the repair mortar is obtained after stirring evenly.

[0084] The repair mortar prepared in this embodiment was made into a test piece and placed in a curing box for curing under standard conditions for 7 days. Then, the compressive strength of the test piece was measured according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). In addition, the chloride ion diffusion coefficient of the repair mortar prepared in this embodiment was tested according to the "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" (GBT 50082-2009). The results are: 7d compressive strength = 42.46 MPa. Chloride ion diffusion coefficient = 4.77×10 −12 m 2 s −1 .

[0085] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation process for a cement-based composite mortar for repairing cracks in marine concrete structures, characterized in that: The steps include: (1) dispersing graphene oxide in a strong alkaline solution to form an alkaline suspension for later use; (2) mixing steel slag fine aggregate and an aqueous solution of a polycarboxylate water-reducing agent to form a wet material, then spraying the alkaline suspension while stirring, and then heating the obtained mixture in a closed environment for reaction; after completion, drying the obtained product to obtain a modified fine aggregate for standby use; (3) Take the following raw materials: 300-400 parts by weight of Portland cement, 410-462 parts by weight of modified fine aggregate, 70-90 parts by weight of activated coal gangue, 90-120 parts by weight of fly ash, 35-50 parts by weight of silica fume, and 100-150 parts by weight of emulsified asphalt; first, mix the Portland cement, modified fine aggregate, activated coal gangue, fly ash and silica fume evenly, then add the emulsified asphalt and water and mix evenly to obtain the repair mortar.

2. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (1), the ratio of graphene oxide to strong alkali solution is 1 g: 30-40 ml, and the concentration of the strong alkali solution is 2-4 mol / L.

3. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (1), the strong alkaline solution includes any one of sodium hydroxide and potassium hydroxide solution.

4. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (2), the ratio of the steel slag fine aggregate to the aqueous solution of the polycarboxylate water-reducing agent is 1 g: 1-2 ml, and the mass fraction of the aqueous solution of the polycarboxylate water-reducing agent is 3-7%.

5. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (2), the ratio of the steel slag fine aggregate to the alkaline suspension is 1 g: 0.8-1.2 ml.

6. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: The particle size of the steel slag fine aggregate is 0.2-0.5 mm.

7. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (2), the heating temperature is 70-90° C. and the reaction time is 40-55 min.

8. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 1, characterized in that: In step (3), the solid content of the emulsified asphalt is 50-65%.

9. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to any one of claims 1 to 8, characterized in that: In step (2), the drying temperature is 50-60° C. and the drying time is 1.5-2 h.

10. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to any one of claims 1 to 8, characterized in that: In step (3), water is added according to a water-cement ratio of 0.28 to 0.

33.

11. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to any one of claims 1 to 8, characterized in that: The activated coal gangue is prepared by the following method: coal gangue particles and sodium hydroxide solid powder are mixed and then heat treated, and after completion, the obtained product is cooled, and then mechanically ground and sieved to obtain the activated coal gangue.

12. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 11, characterized in that: The mass ratio of the coal gangue particles to the sodium hydroxide solid powder is 1:0.13-0.

17.

13. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 11, characterized in that: The heat treatment temperature is 500-600° C., and the treatment time is 20-30 minutes.

14. The preparation process of the cement-based composite mortar for repairing cracks in marine concrete structures according to claim 11, characterized in that: The particle size of the activated coal gangue is between 0.1 and 0.2 mm.

Citation Information

Patent Citations

  • Preparation method of high-density concrete road

    CN107382215A

  • 3D printing graphene oxide reinforced cement-based material and preparation method thereof

    CN113526934A