A butterfly-shaped optical cable that is resistant to bending and damage

By using rubber elastomers and low-friction polyolefin materials as outer and inner protective sheaths in the optical cable, combined with modified porous titanium dioxide and carbon fiber fillers, the mechanical strength and bending resistance of the optical cable are improved, solving the problem of optical cables in high-density wiring environments. Damage issues under bending and impact are eliminated, achieving more efficient fiber protection and resource utilization.

CN118502049BActive Publication Date: 2024-10-11ZHEJIANG DONGTONG OPTICAL NETWORK & IOT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962727.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-11
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

Existing optical cables are easily damaged by bending and impact, making it difficult to effectively protect internal optical fibers in high-density wiring environments, resulting in tight fiber channel resources and difficulty in use.

Method used

It adopts butterfly-shaped optical cable design. The outer protective sleeve is made of rubber elastomer. The inner protective sleeve is made of low-friction polyolefin material, combined with modified porous titanium dioxide and modified carbon fiber filler. The mechanical strength and bending resistance of the optical cable are improved through the synergistic compounding of materials. folding performance.

Benefits of technology

It achieves high wear resistance and damage resistance of the optical cable under multiple bends and impacts, effectively protects the internal optical fiber, extends the service life of the optical cable and the utilization efficiency of channel resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118502049B_ABST
    Figure CN118502049B_ABST
Patent Text Reader

Abstract

The present invention provides a butterfly optical cable that is resistant to bending and damage, comprising a butterfly-shaped outer protective sheath 1, an optical fiber 3 is arranged in the middle of the outer protective sheath, a reinforcing core material 4 is arranged on each side of the optical fiber 3, and an inner protective sheath 2 is arranged inside the outer protective sheath; wherein the inner protective sheath 2 is made of a low-friction polyolefin material, and the outer protective sheath 1 is made of a rubber elastomer. The present invention improves the mechanical strength and bending resistance of the optical cable by synergistically compounding the materials of the inner protective sheath and the outer protective sheath of the butterfly optical cable. The butterfly optical cable of the present invention has the performance of being resistant to multiple bendings and damage, and can effectively protect the internal optical fiber from damage in the case of multiple bendings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of communication optical cable manufacturing, and in particular relates to a butterfly-shaped optical cable that is resistant to bending and damage. Background Art

[0002] In recent years, with the development of communication technology and transmission network, the scale of optical fiber laying is gradually increasing, which makes the optical fiber channel resources in the same area increasingly tight. In order to set up as many optical fibers as possible in a limited resource space, multi-core optical cables are widely used in high-density indoor and outdoor applications. Branch optical cables and distribution optical cables are commonly used. Distribution optical cables are suitable for indoor, indoor / outdoor applications, trunks within and between buildings, distribution frames, wiring between telecommunication rooms, and connection cables in risers and pressurized environments, horizontal wiring of FTTD, EDA areas of data centers, and factory workshop automation. It is very necessary to develop butterfly optical cables that are resistant to bending and damage. Summary of the invention

[0003] The present invention provides a butterfly optical cable that is resistant to bending and damage, comprising a butterfly-shaped outer protective sheath 1, an optical fiber 3 is arranged in the middle of the outer protective sheath, a reinforcing core material 4 is arranged on the left and right sides of the optical fiber 3, and an inner protective sheath 2 is arranged inside the outer protective sheath; wherein the inner protective sheath 2 is made of a low-friction polyolefin material, and the outer protective sheath 1 is made of a rubber elastomer. The present invention improves the mechanical strength and bending resistance of the optical cable by synergistically compounding the materials of the inner protective sheath and the outer protective sheath of the butterfly optical cable. The butterfly optical cable of the present invention has the performance of being resistant to multiple bendings and damage, and can effectively protect the internal optical fiber from damage in the case of multiple bendings.

[0004] The specific plan is as follows:

[0005] A butterfly-shaped optical cable that is resistant to bending and damage, comprising a butterfly-shaped outer protective sheath 1, an optical fiber 3 is arranged in the middle of the outer protective sheath, a reinforcing core material 4 is arranged on each side of the optical fiber 3, and an inner protective sheath 2 is arranged inside the outer protective sheath; the characteristics are:

[0006] The outer protective sleeve 1 comprises the following components in parts by mass: 80-90 parts of EPDM rubber, 30-35 parts of polyamide, 20-25 parts of modified porous titanium dioxide material, 4-8 parts of plasticizer, 5-8 parts of maleic anhydride grafted EPDM rubber, 3-6 parts of stearic acid, and 2-5 parts of antioxidant.

[0007] The inner protective sleeve 2 comprises the following components in parts by mass: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 10-15 parts of modified fiber filler, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, and 1-2 parts of polymethylvinylsiloxane.

[0008] Furthermore, the plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.

[0009] Furthermore, the antioxidant is antioxidant 1010 or 2246.

[0010] Furthermore, the outer protective sleeve 1 comprises the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of plasticizer, 7 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant.

[0011] Furthermore, the inner protective sleeve 2 includes the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 13 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane.

[0012] Furthermore, the modified porous titanium dioxide filler is prepared by the following method:

[0013] 1) Tetraethyl titanate is dispersed in ethanol, and then acetic acid solution is added to react completely to obtain a precursor solution;

[0014] 2) Add polyvinyl pyrrolidone and ethylenediamine to the precursor solution, stir evenly, and dry to obtain a gel;

[0015] 3) Soaking the gel in ethanol, drying, calcining, crushing and grinding to obtain a porous titanium dioxide material;

[0016] 4) Dissolve hexadecyltrimethylammonium bromide and 1-butyl-3-methylimidazole chloride in deionized water, add porous titanium dioxide material, chitosan, glutaraldehyde, and acetic acid, perform hydrothermal reaction, filter, and dry to obtain a modified porous titanium dioxide filler.

[0017] Furthermore, the modified porous titanium dioxide filler is prepared by the following method:

[0018] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8-1.2 mol of deionized water, and react at room temperature for 6-8 hours to obtain a precursor solution;

[0019] 2) Add 10-15g polyvinyl pyrrolidone and 10-15g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0020] 3) Soak the gel in ethanol for 30-60 hours, dry it, and then calcine it at 500-600°C in an air atmosphere for 6-10 hours, crush it, and grind it to obtain a porous titanium dioxide material;

[0021] 4) Add 50g of porous titanium dioxide material, 5-10g of hexadecyltrimethylammonium bromide, 20-25g of 1-butyl-3-methylimidazole chloride, 2-4g of chitosan, and 1-2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 70-80 degrees Celsius for complete reaction, filter, and dry to obtain modified porous titanium dioxide filler.

[0022] Furthermore, the modified fiber filler is prepared by the following method:

[0023] A) adding 10g of carbon nanofibers with a length of 40-60 microns into 200ml of 2-3mol / L nitric acid aqueous solution, hydrothermally reacting at 70-80℃ for 6-10h, filtering, washing and drying to obtain activated carbon nanofibers;

[0024] B) Add 10g of activated carbon nanofibers to 200ml of ethanol solution of butyl titanate with a mass fraction of 2-4wt%, add 10g of acetic acid, hydrothermally react at 70-80℃ for 5-10h, filter, wash, dry, and heat to 650-700℃ and calcine for 3-5h;

[0025] C) Take 10g of the product of step B, add 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol into 100ml of N,N-dimethylformamide and mix evenly, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then hydrothermally react at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.

[0026] The present invention has the following beneficial effects:

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] 1) The outer protective sleeve is made of rubber elastomer and has excellent elasticity; the inner protective sleeve is made of low-friction polyolefin material and has excellent mechanical properties;

[0029] 2) The outer protective sheath is made of modified porous titanium dioxide. Titanium dioxide can not only absorb ultraviolet rays, but also can clean the surface of the optical cable as a photocatalyst. In addition, by modifying the surface of the porous titanium dioxide filler, the ionic liquid 1-butyl-3-methylimidazole chloride, the polymer chitosan, and the cross-linking agent glutaraldehyde can greatly improve the affinity between the porous filler and the polymer, improve the mechanical properties of the material, and achieve high wear resistance for the optical cable.

[0030] 3) In the present invention, the filler in the inner protective sheath is made of modified carbon fiber material, and the titanium dioxide particles on the surface of the carbon fiber form protrusions on the fiber surface, so that the carbon fiber can produce an anchoring effect in the sheath, slowing down the slippage of the carbon fiber in the sheath layer, and the modified carbon fiber filler increases the mechanical strength of the sheath layer; a cross-linked coating layer is formed on the surface of the carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the carbon surface is firmly coated and not easy to fall off, thereby solidifying the titanium dioxide on the surface of the carbon fiber. The coating of 1-butyl-3-methylimidazole bromide and polyethylene glycol can not only improve the dispersion performance of the filler, but also improve the bending resistance of the sheath. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a cross-sectional view of the optical cable of the present invention. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with specific implementation methods. In each embodiment and comparative example, the wall thickness of the inner protective sleeve is 0.3 mm, and the thickness of the outer protective sleeve is 0.1 mm; however, the protection scope of the present invention is not limited to the following embodiments, and any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.

[0033] Example 1

[0034] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0035] The outer protective sleeve 1 includes the following components in parts by mass: 80 parts of EPDM rubber, 30 parts of polyamide, 20 parts of modified porous titanium dioxide material, 4 parts of dioctyl phthalate, 5 parts of maleic anhydride grafted EPDM rubber, 3 parts of stearic acid, and 2 parts of antioxidant 1010.

[0036] The inner protective sleeve 2 comprises the following components in parts by mass: 60 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 10 parts of modified fiber filler, 2 parts of antioxidant, 2 parts of maleic anhydride grafted polyethylene, and 1 part of polymethylvinylsiloxane;

[0037] The modified porous titanium dioxide filler is prepared by the following method:

[0038] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8 mol of deionized water, and react at room temperature for 6 hours to obtain a precursor solution;

[0039] 2) Add 10g polyvinyl pyrrolidone and 10g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0040] 3) The gel was immersed in ethanol for 30 hours, dried, calcined at 500°C in an air atmosphere for 6 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0041] 4) Add 50 g of porous titanium dioxide material, 5 g of hexadecyltrimethylammonium bromide, 20 g of 1-butyl-3-methylimidazole chloride, 2 g of chitosan, and 1 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6 hours, filter, and dry to obtain a modified porous titanium dioxide material.

[0042] The modified fiber filler is prepared by the following method:

[0043] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2mol / L nitric acid aqueous solution, and after hydrothermal reaction at 70°C for 10h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of ethanol solution of butyl titanate with a mass fraction of 2wt%, 10g of acetic acid was added, hydrothermal reaction was carried out at 70°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 650°C for calcination for 3h; 10g of the product was taken, added with 5g of 1-butyl-3-methylimidazole bromide and 4g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1g of azobisisobutyronitrile and 1g of stannous isooctanoate were added, stirred evenly and allowed to stand for 10min, then hydrothermally reacted at 70°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain a modified fiber filler.

[0044] Example 2

[0045] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0046] The outer protective sleeve 1 includes the following components in parts by mass: 90 parts of EPDM rubber, 35 parts of polyamide, 25 parts of modified porous titanium dioxide material, 8 parts of dioctyl phthalate, 8 parts of maleic anhydride grafted EPDM rubber, 6 parts of stearic acid, and 5 parts of antioxidant 1010.

[0047] The inner protective sleeve 2 comprises the following components in parts by mass: 70 parts of polyethylene, 40 parts of polyamide, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of modified fiber filler, 5 parts of antioxidant, 4 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0048] The modified porous titanium dioxide filler is prepared by the following method:

[0049] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1.2 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0050] 2) Add 15g polyvinyl pyrrolidone and 15g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0051] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600°C in an air atmosphere for 10 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0052] 4) Add 50g of porous titanium dioxide material, 10g of hexadecyltrimethylammonium bromide, 25g of 1-butyl-3-methylimidazole chloride, 4g of chitosan and 2g of glutaraldehyde into 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6h, filter and dry to obtain modified porous titanium dioxide material.

[0053] The modified fiber filler is prepared by the following method:

[0054] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 3mol / L nitric acid aqueous solution, and after hydrothermal reaction at 80°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 4wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 80°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tube furnace and heated to 700°C for calcination for 3h; 10g of the product was taken, added with 10g of 1-butyl-3-methylimidazole bromide and 6g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 2g of azobisisobutyronitrile and 2g of stannous isooctanoate were added, stirred evenly and allowed to stand for 60min, then hydrothermally reacted at 90°C for 3h, filtered, washed with deionized water, and dried at 80°C to obtain a modified fiber filler.

[0055] Example 3

[0056] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0057] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0058] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0059] The modified porous titanium dioxide filler is prepared by the following method:

[0060] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0061] 2) Add 12g polyvinyl pyrrolidone and 12g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0062] 3) The gel was immersed in ethanol for 40 hours, dried, calcined at 5500°C in air atmosphere for 8 hours, crushed and ground to obtain a porous titanium dioxide material;

[0063] 4) Add 50 g of porous titanium dioxide material, 8 g of hexadecyltrimethylammonium bromide, 22 g of 1-butyl-3-methylimidazole chloride, 3 g of chitosan, and 2 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6 hours, filter, and dry to obtain a modified porous titanium dioxide material.

[0064] The modified fiber filler is prepared by the following method:

[0065] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of nitric acid aqueous solution with a concentration of 2.5mol / L, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of ethanol solution of butyl titanate with a mass fraction of 3wt%, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain a modified fiber filler.

[0066] Example 4

[0067] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0068] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0069] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0070] The modified porous titanium dioxide filler is prepared by the following method:

[0071] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 1.2 mol of deionized water, and react at room temperature for 6 hours to obtain a precursor solution;

[0072] 2) Add 10g polyvinyl pyrrolidone and 15g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0073] 3) The gel was immersed in ethanol for 30 hours, dried, calcined at 600°C in an air atmosphere for 6 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0074] 4) Add 50g of porous titanium dioxide material, 5g of hexadecyltrimethylammonium bromide, 25g of 1-butyl-3-methylimidazole chloride, 2g of chitosan, and 2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6h, filter, and dry to obtain a modified porous titanium dioxide material.

[0075] The modified fiber filler is the filler prepared in Example 3.

[0076] Example 5

[0077] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0078] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0079] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0080] The modified porous titanium dioxide filler is prepared by the following method:

[0081] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0082] 2) Add 15g polyvinyl pyrrolidone and 10g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0083] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600°C in an air atmosphere for 10 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0084] 4) Add 50 g of porous titanium dioxide material, 10 g of hexadecyltrimethylammonium bromide, 20 g of 1-butyl-3-methylimidazole chloride, 4 g of chitosan, and 1 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6 hours, filter, and dry to obtain a modified porous titanium dioxide material.

[0085] The modified fiber filler is the filler prepared in Example 3.

[0086] Comparative Example 1

[0087] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0088] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0089] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0090] The modified porous titanium dioxide filler is prepared by the following method:

[0091] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0092] 2) Add 15g polyvinyl pyrrolidone and 10g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0093] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600°C in an air atmosphere for 10 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0094] 4) Add 50 g of porous titanium dioxide material, 10 g of hexadecyltrimethylammonium bromide, 4 g of chitosan, and 1 g of glutaraldehyde into 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6 hours, filter, and dry to obtain a modified porous titanium dioxide material.

[0095] The modified fiber filler is the filler prepared in Example 3.

[0096] Comparative Example 2

[0097] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0098] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0099] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0100] The modified porous titanium dioxide filler is prepared by the following method:

[0101] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0102] 2) Add 15g polyvinyl pyrrolidone and 10g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0103] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600°C in an air atmosphere for 10 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0104] 4) Add 50 g of porous titanium dioxide material, 10 g of hexadecyltrimethylammonium bromide, 20 g of 1-butyl-3-methylimidazole chloride, and 1 g of glutaraldehyde to 200 ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6 hours, filter, and dry to obtain a modified porous titanium dioxide material.

[0105] The modified fiber filler is the filler prepared in Example 3.

[0106] Comparative Example 3

[0107] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0108] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0109] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0110] The modified porous titanium dioxide filler is prepared by the following method:

[0111] 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8 mol of deionized water, and react at room temperature for 8 hours to obtain a precursor solution;

[0112] 2) Add 15g polyvinyl pyrrolidone and 10g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel;

[0113] 3) The gel was immersed in ethanol for 60 hours, dried, calcined at 600°C in an air atmosphere for 10 hours, crushed, and ground to obtain a porous titanium dioxide material;

[0114] 4) Add 50g of porous titanium dioxide material, 10g of hexadecyltrimethylammonium bromide, 20g of 1-butyl-3-methylimidazole chloride, and 4g of chitosan into 200ml of 5% acetic acid solution, perform hydrothermal reaction at 80 degrees Celsius for 6h, filter, and dry to obtain a modified porous titanium dioxide material.

[0115] The modified fiber filler is the filler prepared in Example 3.

[0116] Comparative Example 4

[0117] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0118] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0119] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0120] The modified porous titanium dioxide filler is the filler prepared in Example 3.

[0121] The modified fiber filler is prepared by the following method:

[0122] 10 g of carbon nanofibers with a diameter of 40 microns were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, and subjected to hydrothermal reaction at 75°C for 8 hours. The mixture was filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers. 10 g of activated carbon nanofibers were added to 200 ml of an ethanol solution of 3 wt% butyl titanate, 10 g of acetic acid was added, and subjected to hydrothermal reaction at 75°C for 6 hours. The mixture was filtered, washed with deionized water, and dried at 80°C. The mixture was placed in a tubular furnace and heated to 670°C and calcined for 4 hours to obtain a modified fiber filler.

[0123] Comparative Example 5

[0124] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0125] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0126] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0127] The modified porous titanium dioxide filler is the filler prepared in Example 3.

[0128] The modified fiber filler is prepared by the following method:

[0129] 10 g of carbon nanofibers with a diameter of 40 μm were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, subjected to hydrothermal reaction at 75° C. for 8 h, filtered, washed with deionized water, and dried at 80° C. to obtain activated carbon nanofibers; 10 g of activated carbon nanofibers, 8 g of 1-butyl-3-methylimidazole bromide, and 5 g of polyethylene glycol were added to 100 ml of N,N-dimethylformamide and mixed evenly, 1.5 g of azobisisobutyronitrile and 1.5 g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30 min, followed by hydrothermal reaction at 80° C. for 4 h, filtered, washed with deionized water, and dried at 80° C. to obtain a modified fiber filler.

[0130] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified fiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber and the reinforcing member through a screw extruder, wherein the optical fiber is at the center of the butterfly sheath, and the reinforcing member is at the two wings of the butterfly sheath, to obtain the bending and damage-resistant butterfly optical cable.

[0131] Comparative Example 6

[0132] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0133] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0134] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0135] The modified porous titanium dioxide filler is the filler prepared in Example 3.

[0136] The modified fiber filler is prepared by the following method:

[0137] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added to 8g of 1-butyl-3-methylimidazole bromide in 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain a modified fiber filler.

[0138] Comparative Example 7

[0139] The butterfly optical cable comprises a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath 2 is arranged inside the outer protective sheath;

[0140] The outer protective sleeve 1 includes the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of dioctyl phthalate, 6 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant 1010.

[0141] The inner protective sleeve 2 comprises the following components in parts by mass: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 12 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane;

[0142] The modified porous titanium dioxide filler is the filler prepared in Example 3.

[0143] The modified fiber filler is prepared by the following method:

[0144] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% ethanol solution of butyl titanate, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace and calcined for 4h; 10g of the product was taken, added with 5g of polyethylene glycol to 100ml of N,N-dimethylformamide, mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain a modified fiber filler.

[0145] Experiments and Data

[0146] The tensile strength and environmental stress cracking time of the sheath material are tested in accordance with the national standard GB / T2951.

[0147] The wear resistance performance refers to the standard GB / T17737.324-2018 "Mechanical test methods for coaxial communication cables - Cable wear resistance test" to measure the loss mass of the specimen after 500 cycles.

[0148] YD / T1997.1-2022 "Introduction Cable for Communication Part 1: Butterfly Cable" performs performance testing on optical cables. Repeated bending: residual additional attenuation.

[0149] The results are shown in Table 1.

[0150] Table 1

[0151]

[0152] Tests and Results

[0153] As can be seen from Table 1, the effects of various parameters in the process and the effects on product performance can be seen from the embodiments and comparative examples. The outer protective sleeve is made of rubber elastomer and has excellent elasticity; the inner protective sleeve is made of low-friction polyolefin material and has excellent mechanical properties; the material of the outer protective sleeve adopts modified porous titanium dioxide filler, and the surface modification of the porous titanium dioxide filler can greatly improve the affinity between the porous filler and the polymer, and can improve the mechanical properties of the material, and the optical cable can achieve high wear resistance; titanium dioxide can not only absorb ultraviolet rays, but also can achieve the purpose of cleaning the surface of the optical cable as a photocatalyst, and in the present invention, the filler in the inner protective sleeve adopts modified carbon fiber material, and a cross-linked coating layer is formed on the surface of the carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the carbon surface is firmly coated and not easy to fall off, so that titanium dioxide is solidified on the surface of the carbon fiber to form protrusions, so that the carbon fiber can produce an anchoring effect in the sheath, slowing down the slippage of the carbon fiber in the sheath layer, and the modified carbon fiber filler increases the mechanical strength of the sheath layer.

[0154] Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A butterfly-shaped optical cable that is resistant to bending and damage, comprising a butterfly-shaped outer protective sheath, an optical fiber is arranged in the middle of the outer protective sheath, a reinforcing core material is arranged on each side of the optical fiber, and an inner protective sheath is arranged inside the outer protective sheath; characterized in that: The outer protective sleeve comprises the following components in parts by mass: 80-90 parts of EPDM rubber, 30-35 parts of polyamide, 20-25 parts of modified porous titanium dioxide material, 4-8 parts of plasticizer, 5-8 parts of maleic anhydride grafted EPDM rubber, 3-6 parts of stearic acid, and 2-5 parts of antioxidant; the modified porous titanium dioxide material is prepared by the following method: 1) Disperse 1 mol of tetraethyl titanate in 500 mL of ethanol, add 1 mol of acetic acid and 0.8-1.2 mol of deionized water, and react at room temperature for 6-8 hours to obtain a precursor solution; 2) Add 10-15g polyvinyl pyrrolidone and 10-15g ethylenediamine to 100ml precursor solution, stir evenly, and dry to obtain a gel; 3) Soak the gel in ethanol for 30-60 hours, dry it, and then calcine it at 500-600°C in an air atmosphere for 6-10 hours, crush it, and grind it to obtain a porous titanium dioxide material; 4) Add 50g of porous titanium dioxide material, 5-10g of hexadecyltrimethylammonium bromide, 20-25g of 1-butyl-3-methylimidazole chloride, 2-4g of chitosan, and 1-2g of glutaraldehyde to 200ml of 5% acetic acid solution, perform hydrothermal reaction at 70-80 degrees Celsius, filter, and dry to obtain a modified porous titanium dioxide material; The inner protective sleeve comprises the following components in parts by mass: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 10-15 parts of modified fiber filler, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, and 1-2 parts of polymethylvinylsiloxane. The modified fiber filler in the inner protective sleeve adopts modified carbon fiber material, and titanium dioxide particles on the surface of the carbon fiber form protrusions on the fiber surface, so that the carbon fiber can produce an anchoring effect in the sheath; a cross-linked coating layer is formed on the surface of the carbon fiber by polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the carbon surface is firmly coated to solidify the titanium dioxide on the surface of the carbon fiber.

2. A butterfly-shaped optical cable resistant to bending and damage as claimed in claim 1, characterized in that: The plasticizer is selected from one or a combination of dioctyl phthalate, butyl benzyl phthalate, dicyclohexyl phthalate, dibutyl phthalate, diisobutyl phthalate, dimethyl phthalate, and diethyl phthalate.

3. A butterfly-shaped optical cable resistant to bending and damage as claimed in claim 1, characterized in that: The antioxidant is selected from one or more of antioxidant 1010, antioxidant 1790, antioxidant 245, antioxidant 168, antioxidant CA, antioxidant 264, and antioxidant 1076.

4. A butterfly-shaped optical cable resistant to bending and damage as claimed in claim 1, characterized in that: The outer protective sleeve comprises the following components in parts by mass: 85 parts of EPDM rubber, 32 parts of polyamide, 22 parts of modified porous titanium dioxide material, 6 parts of plasticizer, 7 parts of maleic anhydride grafted EPDM rubber, 5 parts of stearic acid, and 3 parts of antioxidant.

5. A butterfly-shaped optical cable resistant to bending and damage as claimed in claim 1, characterized in that: The inner protective sleeve comprises the following components in parts by weight: 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 13 parts of modified fiber filler, 3 parts of antioxidant, 3 parts of maleic anhydride grafted polyethylene, and 2 parts of polymethylvinylsiloxane.