Determination of rubber soluble content in rubber modified asphalt mixture prepared by dry process

Through frequency scanning and multiple stress creep recovery test, the percentage of rubber dissolution in rubber modified asphalt was calculated, which solved the problem that the rubber modification effect in dry preparation of rubber modified asphalt was undetermined, and achieved high-accurate dissolution content determination , provides a basis for research on the properties of modified asphalt.

CN118501422BActive Publication Date: 2024-12-03CHANGSHA UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410601748.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-12-03
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

The degree of interaction between rubber and asphalt in the dry preparation of rubber modified asphalt is unknown, resulting in the inability to determine the modification effect and lack of effective measurement methods.

Method used

By obtaining different asphalt samples, performing frequency scanning tests and multiple stress creep recovery tests, rut factor and average stress recovery rate are calculated, and the percentage of rubber dissolution in rubber modified asphalt is obtained, and the rubber dissolution content is determined.

Benefits of technology

A simple and effective method is provided to determine the rubber dissolution content in the dry preparation of rubber modified asphalt, which improves the determination accuracy and can be widely used in the determination of the percentage of rubber dissolution in rubber modification, providing a theoretical basis for subsequent research.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118501422B_ABST
    Figure CN118501422B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for determining the rubber dissolution content in a rubber-modified asphalt mixture prepared by a dry process, the method comprising: obtaining asphalt samples prepared by different preparation methods, and performing frequency sweep tests and multiple stress creep recovery tests respectively, so as to obtain the rutting factors and average stress recovery rates corresponding to each asphalt sample at different temperatures; obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature and test according to the rutting factors and average stress recovery rates of the rubber-modified asphalt and the asphalt without rubber at the same preset temperature, and obtaining the rubber dissolution percentages in the rubber-modified asphalt of the frequency sweep test and the multiple stress creep recovery test respectively according to the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature; obtaining the target rubber dissolution content according to the rubber dissolution percentages in the rubber-modified asphalt under different tests. The present invention aims to accurately determine the rubber solubility in the dry process rubber-modified asphalt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road materials, and in particular to a method for determining the rubber dissolution content in a rubber-modified asphalt mixture prepared by a dry process. Background Art

[0002] At present, the rapid development of the transportation industry and the automobile industry has led to an increasing trend in waste tires year by year. Rubber-modified asphalt has the advantages of good road performance and green environmental protection. The methods of rubber-modified asphalt are divided into dry method and wet method. The dry process for preparing rubber-modified asphalt is simpler than the wet process, so it is more popular. However, the degree of interaction between rubber and asphalt in the process of preparing rubber-modified asphalt by dry process is unknown, and the effect of improving the performance of modified asphalt is unknown, so a measurement method is urgently needed to determine its modification effect. Summary of the invention

[0003] The main purpose of the present invention is to provide a method for determining the soluble rubber content in a rubber-modified asphalt mixture prepared by a dry process, aiming to solve the technical problem that the modification effect of rubber in the existing modified asphalt cannot be determined.

[0004] To achieve the above object, the present invention provides a method for determining the soluble rubber content in a rubber-modified asphalt mixture prepared by a dry process, the method comprising the following steps:

[0005] Step 1, obtaining asphalt samples, wherein the samples include base asphalt, rubber-modified asphalt obtained by wet process, rubber-modified asphalt obtained by dry process extraction, and base asphalt obtained by extracting ordinary asphalt mixture;

[0006] Step 2, subjecting the asphalt samples in step 1 to a frequency sweep test and a multiple stress creep recovery test at a preset temperature to obtain the rutting factor and average stress recovery rate corresponding to each sample at different temperatures;

[0007] Step 3, obtaining asphalt rutting factor coefficients of dry process and wet process at corresponding temperatures according to the rutting factor of rubber-modified asphalt and the rutting factor of rubber-free asphalt at the same preset temperature in step 2, and obtaining the rubber dissolution percentage in the rubber-modified asphalt under the frequency sweep test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature;

[0008] Step 4, obtaining asphalt rutting factor coefficients of dry process and wet process at corresponding temperatures according to the average stress recovery rate of rubber-modified asphalt and the average stress recovery rate of rubber-free asphalt at the same preset temperature in step 2, and obtaining the rubber dissolution percentage in the rubber-modified asphalt under the multiple stress creep recovery test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature;

[0009] Step 5, weighted calculation of the rubber solubility percentage in the rubber modified asphalt in step 3 and step 4 to obtain the target rubber solubility content.

[0010] Optionally, in step 3, the specific step of obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature according to the rutting factor of the rubber-modified asphalt and the rutting factor of the rubber-free asphalt at the same preset temperature in step 2 comprises:

[0011] Step 31, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the rutting factor of the rubber modified asphalt obtained by the wet process at the same preset temperature to the rutting factor of the base asphalt;

[0012] Step 32, according to the same preset temperature, the rutting factor of the rubber modified asphalt extracted by the dry process is compared with the rutting factor of the base asphalt extracted by the ordinary asphalt mixture to obtain the asphalt rutting factor coefficient at the corresponding temperature of the dry process.

[0013] Optionally, in step 3, the specific step of obtaining the percentage of rubber dissolved in the rubber-modified asphalt under the frequency sweep test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature includes:

[0014] Step 33, weighted calculation is performed on the ratio of the asphalt rutting factor coefficients of the dry process and the wet process at the same temperature to obtain the rubber dissolution percentage in the rubber modified asphalt under the frequency sweep test.

[0015] Optionally, in step 4, the specific step of obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature according to the average stress recovery rate of the rubber-modified asphalt and the average stress recovery rate of the rubber-free asphalt at the same preset temperature in step 2 includes:

[0016] Step 41, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the average stress recovery rate of the rubber modified asphalt obtained by the wet process at the same preset temperature to the average stress recovery rate of the base asphalt;

[0017] Step 42, according to the average stress recovery rate of the rubber modified asphalt extracted by the dry process at the same preset temperature, and the average stress recovery rate of the base asphalt extracted by the ordinary asphalt mixture, the asphalt rutting factor coefficient at the corresponding temperature of the dry process is obtained.

[0018] Optionally, in step 4, the specific step of obtaining the percentage of rubber dissolved in the rubber modified asphalt under the multiple stress creep recovery test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature includes:

[0019] Step 43, weighted calculation is performed on the ratio of the average stress recovery rate of the dry process and the average stress recovery rate of the wet process at the same temperature to obtain the percentage of rubber dissolved in the rubber modified asphalt under the multiple stress creep recovery test.

[0020] Optionally, in step 2, the asphalt samples in step 1 are subjected to frequency sweep tests at preset temperatures to obtain the complex shear modulus G corresponding to each sample at different temperatures. * and phase angle δ, and according to the complex shear modulus G * The rutting factor corresponding to each sample at different temperatures is obtained by using the phase angle δ, where rutting factor = G * / sinδ.

[0021] Optionally, in step 2, the preset temperature of the frequency sweep test and the multiple stress creep recovery test is 58-64°C.

[0022] Optionally, in step 1, the rubber content in the rubber-modified asphalt produced by the wet process and the rubber-modified asphalt produced by the dry process is 10%.

[0023] Optionally, in step 1, the mass proportion of old asphalt in the rubber modified asphalt extracted by dry process is 17-25%, and the mass proportion of old asphalt in the base asphalt extracted by ordinary asphalt mixture is 17-25%.

[0024] Optionally, in step 1, the base asphalt grade is PG58-34.

[0025] Beneficial effects:

[0026] The present invention provides a method for determining the rubber dissolution content in a rubber-modified asphalt mixture prepared by a dry process, by obtaining different asphalt samples, and performing frequency sweep tests and multiple stress creep recovery tests at preset temperatures, respectively, to obtain the rutting factors and average stress recovery rates corresponding to each sample at different temperatures, and based on the ratio of the corresponding rutting factors and average stress recovery rates between the rubber-modified asphalt obtained by dry process extraction at the same temperature / the rubber-modified asphalt and the rubber-free asphalt in the wet process, to obtain the rutting factor coefficients under different tests, and finally weighted calculation of the rutting factor coefficients under different tests, to finally obtain the target rubber dissolution content. Then, the present invention can intuitively show from the asphalt performance test results that the rubber-modified asphalt can improve the rutting factor coefficient and the rutting recovery rate, indirectly reflecting the mutual dissolution content of the rubber asphalt, and the percentage of the rubber left in the total amount of rubber after extraction is the rubber dissolution percentage. The whole calculation process is simple and convenient, and does not require the use of complex equipment, so that the final obtained rubber dissolution percentage accuracy is higher than the prior art, and can be widely used in the determination of the rubber dissolution percentage in a variety of rubber modifications, providing a theoretical basis for further research on the performance of modified asphalt in the future. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic flow chart of a first embodiment of a method for determining the soluble rubber content in a rubber-modified asphalt mixture prepared by a dry method according to the present invention;

[0028] Figure 2 It is the linear fitting diagram of rutting factor and rubber content;

[0029] Figure 3 It is the linear fitting diagram of average stress recovery rate and rubber content;

[0030] Figure 4 is the complex shear modulus G of the asphalt sample that changes with temperature * picture;

[0031] Figure 5 is the phase angle δ diagram of asphalt sample changing with temperature;

[0032] Figure 6 is the rutting factor G of the asphalt sample that changes with temperature * / sinδ graph;

[0033] Figure 7 This is the stress recovery rate diagram of asphalt sample under stress state changing with temperature.

[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0035] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0036] Reference Figure 1 , a flow chart of a first embodiment is provided for a method for determining the soluble rubber content in a rubber-modified asphalt mixture prepared by a dry process of the present invention, the method comprising:

[0037] Step 1, obtaining an asphalt sample, wherein the sample includes base asphalt, rubber-modified asphalt obtained by a wet process, rubber-modified asphalt obtained by a dry process, and base asphalt obtained by extracting a common asphalt mixture. Specifically, the base asphalt grade is PG58-34, and the rubber content in the rubber-modified asphalt obtained by a wet process and the rubber-modified asphalt obtained by a dry process is greater than 0 and less than or equal to 20%, preferably 10%. And the mass proportion of old asphalt in the rubber-modified asphalt obtained by the dry process is 17-25%, and the mass proportion of old asphalt in the base asphalt obtained by extracting a common asphalt mixture is 17-25%. The rubber is mostly waste tires, and then the waste tires are processed into rubber powder for asphalt modification, which can effectively reduce environmental pollution and reduce the production cost of modified asphalt.

[0038] Step 2: Perform a frequency sweep test and a multiple stress creep recovery test on the asphalt samples in step 1 at a preset temperature to obtain the rutting factor and the average stress recovery rate corresponding to each sample at different temperatures. The asphalt samples in step 1 are subjected to a frequency sweep test at a preset temperature to obtain the complex shear modulus G corresponding to each sample at different temperatures. * and phase angle δ, and according to the complex shear modulus G * The rutting factor corresponding to each sample at different temperatures is obtained by using the phase angle δ, where rutting factor = G * / sinδ, and the rubber content is in direct proportion to the rutting factor, and the rubber content is in direct proportion to the average stress recovery rate. The preset temperature of the frequency sweep test is 34-82°C, and the preset temperature of the multiple stress creep recovery test is 52-76°C. Preferably, the preset temperature of the frequency sweep test and the multiple stress creep recovery test is 58-64°C.

[0039] Step 3, obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature based on the rutting factor of the rubber-modified asphalt and the rutting factor of the rubber-free asphalt at the same preset temperature in step 2, and obtaining the rubber solubility percentage in the rubber-modified asphalt under the frequency scanning test based on the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature.

[0040] Specifically, the step of obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature according to the rutting factor of the rubber-modified asphalt and the rutting factor of the rubber-free asphalt at the same preset temperature in step 2 specifically includes:

[0041] Step 31, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the rutting factor of the rubber modified asphalt obtained by the wet process at the same preset temperature to the rutting factor of the base asphalt.

[0042] Step 32, according to the same preset temperature, the rutting factor of the rubber modified asphalt extracted by the dry process is compared with the rutting factor of the base asphalt extracted by the ordinary asphalt mixture to obtain the asphalt rutting factor coefficient at the corresponding temperature of the dry process.

[0043] Specifically, the rutting factor F of rubber modified asphalt under the frequency sweep test is CZ The calculation formula is

[0044]

[0045] In the formula [G * / sinδ] 橡胶改性is the rutting factor of the rubber modified asphalt extracted by dry process or the rubber modified asphalt obtained by wet process, [G * / sinδ] 不含橡胶 The rutting factor of the base asphalt or base asphalt extracted from ordinary asphalt mixture. The rutting factor coefficient of the rubber modified asphalt extracted by dry process at T1 temperature is F CZG-T1 The rutting factor coefficient of the rubber modified asphalt extracted by dry process at T2 temperature is expressed as F CZG-T2 The rutting factor coefficient of the modified asphalt prepared by the wet process at T1 temperature is expressed by F CZS-T1 The rutting factor coefficient of the modified asphalt prepared by dry process at T2 temperature is expressed by F CZS-T2 express.

[0046] The specific steps of obtaining the percentage of rubber dissolved in the rubber modified asphalt under the frequency sweep test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature include:

[0047] Step 33, weighted calculation is performed on the ratio of the asphalt rutting factor coefficients of the dry process and the wet process at the same temperature to obtain the rubber dissolution percentage in the rubber modified asphalt under the frequency sweep test. Specifically, the coefficients at temperatures T1 and T2 are highly correlated, and then the weighted average calculation is performed to obtain the rubber dissolution percentage IRP in the asphalt binder. cz , the specific formula is:

[0048]

[0049] Step 4, according to the average stress recovery rate of the rubber-modified asphalt at the same preset temperature and the average stress recovery rate of the rubber-free asphalt in step 2, the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature are obtained, and according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature, the rubber dissolution percentage in the rubber-modified asphalt under the multiple stress creep recovery test is obtained.

[0050] Specifically, the specific steps of obtaining the asphalt rutting factor coefficients of the dry process and the wet process at the corresponding temperature according to the average stress recovery rate of the rubber-modified asphalt and the average stress recovery rate of the rubber-free asphalt at the same preset temperature in step 2 include:

[0051] Step 41, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the average stress recovery rate of the rubber modified asphalt obtained by the wet process at the same preset temperature to the average stress recovery rate of the base asphalt;

[0052] Step S42, according to the average stress recovery rate of the rubber modified asphalt extracted by the dry process at the same preset temperature, and the average stress recovery rate of the base asphalt extracted by the ordinary asphalt mixture, the asphalt rutting factor coefficient at the corresponding temperature of the dry process is obtained.

[0053] Among them, the rutting factor coefficient F of rubber modified asphalt under multiple stress creep recovery test is R The calculation formula is

[0054]

[0055] Where [R_0.1] 橡胶改性 is the average stress recovery rate of rubber modified asphalt extracted by dry process or rubber modified asphalt obtained by wet process, [R_0.1] 不含橡胶 F is the average stress recovery rate of the base asphalt or base asphalt extracted from the ordinary asphalt mixture, and the rutting factor coefficient of the rubber modified asphalt extracted by the dry process at T1 temperature is F RG-T1 The rutting factor coefficient of the rubber modified asphalt extracted by dry process at T2 temperature is expressed as F RG-T2 The rutting factor coefficient of the modified asphalt prepared by the wet process at T1 temperature is expressed by F RS-T1 The rutting factor coefficient of the modified asphalt prepared by dry process at T2 temperature is expressed by F RS-T2 express.

[0056] The specific steps of obtaining the rubber dissolution percentage in the rubber modified asphalt under the multiple stress creep recovery test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature include:

[0057] Step 43, weighted calculation is performed on the ratio of the average stress recovery rate of the dry process and the average stress recovery rate of the wet process at the same temperature to obtain the percentage of rubber dissolved in the rubber modified asphalt under the multiple stress creep recovery test.

[0058] Specifically, the coefficients at temperatures T1 and T2 are highly correlated, and the weighted average calculation is then performed to obtain the rubber dissolution percentage IRP in the asphalt binder under the multiple stress creep recovery test: R , the specific formula is:

[0059]

[0060] Step 5, weighted calculation of the rubber solubility percentage in the rubber modified asphalt in step 3 and step 4 to obtain the target rubber solubility content.

[0061] Specifically, the weighted average of the rubber dissolution percentages obtained under the above two experiments is used to obtain the target rubber dissolution percentage. The specific formula is:

[0062]

[0063] In this embodiment, by obtaining different asphalt samples, and performing frequency sweep tests and multiple stress creep recovery tests at preset temperatures, the rutting factors and average stress recovery rates corresponding to each sample at different temperatures are obtained, and based on the ratio of the corresponding rutting factors and average stress recovery rates between the rubber modified asphalt extracted by the dry process / the rubber modified asphalt and the rubber-free asphalt in the wet process at the same temperature, the rutting factor coefficients under different tests are obtained, and finally the rutting factor coefficients under different tests are weighted and calculated to finally obtain the target rubber dissolution content. The whole calculation process is simple and convenient, and no complex equipment is used, so that the final rubber dissolution percentage accuracy is higher than that of the prior art, and it can be widely used in the determination of the rubber dissolution percentage in various rubber modifications, providing a theoretical basis for further research on the performance of modified asphalt. For example, it can be used to guide the rubber modified asphalt material preparation factory to produce high-performance dry-process rubber modified asphalt mixtures; it can also guide the variables of rubber addition according to performance requirements, and then dry-process rubber modified asphalt mixtures with different performance requirements can be prepared; finally, it provides a basis for guiding the regeneration of aged rubber modified asphalt mixtures.

[0064] Further, in order to better illustrate the specific effect of the method for determining the rubber soluble content in the rubber-modified asphalt mixture prepared by the dry method of the present invention, the following is described in detail through specific examples:

[0065] Example 1

[0066] The method of the present invention is used to test the sample asphalt to determine the corresponding data, and the obtained data is linearly fitted. The fitting data after fitting are shown in Table 1 and the fitting graph is shown in Figure 2-3 As shown, it can be seen that the rubber content and the rutting factor are in direct proportion, and the rubber content and the average stress recovery rate are also in direct proportion, which provides a theoretical premise for the establishment of subsequent formulas.

[0067] Table 1-Linear fitting data of rubber content and rutting factor

[0068]

[0069] Note: x refers to the percentage of rubber content

[0070] Example 2

[0071] 1. Prepare test materials.

[0072] Ordinary asphalt mixture 1, rubber modified asphalt mixture prepared by dry process 1. The parameters of the two asphalt mixtures are shown in Table 2.

[0073] Table 2 shows the test material parameters

[0074]

[0075] The above two asphalt mixtures were subjected to extraction procedures, and two asphalt samples were added, namely base asphalt and laboratory wet process to prepare completely dissolved rubber modified asphalt. The above four asphalt binder grades are all PG58-34, and the rubber content is 10% of the asphalt binder weight.

[0076] 2. Conduct experiments to obtain test parameters.

[0077] The above four asphalts were subjected to frequency sweep test and multiple stress creep recovery test (MSCR) on a dynamic shear instrument at 34-82°C according to the regulations. Among them, the experimental parameters obtained for the frequency sweep test are: complex shear modulus G * and phase angle δ and rutting factor G * / si nδ, where Figure 2 The figure shows the change of rutting factor with rubber content. Figure 3 The figure shows the change of average stress rate with rubber content at 0.1kPa. Figure 4 The figure shows the change of complex shear modulus of the samples at 34-82°C. As the scanning frequency increases, the complex shear modulus of each asphalt shows an upward trend. Among them, the complex shear modulus of the base asphalt extracted from ordinary asphalt mixture 1 is in the middle range compared with other asphalts, and the complex shear modulus of the base asphalt extracted from ordinary asphalt mixture 2 is higher than other asphalts. Figure 5 The data for the phase angle measurement of the sample is converted to frequency. As the scanning frequency increases, the phase angle shows a trend of first increasing and then decreasing. At low frequencies, the extracted asphalt has a higher phase angle than the base asphalt. At high frequencies, the extracted asphalt has a lower phase angle than the base asphalt. The difference in phase angle between the base asphalt extracted from ordinary asphalt mixture 1 and ordinary asphalt mixture 2 is the smallest. Similar to the base asphalt and the laboratory wet-process rubber-modified asphalt, the asphalt extracted from the rubber-containing mixture has a lower phase angle than the asphalt extracted from the non-rubber mixture. It can be seen that at a conversion frequency of 10 -2 When the phase angle of each sample is around HZ, it tends to be stable. Figure 6The figure shows the change of the rutting factor of the sample at 34-82℃. It can be seen from the figure that ① the rutting factor shows a decreasing trend with the increase of temperature. ② The rutting factor of the base asphalt is the lowest. ③ The rutting factor value of the base asphalt extracted from the ordinary asphalt mixture is lower than the rutting factor of the asphalt extracted from the rubber-containing asphalt mixture. ④ The rutting factor of the rubber-modified asphalt prepared by the laboratory wet method is lower at low temperatures and higher at high temperatures. For the multiple stress creep recovery test, the experimental parameters are: the average stress recovery rate R, such as Figure 7 The figure shows the change of the average stress recovery rate of the samples at 34-82℃. It can be seen from the figure that ① the stress recovery rate decreases with the increase of temperature. ② Among them, the stress recovery rate of rubber modified asphalt prepared by laboratory wet method is the highest. ③ Under high stress levels, asphalt binder is more likely to undergo irreversible deformation. Therefore, as the stress level increases, the recovery rate deteriorates. ④ Under lower stress conditions, the base asphalt extracted from ordinary asphalt mixture has similar recovery performance to the base asphalt.

[0078] 3. Calculate the soluble rubber content in the dry-process rubber-modified asphalt.

[0079] 1) Calculate the rubber dissolution content under the frequency sweep test.

[0080] ① Calculate the asphalt rutting factor F under the frequency sweep test CZ .

[0081]

[0082] In the formula [G * / sinδ] 橡胶改性 The rutting factor of the rubber modified asphalt extracted by dry process or the rubber modified asphalt obtained by wet process; [G * / sinδ] 不含橡胶 It is the base asphalt extracted from ordinary asphalt mixture or the rutting factor of base asphalt.

[0083] according to Figure 6 The rutting factors shown vary with temperature. In this embodiment, the rutting factors of the base asphalt obtained at 58°C and 64°C, the rubber modified asphalt prepared by the wet process, the base asphalt 1 extracted from ordinary asphalt mixture, and the rubber modified asphalt 1 extracted by the dry process are summarized in Table 3.

[0084] Table 3 shows the rutting factors of asphalt samples at 58℃ and 64℃

[0085]

[0086] According to formula 1, the rutting factor of the rubber modified asphalt 1 extracted by dry process in Table 3 is compared with the base asphalt 1 extracted from ordinary asphalt mixture to obtain the rutting factor coefficient F CZ .

[0087] The detailed calculation process is as follows:

[0088]

[0089] F CZG-58 : Rutting factor coefficient of rubber modified asphalt 1 obtained by dry extraction at 58°C;

[0090] [G * / si nδ] 橡胶改性1 : Rutting factor of rubber modified asphalt 1 extracted by dry process at 58℃; [G * / si nδ] 不含橡胶1 : The rutting factor of base asphalt 1 was obtained by extracting ordinary asphalt mixture at 58°C.

[0091]

[0092] F CZS-58 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃; [G * / si nδ] 橡胶改性2 : Rutting factor of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃;

[0093] [G * / si nδ] 不含橡胶2 : Rutting factor of base asphalt at 58℃.

[0094] Similarly, the rutting factor coefficients of dry and wet rubber modified asphalt at 64°C are calculated as follows:

[0095]

[0096]

[0097] [G * / si nδ] 橡胶改性3 : Rutting factor of rubber modified asphalt 1 extracted by dry process at 64℃; [G * / si nδ] 不含橡胶3 : Rutting factor of base asphalt 1 obtained by extraction of common asphalt mixture at 64℃; [G * / si nδ] 橡胶改性4 : Rutting factor of completely dissolved rubber modified asphalt obtained by laboratory wet process at 64℃;

[0098] [G* / si nδ] 不含橡胶4 : Rutting factor of base asphalt at 64℃;

[0099] F CZG-64 : Rutting factor coefficient of rubber modified asphalt 1 obtained by dry extraction at 64°C; F CZS-64 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 64℃.

[0100] ② Calculate the rubber dissolution percentage IRP in the dry preparation of rubber modified asphalt under the frequency sweep test cz .

[0101]

[0102] Where F CZG-58 is the rutting factor coefficient of rubber modified asphalt 1 obtained by dry extraction at 58°C,

[0103] F CZG-64 is the rutting factor coefficient of rubber modified asphalt 1 obtained by dry extraction at 64°C, F CZS-58 is the rutting factor coefficient of rubber modified asphalt prepared by wet process at 58℃,

[0104] F CZS-64 It is the rutting factor coefficient of rubber modified asphalt prepared by wet process at 64℃.

[0105] According to formula 2, the calculation result in ① is substituted into formula 2. The detailed calculation process is as follows:

[0106]

[0107] 2) Calculate the rubber dissolution content under the multiple stress creep test (MSCR).

[0108] ① Calculate the asphalt rutting factor F under the MSCR test CZ .

[0109]

[0110] Where [R_0.1] 橡胶改性 The average stress recovery rate of the rubber modified asphalt extracted by dry process or the rubber modified asphalt obtained by wet process at 0.1kPa, [R_0.1] 不含橡胶 It is the average stress recovery rate of base asphalt extracted from ordinary asphalt mixture or base asphalt at 0.1kPa. Figure 7The average stress recovery rates of the base asphalt, rubber modified asphalt prepared by wet process, rubber modified asphalt 1 obtained by dry process extraction, and base asphalt 1 extracted from ordinary asphalt mixture under 0.1 kPa stress state are listed in Table 4.

[0111] Table 4 - Average stress recovery rates of samples at 58°C and 64°C

[0112]

[0113] According to Formula 3, the rutting factor coefficient F is obtained by comparing the average stress recovery rate of the rubber modified asphalt 1 extracted by the dry process in Table 4 under a stress of 0.1 kPa with the average stress recovery rate of the base asphalt 1 extracted from the ordinary asphalt mixture under a stress of 0.1 kPa. R The detailed calculation process is as follows:

[0114]

[0115] F RG-58 : Rutting factor coefficient of rubber modified asphalt 1 extracted by dry process at 58℃ under 0.1kPa stress;

[0116] [R_0.1] 橡胶改性1 : Average stress recovery rate of rubber modified asphalt 1 extracted by dry process at 58°C at 0.1kPa;

[0117] [R_0.1] 不含橡胶1 : The average stress recovery rate of matrix asphalt 1 at 0.1 kPa was obtained by extracting ordinary asphalt mixture at 58°C.

[0118]

[0119] F RS-58 :Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃ under 0.1kPa stress;

[0120] [R_0.1] 橡胶改性2 :Average stress recovery rate of rubber modified asphalt prepared by wet method in laboratory at 58℃ under 0.1kPa;

[0121] [R_0.1] 不含橡胶2 : Average stress recovery rate of matrix asphalt at 0.1 kPa at 58 °C.

[0122] Similarly, calculate the rutting factor coefficient of dry and wet process rubber asphalt at 64℃:

[0123]

[0124]

[0125] [R_0.1] 橡胶改性3 :Average stress recovery rate of rubber modified asphalt 1 extracted by dry process at 64℃ at 0.1kPa; [R_0.1] 不含橡胶3 :The average stress recovery rate of base asphalt 1 at 0.1 kPa obtained by extracting ordinary asphalt mixture at 64°C; [R_0.1] 橡胶改性4 : Average stress recovery rate of rubber modified asphalt prepared by wet method in laboratory at 64℃ under 0.1kPa;

[0126] [R_0.1] 不含橡胶4 : Average stress recovery rate of matrix asphalt at 0.1 kPa at 64 °C;

[0127] F RG-64 : Rutting factor coefficient of rubber modified asphalt 1 extracted by dry process at 64℃ under 0.1kPa stress; F RS-64 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 64℃ under 0.1kPa stress.

[0128] ② Calculate the rubber dissolution percentage I RP in the dry-process rubber asphalt under the MSCR test R

[0129]

[0130] Where F RG-58 is the rutting factor coefficient of rubber modified asphalt 1 extracted by dry process at 58℃ under 0.1kPa stress,

[0131] F RG-64 is the rutting factor coefficient of rubber modified asphalt 1 extracted by dry process at 64℃ under 0.1kPa stress,

[0132] F RS-58 The rutting factor coefficient of rubber modified asphalt 1 prepared by wet process at 58°C under 0.1kPa stress is:

[0133] F RS-64 The rutting factor coefficient of rubber modified asphalt 1 prepared by wet process at 64°C under 0.1 kPa stress.

[0134] According to formula 4, the calculation result in ① is substituted into formula 4, and the detailed calculation is as follows:

[0135]

[0136] 4. Determine the final rubber dissolution content. The specific formula is:

[0137]

[0138] where I RP CZ is the rubber solubility coefficient in rubber modified asphalt 1 obtained by dry extraction under frequency sweep test; IRP R It is the rubber solubility coefficient in rubber modified asphalt 1 obtained by dry extraction under multiple stress creep recovery test.

[0139] The rubber dissolution percentage I RP in the dry-process rubber-modified asphalt prepared under the frequency sweep test calculated in 3 is CZ Rubber dissolution percentage in rubber modified asphalt prepared by dry method under IRP and MSCR test R The final rubber dissolution content was obtained by weighted average calculation.

[0140]

[0141] Example 3:

[0142] 1. Preparation of experimental materials.

[0143] On the basis of Example 1, the asphalt mixture samples prepared by dry process are replaced, that is, ordinary asphalt mixture 2 and rubber modified asphalt mixture 2 prepared by dry process are used. The design information of the two mixtures is shown in Table 5.

[0144] Table 5 shows the parameters of the sample asphalt

[0145]

[0146] The above asphalt mixture was subjected to extraction process. Two asphalt samples were also added, namely base asphalt and laboratory wet process to prepare completely dissolved rubber modified asphalt. The above four asphalt binder grades are PG58-34, and the rubber content is 10% of the asphalt binder weight.

[0147] 2. Conduct experiments to obtain test parameters.

[0148] The above four asphalts were subjected to frequency sweep test and multiple stress creep recovery test (MSCR) on a dynamic shear instrument according to the regulations. The experimental parameters obtained for the frequency sweep test are: complex shear modulus G * and phase angle δ and rutting factor G * / si nδ, Figure 4 The figure shows the change of complex shear modulus of the sample at 34-82℃. Figure 5 The data of the phase angle of the sample is measured by the conversion frequency. It can be seen that when the conversion frequency is 10 -2 When the phase angle of each sample is around HZ, it tends to be stable. Figure 6The figure shows the change of the rutting factor of the sample at 34-82℃. For the multiple stress creep recovery test, the experimental parameters are: the average stress recovery rate R, such as Figure 7 Shown is the change in the average stress recovery rate of the samples at 34-82°C.

[0149] 3. Calculate the soluble rubber content in the dry-process rubber-modified asphalt.

[0150] 1) Calculate the rubber dissolution content under the frequency sweep test.

[0151] ① Calculate the rutting factor F of asphalt binder under frequency sweep test CZ .

[0152]

[0153] In the formula [G * / sinδ] 橡胶改性 The rutting factor of the rubber modified asphalt extracted by dry process or the rubber modified asphalt obtained by wet process; [G * / sinδ] 不含橡胶 It is the base asphalt extracted from ordinary asphalt mixture or the rutting factor of base asphalt.

[0154] according to Figure 6 The rutting factors shown vary with temperature. In this embodiment, the rutting factors of the base asphalt obtained at 58°C and 64°C, the rubber-modified asphalt prepared by the wet method, the base asphalt 2 extracted from ordinary asphalt mixture, and the rubber-modified asphalt 2 extracted by the dry method are summarized in Table 6.

[0155] Table 6 shows the rutting factors of asphalt samples at 58℃ and 64℃

[0156]

[0157] According to Formula 6, the rutting factor coefficient F is obtained by comparing the rutting factor of the rubber modified asphalt 2 extracted by the dry process in Table 6 with the rutting factor of the base asphalt 2 extracted from the ordinary asphalt mixture. CZ The detailed calculation process is as follows:

[0158]

[0159] F CZG-58 : Rutting factor coefficient of rubber modified asphalt 2 obtained by dry extraction at 58°C;

[0160] [G * / si nδ] 橡胶改性1 : Rutting factor of rubber modified asphalt 2 obtained by dry extraction at 58°C; [G * / s inδ]不含橡胶1 : The rutting factor of base asphalt 2 was obtained by extracting ordinary asphalt mixture at 58℃.

[0161]

[0162] F CZS-58 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃;

[0163] [G * / si nδ] 橡胶改性2 : The completely dissolved rubber modified asphalt rutting factor was obtained by laboratory wet process at 58℃;

[0164] [G * / si nδ] 不含橡胶2 : Rutting factor of base asphalt at 58℃.

[0165] Similarly, the rutting factor coefficients of dry and wet rubber modified asphalt at 64°C are calculated as follows:

[0166]

[0167]

[0168] [G * / si nδ] 橡胶改性3 : Rutting factor of rubber modified asphalt 2 extracted by dry process at 64℃; [G * / si nδ] 不含橡胶3 : The rutting factor of base asphalt 2 was obtained by extracting ordinary asphalt mixture at 64℃;

[0169] [G * / si nδ] 橡胶改性4 : The rutting factor of completely dissolved rubber modified asphalt was obtained by laboratory wet process at 64℃;

[0170] [G * / si nδ] 不含橡胶4 : Rutting factor of base asphalt at 64℃;

[0171] F CZG-64 : Rutting factor coefficient of rubber modified asphalt 2 obtained by dry extraction at 64°C;

[0172] F CZS-58 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃.

[0173] ② Calculate the rubber dissolution percentage IRP in the dry preparation of rubber modified asphalt under the frequency sweep test cz .

[0174]

[0175] Where F CZG-58 is the rutting factor coefficient of rubber modified asphalt 2 obtained by dry extraction at 58°C,

[0176] F CZG-64 is the rutting factor coefficient of rubber modified asphalt 2 obtained by dry extraction at 64°C, F CZS-58 is the rutting factor coefficient of rubber modified asphalt prepared by wet process at 58℃,

[0177] F CZS-64 It is the rutting factor coefficient of rubber modified asphalt prepared by wet process at 64℃.

[0178] According to formula 7, the calculation result in ① is substituted into formula 7. The detailed calculation process is as follows:

[0179]

[0180] 2) Calculate the rubber dissolution content under the multiple stress creep test (MSCR).

[0181] ① Calculate the rutting factor F of asphalt binder under MSCR test CZ .

[0182]

[0183] Where [R_0.1] 橡胶改性 The average stress recovery rate of the rubber modified asphalt extracted by dry process or the rubber modified asphalt obtained by wet process at 0.1kPa,

[0184] [R_0.1] 不含橡胶 It is the average stress recovery rate of base asphalt extracted from ordinary asphalt mixture or base asphalt at 0.1kPa.

[0185] according to Figure 7 The average stress recovery rates of base asphalt, rubber modified asphalt prepared by wet process, rubber modified asphalt 2 obtained by dry process extraction, and base asphalt 2 extracted from ordinary asphalt mixture under 0.1 kPa stress state are listed in Table 7.

[0186] Table 7 - Average stress recovery rates of samples at 58°C and 64°C

[0187]

[0188] According to Formula 8, the rutting factor coefficient F is obtained by comparing the average stress recovery rate of the rubber modified asphalt 2 extracted by the dry process in Table 7 under a stress of 0.1 kPa with the average stress recovery rate of the base asphalt 2 extracted from the ordinary asphalt mixture under a stress of 0.1 kPa.R The detailed calculation process is as follows:

[0189]

[0190] F RG-58 : Rutting factor coefficient of rubber modified asphalt 2 extracted by dry process at 58°C under 0.1kPa stress;

[0191] [R_0.1] 橡胶改性1 : Average stress recovery rate of rubber modified asphalt 2 extracted by dry process at 58°C at 0.1kPa;

[0192] [R_0.1] 不含橡胶1 : The average stress recovery rate of matrix asphalt 2 at 0.1 kPa was obtained by extracting ordinary asphalt mixture at 58°C.

[0193]

[0194] F RS-58 : Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 58℃;

[0195] [R_0.1] 橡胶改性2 :Average stress recovery rate of rubber modified asphalt prepared by wet method in laboratory at 58℃ under 0.1kPa;

[0196] [R_0.1] 不含橡胶2 : Average stress recovery rate of matrix asphalt at 0.1 kPa at 58 °C.

[0197] Similarly, the rutting factor coefficients of rubber modified asphalt prepared by dry and wet processes at 64°C are calculated as follows:

[0198]

[0199]

[0200] [R_0.1] 橡胶改性3 :Average stress recovery rate of rubber modified asphalt 2 extracted by dry process at 64℃ at 0.1kPa; [R_0.1] 不含橡胶3 :The average stress recovery rate of matrix asphalt 2 at 0.1 kPa obtained by extracting ordinary asphalt mixture at 64°C; [R_0.1] 橡胶改性4 : Average stress recovery rate of rubber modified asphalt prepared by wet method in laboratory at 64℃ under 0.1kPa;

[0201] [R_0.1] 不含橡胶4 : Average stress recovery rate of matrix asphalt at 0.1 kPa at 64 °C;

[0202] FRG-64 : Rutting factor coefficient of rubber modified asphalt 2 extracted by dry process at 64℃ under 0.1kPa stress;

[0203] F RS-64 :Rutting factor coefficient of completely dissolved rubber modified asphalt prepared by laboratory wet process at 64℃ under 0.1kPa stress;

[0204] ② Calculate the rubber dissolution percentage I RP in the dry-process rubber-modified asphalt under the MSCR test R

[0205]

[0206] Where F RG-58 is the rutting factor coefficient of rubber modified asphalt 2 extracted by dry process at 58°C under 0.1kPa stress,

[0207] F RG-64 is the rutting factor coefficient of rubber modified asphalt 2 extracted by dry process at 64℃ under 0.1kPa stress,

[0208] F RS-58 is the rutting factor coefficient of rubber modified asphalt 2 extracted at 58℃ under 0.1kPa stress,

[0209] F RS-64 The rutting factor coefficient of rubber modified asphalt 2 prepared by wet process at 64°C under 0.1 kPa stress.

[0210] According to formula 9, the calculation result in ① is substituted into formula 4, and the detailed calculation is as follows:

[0211]

[0212] 4. Determine the final rubber dissolution content. The specific formula is:

[0213]

[0214] where I RP CZ is the rubber solubility coefficient of rubber modified asphalt 2 obtained by dry extraction under frequency sweep test; I RP R It is the rubber solubility coefficient of rubber modified asphalt 2 obtained by dry extraction under multiple stress creep recovery test.

[0215] The rubber dissolution percentage I RP in the dry-process rubber-modified asphalt prepared under the frequency sweep test calculated in 3 is CZ Rubber dissolution percentage in dry-process rubber asphalt prepared under I RP and MSCR test R The final rubber dissolution content was obtained by weighted average calculation.

[0216]

[0217] The rubber soluble content in the rubber modified asphalt 1 obtained by dry extraction obtained from Examples 2-3 and the rubber soluble content in the rubber modified asphalt 2 obtained by dry extraction. The final soluble contents were determined to be 57.59% and 61.96% respectively, and the final structures obtained were not much different, and the feasibility of the determination method of the present invention was supported by data. That is, the method of the present invention can effectively reflect the rubber soluble content in the rubber modified asphalt prepared by the dry process. In addition, except for the case where the rubber addition amount is 10% as exemplified in the above Examples 2-3, it is also feasible to use the determination method of the present invention to determine the rubber soluble content of the rubber modified asphalt prepared by the dry process with other rubber contents greater than 0 and less than or equal to 20%, which will not be listed in detail here.

[0218] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or system. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or system including the element.

[0219] The serial numbers of the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.

[0220] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for determining the soluble rubber content in a rubber-modified asphalt mixture prepared by a dry process, characterized in that: The method comprises the following steps: Step 1, obtaining asphalt samples, wherein the samples include base asphalt, rubber-modified asphalt obtained by a wet process, base asphalt extracted from ordinary asphalt mixture, and rubber-modified asphalt extracted by a dry process; Step 2, subjecting the asphalt samples in step 1 to a frequency sweep test and a multiple stress creep recovery test at a preset temperature to obtain the rutting factor and average stress recovery rate corresponding to each sample at different temperatures; Step 3, obtaining asphalt rutting factor coefficients of dry process and wet process at corresponding temperatures according to the rutting factor of rubber-modified asphalt and the rutting factor of rubber-free asphalt at the same preset temperature in step 2, and obtaining the rubber dissolution percentage in the rubber-modified asphalt under the frequency sweep test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature; Step 4, obtaining asphalt rutting factor coefficients of dry process and wet process at corresponding temperatures according to the average stress recovery rate of rubber-modified asphalt and the average stress recovery rate of rubber-free asphalt at the same preset temperature in step 2, and obtaining the rubber dissolution percentage in the rubber-modified asphalt under the multiple stress creep recovery test according to the asphalt rutting factor coefficients corresponding to the dry process and the wet process at each preset temperature; Step 5, performing weighted calculation on the rubber solubility percentages in the rubber modified asphalt in Step 3 and Step 4 to obtain a target rubber solubility content; Among them, step 2 is specifically as follows: The asphalt samples in step 1 are subjected to frequency sweep tests at preset temperatures to obtain the complex shear modulus G corresponding to each sample at different temperatures. * and phase angle δ, and according to the complex shear modulus G * The rutting factor corresponding to each sample at different temperatures is obtained by using the phase angle δ, where rutting factor = G * / sinδ Step 3 is as follows: Step 31, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the rutting factor of the rubber modified asphalt obtained by the wet process at the same preset temperature to the rutting factor of the base asphalt; Step 32, according to the same preset temperature, the rutting factor of the rubber modified asphalt extracted by the dry process is compared with the rutting factor of the base asphalt extracted by the ordinary asphalt mixture to obtain the asphalt rutting factor coefficient at the corresponding temperature of the dry process; Step 33, weighted calculation is performed on the ratio of the asphalt rutting factor coefficients of the dry process and the wet process at the same temperature to obtain the rubber dissolution percentage in the rubber modified asphalt under the frequency sweep test; And the specific steps of step 4 are: Step 41, obtaining the rutting factor coefficient of the rubber modified asphalt at the corresponding temperature of the wet process according to the ratio of the average stress recovery rate of the rubber modified asphalt obtained by the wet process at the same preset temperature to the average stress recovery rate of the base asphalt; Step 42, according to the average stress recovery rate of the rubber modified asphalt extracted by the dry process at the same preset temperature, and the average stress recovery rate of the base asphalt extracted by the ordinary asphalt mixture, the asphalt rutting factor coefficient at the corresponding temperature of the dry process is obtained; Step 43, weighted calculation is performed on the ratio of the average stress recovery rate of the dry process and the average stress recovery rate of the wet process at the same temperature to obtain the percentage of rubber dissolved in the rubber modified asphalt under the multiple stress creep recovery test.

2. The method for determining the soluble rubber content in the rubber-modified asphalt mixture prepared by dry process according to claim 1, characterized in that: In step 2, the preset temperature of the frequency sweep test and the multiple stress creep recovery test is 58-64°C.

3. The method for determining the soluble rubber content in the rubber-modified asphalt mixture prepared by dry process as claimed in claim 1, characterized in that: In step 1, the rubber content in the rubber-modified asphalt prepared by the wet process and the rubber-modified asphalt prepared by the dry process is 10%.

4. The method for determining the soluble rubber content in the rubber-modified asphalt mixture prepared by dry process as claimed in claim 1, characterized in that: In step 1, the mass proportion of old asphalt in the rubber modified asphalt extracted by dry process is 17-25%, and the mass proportion of old asphalt in the base asphalt extracted by ordinary asphalt mixture is 17-25%.

5. The method for determining the soluble rubber content in the rubber-modified asphalt mixture prepared by dry process as claimed in claim 1, characterized in that: In step 1, the base asphalt grade is PG58-34.

Citation Information

Patent Citations

  • Method and system for determining properties of an asphalt material

    CA2790246A1

  • Method for measuring SBS content in SBS modified asphalts by virtue of DSR

    CN104777288A

  • Method for evaluating high-temperature performance of SBS modified asphalt

    CN116482165A

  • Method for measuring SBS content in star-shaped SBS latex modified emulsified asphalt

    CN116990192A

  • Composite modified asphalt mixing amount optimization method based on response surface-entropy weight method

    CN117577246A