Preparation method of calcium zinc stabilizer for PVC transparent film

By optimizing the raw material ratio and preparation process, using a combination of calcium salts, zinc salts, lubricants and antioxidants, the thermal stability and antioxidant properties of the PVC transparent film are enhanced, and the thermal stability shortcomings of the existing calcium and zinc stabilizers are solved. problem and achieve more efficient performance improvement.

CN118496679BActive Publication Date: 2024-10-08SHANDONG ZHENXI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410977478.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-08
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Existing calcium zinc stabilizers have limited effect in improving the thermal stability of PVC transparent films. At the same time, traditional lead salt stabilizers are gradually being replaced due to their high toxicity. A calcium stabilizer that can both improve thermal stability and maintain excellent performance is needed. Zinc stabilizer.

Method used

By optimizing the raw material ratio and preparation process, using a specific ratio of calcium salts, zinc salts, lubricants, antioxidants and synergists, the calcium zinc stabilizer is prepared through steps such as dissolution, stirring, reaction and evaporation under reduced pressure, and Chemical substances such as trans-epoxy o-methylenedione, 5-aminobenzimidazole and 1,2-dimercapto-o-carborane enhance the stability of the molecular structure.

Benefits of technology

Significantly improves the thermal stability and anti-oxidation performance of PVC transparent film, prolongs the stability in high temperature or oxidizing environments, and provides longer-term protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a preparation method of a calcium zinc stabilizer for PVC transparent film, and relates to the field of polymer material additives. The calcium zinc stabilizer is prepared by mixing appropriate amounts of calcium salt, zinc salt, lubricant, antioxidant and synergist, and reacting and processing under specific conditions to obtain a stabilizer suitable for PVC transparent film. The stabilizer can not only effectively improve the thermal stability of the PVC transparent film, but also effectively improve its antioxidant property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer material additives, in particular to a method for preparing a calcium zinc stabilizer dedicated to PVC transparent films. Background Art

[0002] PVC (polyvinyl chloride) transparent film is widely used in food packaging, medical packaging, window film, advertising materials and other fields due to its excellent transparency, physical properties and processing performance. Transparent film has various usage scenarios and requires it to have excellent performance in chemical corrosion resistance, light stability and other aspects.

[0003] The patent with authorization announcement number CN107964250B discloses a high-efficiency composite lead salt stabilizer prepared using white smoke ash and a preparation method thereof. The high-efficiency composite lead salt stabilizer is composed of the following components by mass: 1 part of a basic lead sulfate salt complex prepared using white smoke ash, 0.1-0.5 parts of a stearated lead salt complex prepared using white smoke ash, 0.05-0.3 parts of dibasic lead phosphite, 0.04-0.3 parts of stearate, 0.04-0.3 parts of paraffin, and 0.005-0.02 parts of an antioxidant; the high-efficiency composite lead salt stabilizer is prepared using white smoke ash as the main raw material through an acid leaching modification process, a stearating process, and a compounding and molding process.

[0004] The patent with the authorization announcement number CN109825002B discloses an environmentally friendly calcium zinc stabilizer for PVC, which comprises the following components by weight: 10-30 parts of calcium salt main stabilizer, 10-30 parts of zinc salt main stabilizer, 15-25 parts of modified hydrotalcite, 10-20 parts of lubricant, 5-10 parts of modified halloysite nanotubes, 1-5 parts of antioxidant, 1-5 parts of auxiliary stabilizer and 1-5 parts of ultraviolet absorber. The environmentally friendly calcium zinc stabilizer for PVC of the invention has high stability, strong initial tinting strength and good precipitation resistance, which overcomes the defect of easy precipitation in the traditional calcium zinc processing process.

[0005] The patent with the authorization announcement number CN102391592B discloses an environmentally friendly calcium zinc stabilizer for PVC calendering film and its preparation method, which is composed of the following raw materials in mass percentage: 10-30% calcium salt main stabilizer, 10-30% zinc salt main stabilizer, 30-50% hydrotalcite, 10-20% lubricant, 5-15% thiophene heterocyclic compound, 1-5% antioxidant, 1-5% ultraviolet absorber, 1-5% auxiliary stabilizer. The preparation method of the environmentally friendly calcium zinc stabilizer for PVC calendering film is as follows: the raw materials are put into a high-speed mixer in three stages, stirred for 30 minutes at 55-56°C, and the stirrer speed is 1000-1500r / min.

[0006] However, although traditional stabilizers such as lead salts can improve the performance of PVC, they are gradually replaced by calcium-zinc composite stabilizers due to their high toxicity and harmfulness to the environment and human body. However, the existing calcium-zinc stabilizers have limited effect in improving thermal stability. Therefore, there is an urgent need for a calcium-zinc stabilizer that can both improve thermal stability and maintain the excellent performance of PVC transparent film. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a calcium zinc stabilizer for PVC transparent film to solve the problems existing in the prior art. The calcium zinc stabilizer provided by the present invention significantly improves the thermal stability of the PVC transparent film and enhances its antioxidant properties by optimizing the raw material ratio and the preparation process.

[0008] In order to achieve the above-mentioned invention object, this method proposes the following solution:

[0009] The preparation method of calcium zinc stabilizer for PVC transparent film comprises the following steps:

[0010] S1: Weigh the following raw materials by weight: 10-15 parts of calcium salt, 3-8 parts of zinc salt, 5-10 parts of lubricant, 2-5 parts of antioxidant, and 0.2-1 part of synergist;

[0011] S2: dissolving calcium salt and zinc salt in 145-160 parts of solvent, stirring evenly to obtain a mixed solution;

[0012] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50-70°C;

[0013] S4: adding antioxidant, reacting for 1-2 hours, and filtering to remove insoluble matter;

[0014] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0015] S6: crushing the calcium zinc stabilizer solid to a particle size of 10-30 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0016] Preferably, the calcium salt in S1 is one or more of calcium stearate and calcium caprate.

[0017] Preferably, the zinc salt in S1 is one or more of zinc stearate, zinc decanoate and zinc acetate.

[0018] Preferably, the lubricant in S1 is one or more of paraffin wax, polyethylene wax or stearic acid.

[0019] Preferably, the antioxidant in S1 is one or more of 2,6-di-tert-butyl-4-methylphenol (BHT), antioxidant 1010 or antioxidant 168.

[0020] Preferably, the preparation method of the synergist in S1 is:

[0021] In a stirred reactor, nitrogen is used to replace air, 20-40 parts of trans-epoxy-o-carborane and 7-14 parts of 5-aminobenzimidazole are added in an amount of weight; 10-20 parts of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) are added in an amount of weight; 200-400 parts of DMF are added; sodium ethoxide is used as a catalyst in an amount of weight ...

[0022] Preferably, the solvent in S2 is one or more of ethanol, propanol and ethyl acetate.

[0023] Preferably, the reduced pressure evaporation temperature in S5 is 40-70° C., the vacuum degree is 200-300 mbar, and the rotation speed of the rotary evaporation flask is 60-100 rpm.

[0024] Reaction mechanism: The introduction of o-dione provides the necessary functional groups for subsequent reactions through its unique chemical structure. In the reaction with 5-aminobenzimidazole, the active center of o-dione promotes the ring-opening reaction and forms a more stable intermediate.

[0025] Then, when this intermediate meets 1,2-dimercapto-o-carborane, a thiol-epoxy ring-opening reaction occurs. In this process, the structure of carborane provides additional stability for the reaction, making the entire molecular structure more robust.

[0026] Beneficial effects: This series of reactions is not just a simple chemical change, they play a key role in improving the effect of calcium zinc stabilizer. First, the addition of o-methyldione enhances the polarity of the molecule, making the entire molecule easier to interact with other substances, thereby improving the effectiveness of the stabilizer.

[0027] Secondly, the introduction of benzimidazole and carborane not only increases the thermal stability of the molecule, but also improves its antioxidant properties. This means that in high temperature or oxidative environments, this enhancer can better maintain its stability and provide longer protection for the calcium zinc stabilizer. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0029] Example 1: A method for preparing a calcium zinc stabilizer for PVC transparent film, wherein the steps are as follows:

[0030] S1: weigh the following raw materials: 10kg calcium salt, 3kg zinc salt, 5kg lubricant, 2kg antioxidant, and 0.2kg synergist;

[0031] S2: Dissolve the calcium salt and zinc salt in 145 kg of solvent and stir evenly to obtain a mixed solution;

[0032] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50°C;

[0033] S4: adding antioxidant, reacting for 1 hour, filtering to remove insoluble matter;

[0034] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0035] S6: The calcium zinc stabilizer solid is crushed to a particle size of 10 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0036] The calcium salt in S1 is calcium stearate.

[0037] The zinc salt in S1 is zinc stearate.

[0038] The lubricant in S1 is paraffin.

[0039] The antioxidant in S1 is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0040] The preparation method of the synergist in S1 is:

[0041] In a stirred reactor, nitrogen is used to replace air, 20 kg of trans-epoxy-o-carborane and 7 kg of 5-aminobenzimidazole are added, 10 kg of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) are added, 200 kg of DMF is added, and 2 kg of sodium ethoxide is used as a catalyst. The reaction is carried out at 50° C. and normal pressure. The reaction mixture is stirred for 50 minutes. The post-treatment method includes rotary evaporation to remove DMF to obtain a synergist.

[0042] The solvent in S2 is ethanol.

[0043] In the S5, the reduced pressure evaporation temperature is 40° C., the vacuum degree is 200 mbar, and the rotation speed of the rotary evaporation flask is 60 rpm.

[0044] Example 2: A method for preparing a calcium zinc stabilizer for PVC transparent film, wherein the steps are as follows:

[0045] S1: weigh the following raw materials: 12kg calcium salt, 5kg zinc salt, 7kg lubricant, 3kg antioxidant, 0.5kg synergist;

[0046] S2: dissolving calcium salt and zinc salt in 150 kg of solvent, stirring evenly to obtain a mixed solution;

[0047] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 60°C;

[0048] S4: adding antioxidant, reacting for 1 hour, filtering to remove insoluble matter;

[0049] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0050] S6: The calcium zinc stabilizer solid is crushed to a particle size of 20 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0051] The calcium salt in S1 is calcium stearate.

[0052] The zinc salt in S1 is zinc decanoate.

[0053] The lubricant in S1 is paraffin.

[0054] The antioxidant in S1 is antioxidant 1010.

[0055] The preparation method of the synergist in S1 is:

[0056] In a stirred reactor, nitrogen is used to replace air, 30 kg of trans-epoxy-o-carborane and 9 kg of 5-aminobenzimidazole are added, 13 kg of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) are added, 300 kg of DMF is added, and 6 kg of sodium ethoxide is used as a catalyst. The reaction is carried out at 55° C. and normal pressure. The reaction mixture is stirred for 75 minutes. The post-treatment method includes rotary evaporation to remove DMF to obtain a synergist.

[0057] The solvent in S2 is propanol.

[0058] In the S5, the reduced pressure evaporation temperature is 50° C., the vacuum degree is 235 mbar, and the rotation speed of the rotary evaporation flask is 75 rpm.

[0059] Example 3: A method for preparing a calcium zinc stabilizer for PVC transparent film, wherein the steps are as follows:

[0060] S1: weigh the following raw materials: 14 kg calcium salt, 6.5 kg zinc salt, 8.5 kg lubricant, 4 kg antioxidant, and 0.8 kg synergist;

[0061] S2: Dissolve the calcium salt and zinc salt in 155 kg of solvent and stir evenly to obtain a mixed solution;

[0062] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 60°C;

[0063] S4: adding antioxidant, reacting for 2 hours, filtering to remove insoluble matter;

[0064] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0065] S6: The calcium zinc stabilizer solid is crushed to a particle size of 20 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0066] The calcium salt in S1 is calcium decanoate.

[0067] The zinc salt in S1 is zinc decanoate.

[0068] The lubricant in S1 is polyethylene wax.

[0069] The antioxidant in S1 is antioxidant 168.

[0070] The preparation method of the synergist in S1 is:

[0071] In a stirred reactor, nitrogen is used to replace air, 30 kg of trans-epoxy-o-carborane and 11.5 kg of 5-aminobenzimidazole are added; 17.5 kg of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) and 300 kg of DMF are added; sodium ethoxide is used as a catalyst and its added amount is 12 kg; the reaction is carried out at 55° C. and normal pressure; the reaction mixture is stirred for 100 minutes; and a post-treatment method includes removing DMF by rotary evaporation to obtain a synergist.

[0072] The solvent in S2 is ethyl acetate.

[0073] In the S5, the reduced pressure evaporation temperature is 60° C., the vacuum degree is 250 mbar, and the rotation speed of the rotary evaporation flask is 85 rpm.

[0074] Example 4: A method for preparing a calcium zinc stabilizer for PVC transparent film, wherein the steps are as follows:

[0075] S1: weigh the following raw materials: 15kg calcium salt, 8kg zinc salt, 10kg lubricant, 5kg antioxidant, and 1kg synergist;

[0076] S2: Dissolve the calcium salt and zinc salt in 160 kg of solvent and stir evenly to obtain a mixed solution;

[0077] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 70°C;

[0078] S4: adding antioxidant, reacting for 2 hours, filtering to remove insoluble matter;

[0079] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0080] S6: The calcium zinc stabilizer solid is crushed to a particle size of 30 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0081] The calcium salt in S1 is calcium decanoate.

[0082] The zinc salt in S1 is zinc acetate.

[0083] The lubricant in S1 is paraffin.

[0084] The antioxidant in S1 is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0085] The preparation method of the synergist in S1 is:

[0086] In a stirred reactor, nitrogen is used to replace air, 40 kg of trans-epoxy-o-carborane and 14 kg of 5-aminobenzimidazole are added; 20 kg of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) are added; 400 kg of DMF is added; sodium ethoxide is used as a catalyst, and its addition amount is 15 kg; the reaction is carried out at 60° C. and normal pressure; the reaction mixture is stirred for 120 minutes; and a post-treatment method includes rotary evaporation to remove DMF to obtain a synergist.

[0087] The solvent in S2 is ethanol.

[0088] In the S5, the reduced pressure evaporation temperature is 70° C., the vacuum degree is 300 mbar, and the rotation speed of the rotary evaporator is 100 rpm.

[0089] Comparative Example 1: A method for preparing a calcium zinc stabilizer for PVC transparent film, wherein the steps are as follows:

[0090] S1: Weigh the following raw materials: 10kg calcium salt, 3kg zinc salt, 5kg lubricant, 2kg antioxidant;

[0091] S2: Dissolve the calcium salt and zinc salt in 145 kg of solvent and stir evenly to obtain a mixed solution;

[0092] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50°C;

[0093] S4: adding antioxidant, reacting for 1 hour, filtering to remove insoluble matter;

[0094] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0095] S6: The calcium zinc stabilizer solid is crushed to a particle size of 10 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0096] The calcium salt in S1 is calcium stearate.

[0097] The zinc salt in S1 is zinc stearate.

[0098] The lubricant in S1 is paraffin.

[0099] The antioxidant in S1 is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0100] The solvent in S2 is ethanol.

[0101] In the S5, the reduced pressure evaporation temperature is 40° C., the vacuum degree is 200 mbar, and the rotation speed of the rotary evaporation flask is 60 rpm.

[0102] Comparative Example 2: Preparation method of calcium zinc stabilizer for PVC transparent film, the operation steps are as follows:

[0103] S1: weigh the following raw materials: 10kg calcium salt, 3kg zinc salt, 5kg lubricant, 2kg antioxidant, and 0.2kg synergist;

[0104] S2: Dissolve the calcium salt and zinc salt in 145 kg of solvent and stir evenly to obtain a mixed solution;

[0105] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50°C;

[0106] S4: adding antioxidant, reacting for 1 hour, filtering to remove insoluble matter;

[0107] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0108] S6: The calcium zinc stabilizer solid is crushed to a particle size of 10 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0109] The calcium salt in S1 is calcium stearate.

[0110] The zinc salt in S1 is zinc stearate.

[0111] The lubricant in S1 is paraffin.

[0112] The antioxidant in S1 is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0113] The preparation method of the synergist in S1 is:

[0114] In a stirred reactor, nitrogen is used to replace air, 20 kg of trans-epoxy-o-methyldione and 7 kg of 5-aminobenzimidazole are added; 200 kg of DMF is added; 2 kg of sodium ethoxide is used as a catalyst; the reaction is carried out at 50° C. and normal pressure; the reaction mixture is stirred for 50 minutes; and a post-treatment method includes removing DMF by rotary evaporation to obtain a synergist.

[0115] The solvent in S2 is ethanol.

[0116] In the S5, the reduced pressure evaporation temperature is 40° C., the vacuum degree is 200 mbar, and the rotation speed of the rotary evaporation flask is 60 rpm.

[0117] Comparative Example 3: Preparation method of calcium zinc stabilizer for PVC transparent film, the operation steps are:

[0118] S1: weigh the following raw materials: 10kg calcium salt, 3kg zinc salt, 5kg lubricant, 2kg antioxidant, and 0.2kg synergist;

[0119] S2: Dissolve the calcium salt and zinc salt in 145 kg of solvent and stir evenly to obtain a mixed solution;

[0120] S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50°C;

[0121] S4: adding antioxidant, reacting for 1 hour, filtering to remove insoluble matter;

[0122] S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid;

[0123] S6: The calcium zinc stabilizer solid is crushed to a particle size of 10 microns to obtain a calcium zinc stabilizer specifically for PVC transparent film.

[0124] The calcium salt in S1 is calcium stearate.

[0125] The zinc salt in S1 is zinc stearate.

[0126] The lubricant in S1 is paraffin.

[0127] The antioxidant in S1 is 2,6-di-tert-butyl-4-methylphenol (BHT).

[0128] The preparation method of the synergist in S1 is:

[0129] In a stirred reactor, nitrogen is used to replace air, 20 kg of trans-epoxy-o-methyldione and 10 kg of 1,2-dimercapto-o-carborane (CAS: 23810-63-1) are added; 200 kg of DMF is added; sodium ethoxide is used as a catalyst, and its addition amount is 2 kg; the reaction is carried out at 50° C. and normal pressure; the reaction mixture is stirred for 50 minutes; and a post-treatment method includes removing DMF by rotary evaporation to obtain a synergist.

[0130] The solvent in S2 is ethanol.

[0131] In the S5, the reduced pressure evaporation temperature is 40° C., the vacuum degree is 200 mbar, and the rotation speed of the rotary evaporation flask is 60 rpm.

[0132] Test methods and results:

[0133] In order to verify the effect of the calcium zinc stabilizer of the present invention, the prepared stabilizer was systematically tested, mainly including antioxidant performance and thermal stability tests. The following are the specific test methods and test results.

[0134] 1. Antioxidant test

[0135] Equipment: Oxidation Induction Time Tester (OIT, Oxidation Induction Time)

[0136] Sample preparation: The calcium zinc stabilizers prepared in Examples 1 to 4 and Comparative Examples 1 to 3 were respectively prepared into test samples with a weight of 10 mg.

[0137] Test conditions: The sample was heated from room temperature to 200°C at a heating rate of 10°C / min in a nitrogen environment, and then oxygen was introduced at 200°C to record the oxidation induction time.

[0138] Table 1: Antioxidant test results of various embodiments and comparative examples

[0139]

[0140] The results show that the use of the calcium zinc stabilizer of the present invention has a long oxidation induction time and can effectively improve the antioxidant performance of PVC.

[0141] 2. Thermal stability test

[0142] Equipment: Thermogravimetric Analyzer (TGA)

[0143] Sample preparation: 5 parts of the calcium zinc stabilizer prepared in Examples 1-4 of the present invention and Comparative Examples 1-3 were weighed and mixed with 100 parts of PVC to prepare a transparent film. The prepared PVC transparent film was cut into small pieces weighing 10 mg for thermogravimetric analysis.

[0144] Test conditions: In a nitrogen environment, the temperature was increased from room temperature to 600°C at a heating rate of 10°C / min.

[0145] Table 2: Thermal stability test results of various embodiments and comparative examples

[0146]

[0147] It can be seen from the test results that the weight retention rate of the PVC transparent film containing the calcium zinc stabilizer of the embodiment of the present invention at different temperatures is better than that of the comparative example, indicating that its thermal stability is significantly improved.

[0148] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. The preparation method of calcium zinc stabilizer for PVC transparent film is characterized by: The operation steps are: S1: Weigh the following raw materials by weight: 10-15 parts of calcium salt, 3-8 parts of zinc salt, 5-10 parts of lubricant, 2-5 parts of antioxidant, and 0.2-1 part of synergist; S2: dissolving calcium salt and zinc salt in 145-160 parts of solvent, stirring evenly to obtain a mixed solution; S3: Add lubricant to the mixed solution, continue stirring, and maintain the temperature at 50-70°C; S4: adding antioxidant, reacting for 1-2 hours, and filtering to remove insoluble matter; S5: evaporating the reaction solution to dryness under reduced pressure to obtain a calcium zinc stabilizer solid; S6: crushing the calcium zinc stabilizer solid to a particle size of 10-30 microns to obtain a calcium zinc stabilizer for PVC transparent film; The preparation method of the synergist in S1 is: In a stirred reactor, nitrogen is used to replace air, 20-40 parts of trans-epoxy-o-carborane and 7-14 parts of 5-aminobenzimidazole are added, 10-20 parts of 1,2-dimercapto-o-carborane are added, 200-400 parts of DMF are added, and 2-15 parts of sodium ethoxide are added as a catalyst. The reaction is carried out at 50-60° C. and normal pressure. The reaction mixture is stirred for 50-120 minutes. The post-treatment method includes rotary evaporation to remove DMF to obtain a synergist.

2. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: The calcium salt in S1 is one or more of calcium stearate and calcium caprate.

3. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: The zinc salt in S1 is one or more of zinc stearate, zinc decanoate and zinc acetate.

4. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: The lubricant in S1 is one or more of paraffin wax, polyethylene wax or stearic acid.

5. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: The antioxidant in S1 is one or more of 2,6-di-tert-butyl-4-methylphenol (BHT), antioxidant 1010 or antioxidant 168.

6. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: The solvent in S2 is one or more of ethanol, propanol and ethyl acetate.

7. The method for preparing the calcium zinc stabilizer for PVC transparent film according to claim 1, characterized in that: In the S5, the reduced pressure evaporation temperature is 40-70° C., the vacuum degree is 200-300 mbar, and the rotation speed of the rotary evaporation flask is 60-100 rpm.