Anti-ant flame-retardant cable and preparation method thereof
By monitoring particle characteristic information and adjusting cable preparation parameters, the problem of unstable anti-ant effect of anti-ant and flame-retardant cables in mass production is solved, and the preparation efficiency and cable quality are improved.
Patent Information
- Application Number
- CN202410909917.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing technology fails to adapt to changes in preparation materials and machines during mass production of cables, resulting in unstable anti-ant effects of anti-ant and flame-retardant cables and affecting preparation efficiency.
By monitoring the mixing process, obtaining particle characteristic information, adjusting the stirring power, heating temperature and stirring duration, the preparation process of the second protective layer is precisely controlled, ensuring that the preparation parameters meet the preset standards, and improving the anti-ant and flame-retardant performance and preparation efficiency of the cable.
It effectively improves the preparation efficiency and anti-ant stability of anti-ant and flame-retardant cables, ensures the quality of the cable, and optimizes the control accuracy of the production process.
Smart Images

Figure CN118507128B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cable preparation, and in particular to an anti-ant flame-retardant cable and a preparation method thereof. Background Art
[0002] Cable is a device for transmitting electric energy or signals, usually composed of several or several groups of wires. With the rapid development of economy, cables are widely used in the fields of communication and electricity. In South China, cables are easily damaged by termites and rodents, which may lead to cable failure. At the same time, most existing cables are made of rubber, which is a flammable material. The sparks formed by the short circuit of the damaged cable can easily ignite the outer material of the cable, causing a fire.
[0003] Chinese patent publication number: CN115050511A, discloses an anti-ant flame-retardant cable and its preparation method, including a cable, wherein the cable is arranged as a sheath layer, a water-blocking layer, an insulating layer and a conductor from the outer layer to the inner layer; the conductor is a composite twisted form of multiple tinned soft round copper wires; the insulating layer is a 35kV ethylene-propylene rubber material; the material of the water-blocking layer is a water-blocking tape wrapped layer; the sheath layer is made of the following raw materials in parts by weight: 1-2 parts of 10% cypermethrin emulsifiable concentrate, 2-4 parts of cloves, 3-5 parts of camphor, and 15-25 parts of low-density polyethylene , 20-30 parts of modified polyurethane elastomer, 10-15 parts of zinc stearate, 5-8 parts of light calcium carbonate, 5-6 parts of kaolin, and 6-8 parts of antioxidant; the kaolin is 5000 mesh calcined kaolin; it can be seen that the above technical scheme has the following problems: in the prior art, in the batch production process, unified production parameters are adopted, and adaptive adjustment of preparation parameters according to changes in preparation raw materials and preparation machines is not considered, which affects the stability of the anti-ant effect of the prepared anti-ant flame retardant cable, and further affects the preparation efficiency of the anti-ant flame retardant cable. Summary of the invention
[0004] To this end, the present invention provides an anti-ant flame retardant cable and a preparation method thereof, so as to overcome the problem in the prior art that, in the mass production process, unified production parameters are adopted without considering adaptive adjustment of the preparation parameters according to changes in the preparation raw materials and preparation machines, which affects the stability of the anti-ant effect of the prepared anti-ant flame retardant cable and further affects the preparation efficiency of the anti-ant flame retardant cable.
[0005] In one aspect, the present invention provides an anti-ant flame-retardant cable, comprising:
[0006] Several cable cores,
[0007] Each cable core is coated in a first protective layer, and a filling composition is filled between each cable core in the first protective layer, and a second protective layer is coated outside the first protective layer;
[0008] The filling composition comprises, by weight, 100 parts of EPDM rubber, 2.3-3.2 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide vulcanizer; 0.3-1.2 parts of co-vulcanizer, 50-67 parts of calcined clay filling reinforcing agent activated by silane coupling agent; 5-7 parts of microcrystalline wax, 0.8-1.2 parts of coupling agent, 8-10 parts of low-density polyethylene, 5-8 parts of zinc oxide nanopowder, 1.2-1.6 parts of antioxidant, 5-6 parts of red lead, 1.0-5 parts of magnesium oxide nanopowder, 15-25 parts of white carbon black, 0.2-5 parts of ion scavenger, 2-5 parts of nano-montmorillonite, and 10-15 parts of flame retardant Al(OH)3;
[0009] The first protective layer comprises, by weight, 30-50 parts of acetylene black, 50-70 parts of graphite powder, 1-2 parts of antioxidant, 3-4 parts of organic peroxide, 4-5 parts of accelerator, 1-2 parts of coupling agent, 10-20 parts of magnesium oxide, 1-1.5 parts of stabilizer, 4-8 parts of methyl silicone oil, 4-5 parts of alkaline neutralizer, and 30-40 parts of processing oil in 100 parts of chlorinated polyethylene;
[0010] The second protective layer includes 40% to 50% by mass of ethylene-vinyl acetate copolymer and ethylene propylene diene monomer rubber, 40% to 55% by mass of aluminum hydroxide and magnesium hydroxide, 0.2% to 0.4% by mass of antioxidant 1010, 2% to 4% by mass of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, and 1.5% to 2% by mass of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant.
[0011] On the other hand, the present invention also provides a method for preparing the above-mentioned anti-ant flame-retardant cable, comprising:
[0012] Step S1, adding each component of the filling composition into an internal mixer in a predetermined ratio for mixing, so as to complete the preparation of the filling composition;
[0013] Step S2, adding the components of the first protective layer into an internal mixer for mixing, so as to complete the preparation of the first protective layer;
[0014] Step S3, preparing a second protective layer,
[0015] Step S31, adding the components of the second protective layer into a reactor according to a preset mass ratio, and heating and stirring the reactor;
[0016] Step S32, when the running time of the reactor reaches an integer multiple of the preset stirring time, obtaining archived image information of each component in the reactor, and determining whether the preparation parameters for the protective layer meet the preset standards based on the particle features in the acquired archived image information;
[0017] Step S33, adjusting the stirring power, heating temperature, or preset stirring time of the reaction kettle for each component according to the area difference between the particle area ratio and the first preset particle area ratio;
[0018] Step S34, the reactor uses the adjusted parameters to process the mixed material;
[0019] Step S35, extruding the mixed material determined to meet the preset standard through an extruder;
[0020] Step S36, vulcanizing the cable sheath obtained after extrusion, and sequentially cooling and winding the vulcanized cable sheath;
[0021] Step S4, wrapping a plurality of cable cores in the first protective layer, filling the filling composition between the cable cores in the first protective layer, and wrapping the second protective layer outside the first protective layer to complete the preparation of the anti-ant flame-retardant cable.
[0022] Further, each particle feature in the archived image information is obtained, and the total area of each particle feature and the particle area ratio of the total area of the archived image information are calculated, and whether the preparation parameters of the protective layer meet the preset standards is determined according to the obtained particle area ratio, including:
[0023] If the particle area ratio is greater than the second preset particle area ratio, determining a treatment method for the reactor according to the area difference between the particle area ratio and the first preset particle area ratio;
[0024] If the particle area ratio is less than or equal to the second preset particle area ratio and greater than the first preset particle area ratio, re-determining whether the preparation parameters of the protective layer meet the preset standards according to the slope of the drawn time-particle area ratio curve at the current time node;
[0025] If the particle area ratio is less than or equal to the first preset particle area ratio, it is determined that the mixed material meets the preset standard.
[0026] Furthermore, a treatment method for the reactor is determined based on the area difference, including:
[0027] If the area difference is less than or equal to the first preset area difference, determining the stirring power of the reactor for each component according to the obtained mixing deviation of each component in the reactor;
[0028] If the area difference is less than or equal to the second preset area difference and greater than the first preset area difference, the heating temperature of the reactor is adjusted to a corresponding value according to the rotation speed deviation; the first preset area difference is less than the second preset area difference;
[0029] If the area difference is greater than the second preset area difference, the preset stirring time is adjusted to a corresponding value according to the difference between the area difference and the second preset area difference, and after the adjustment of the preset stirring time is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
[0030] Further, the archived image information of each component in the reactor is re-obtained at a preset interval, and the particle area ratio of the archived image information is obtained, and the absolute value of the difference between the two particle area ratios is calculated, and the absolute value is recorded as the mixing deviation;
[0031] The adjustment method of the stirring power of the reactor for each component is determined according to the mixing deviation, wherein:
[0032] If the mixing deviation is less than or equal to the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the first preset stirring adjustment coefficient;
[0033] If the mixing deviation is less than or equal to the second preset mixing deviation and greater than the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the second preset stirring adjustment coefficient; the first preset mixing deviation is less than the second preset mixing deviation;
[0034] If the mixing deviation is greater than the second preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the third preset stirring adjustment coefficient;
[0035] After the adjustment of the stirring power is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
[0036] Further, determining whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information includes:
[0037] When the reacquired particle area ratio is greater than the first preset particle area ratio, the heating temperature is adjusted to the corresponding value according to the speed deviation; when the reacquired particle area ratio is less than or equal to the first preset particle area ratio, the reactor is controlled to continue operating using the current operating parameters.
[0038] Further, a regulation mode for the heating temperature is determined based on the rotation speed deviation, wherein:
[0039] If the speed deviation is less than or equal to the first preset speed deviation, the heating temperature is adjusted to a corresponding value using the first preset temperature adjustment coefficient;
[0040] If the speed deviation is less than or equal to the second preset speed deviation and greater than the first preset speed deviation, the heating temperature is adjusted to the corresponding value using the second preset temperature adjustment coefficient; the first preset speed deviation is less than the second preset speed deviation;
[0041] If the speed deviation is greater than the second preset speed deviation, the heating temperature is adjusted to a corresponding value using a third preset temperature adjustment coefficient;
[0042] The process of obtaining the speed deviation is to obtain the stirring speed of the current reactor, obtain the preset speed corresponding to the current stirring power, calculate the difference between the preset speed and the stirring speed, and obtain the speed deviation.
[0043] Further, the difference between the area difference and the second preset area difference is calculated and recorded as the particle difference, and the adjustment method for the preset stirring time is determined based on the particle difference, wherein:
[0044] If the particle difference is less than or equal to the first preset particle difference, the preset stirring time is adjusted to a corresponding value using the first preset time adjustment coefficient;
[0045] If the particle difference is less than or equal to the second preset particle difference and greater than the first preset particle difference, the preset stirring time is adjusted to the corresponding value using the second preset time adjustment coefficient; the first preset particle difference is less than the second preset particle difference;
[0046] If the particle difference is greater than the second preset particle difference, the preset stirring time is adjusted to a corresponding value using the third preset time adjustment coefficient.
[0047] Furthermore, the archived image information of each component in the reactor is continuously obtained at preset intervals, a time-particle area ratio curve is drawn based on each archived image information, and whether the preparation parameters of the protective layer meet the preset standards is determined according to the slope of the time-particle area ratio curve at the current time node, including:
[0048] If the slope is greater than the preset slope, a treatment method for the reactor is determined according to the area difference between the current particle area ratio and the first preset particle area ratio;
[0049] If the slope is less than or equal to a preset slope, it is determined that the mixed material meets the preset standard.
[0050] Compared with the prior art, the beneficial effect of the present invention lies in that, in the process of mass production of anti-ant flame-retardant cables, the preparation process of the second protective layer used for anti-ant flame-retardant is precisely controlled, the mixing situation is monitored during the mixing process of each component, the archived image information is obtained, and the corresponding method of processing raw materials is determined according to the specific situation of the particle characteristics in the archived image information, which effectively improves the preparation efficiency of the second protective layer and further improves the preparation efficiency of the anti-ant flame-retardant cables.
[0051] Furthermore, a specific treatment method for the reactor is determined based on the area difference. When the area difference between the particle area ratio and the first preset particle area ratio is less than or equal to the first preset area difference, there are only small-scale incompletely fused components. In this case, due to stirring problems, the components cannot be fully processed. At this time, the stirring power is processed; when the area difference is less than or equal to the second preset area difference and greater than the first preset area difference, there are large areas of incompletely fused components. In this case, due to temperature problems, the components cannot be fully melted. At this time, the heating temperature of the reactor is increased; when the area difference is greater than the second preset area difference, considering that the detection time is too early and the components cannot be fully processed, the acquisition of the conditions of the components in the reactor is delayed to further determine whether to process the reactor. While effectively and accurately controlling the preparation process of the cable protective layer, the preparation efficiency of the anti-ant flame-retardant cable is further improved.
[0052] Furthermore, the processing conditions of the components in the reactor are obtained, and the adjustment range of the stirring power is determined specifically, and the adjustment range of the stirring power is determined according to the change range of the particle area ratio between the archived image information obtained twice, and the change range of the particle area ratio is inversely proportional to the adjustment range of the stirring power. The operating parameters of the reactor are determined in detail, and the preparation parameters for the cable protective layer are determined, which effectively ensures the quality of the generated cable and further improves the preparation efficiency of the anti-ant flame-retardant cable.
[0053] Furthermore, based on the speed deviation, it is determined whether the material cannot be mixed evenly due to the viscosity not meeting the standard. The stirring power corresponds to a preset speed, and the stirring paddle should reach the corresponding speed under the corresponding stirring power. However, if the actually measured stirring speed does not meet the standard, the heating temperature is adjusted at this time. While effectively improving the anti-ant stability of the prepared anti-ant flame-retardant cable, the preparation efficiency of the anti-ant flame-retardant cable is further improved.
[0054] Furthermore, the change of the particle area ratio in the reactor is obtained. When the slope is greater than the preset slope, the change of the particle area ratio is small, and the melting speed of each material is slow. In this case, the reactor is specifically treated. If the slope is less than or equal to the preset slope, the change of the particle area ratio is large, and the melting speed of each material is fast. The processing of each material can be completed according to the current operating parameters, which effectively ensures the quality of the generated cable and further improves the preparation efficiency of the anti-ant flame-retardant cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is a flowchart of the steps of the method for preparing an ant-proof flame-retardant cable according to an embodiment of the present invention;
[0056] Figure 2 This is a flow chart of determining whether the preparation parameters of the protective layer meet the preset standards according to the particle area ratio in an embodiment of the present invention. DETAILED DESCRIPTION
[0057] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0058] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0059] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0060] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0061] See also Figure 1 as well as Figure 2As shown, they are respectively a flowchart of the steps of the method for preparing an ant-proof flame-retardant cable according to an embodiment of the present invention, and a flowchart of determining whether the preparation parameters of the protective layer meet the preset standards according to the particle area ratio; an ant-proof flame-retardant cable and a preparation method thereof according to an embodiment of the present invention, comprising:
[0062] Several cable cores,
[0063] Each cable core is coated in a first protective layer, and a filling composition is filled between each cable core in the first protective layer, and a second protective layer is coated outside the first protective layer;
[0064] The filling composition comprises, by weight, 100 parts of EPDM rubber, 2.3-3.2 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide vulcanizer; 0.3-1.2 parts of co-vulcanizer, 50-67 parts of calcined clay filling reinforcing agent activated by silane coupling agent; 5-7 parts of microcrystalline wax, 0.8-1.2 parts of coupling agent, 8-10 parts of low-density polyethylene, 5-8 parts of zinc oxide nanopowder, 1.2-1.6 parts of antioxidant, 5-6 parts of red lead, 1.0-5 parts of magnesium oxide nanopowder, 15-25 parts of white carbon black, 0.2-5 parts of ion scavenger, 2-5 parts of nano-montmorillonite, and 10-15 parts of flame retardant Al(OH)3;
[0065] The first protective layer comprises, by weight, 30-50 parts of acetylene black, 50-70 parts of graphite powder, 1-2 parts of antioxidant, 3-4 parts of organic peroxide, 4-5 parts of accelerator, 1-2 parts of coupling agent, 10-20 parts of magnesium oxide, 1-1.5 parts of stabilizer, 4-8 parts of methyl silicone oil, 4-5 parts of alkaline neutralizer, and 30-40 parts of processing oil in 100 parts of chlorinated polyethylene;
[0066] The second protective layer includes 40% to 50% by mass of ethylene-vinyl acetate copolymer and ethylene propylene diene monomer rubber, 40% to 55% by mass of aluminum hydroxide and magnesium hydroxide, 0.2% to 0.4% by mass of antioxidant 1010, 2% to 4% by mass of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, and 1.5% to 2% by mass of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant.
[0067] Specifically, the preparation method of the second protective layer includes:
[0068] Step S1, adding each component of the filling composition into an internal mixer in a predetermined ratio for mixing, so as to complete the preparation of the filling composition;
[0069] Step S2, adding the components of the first protective layer into an internal mixer for mixing, so as to complete the preparation of the first protective layer;
[0070] Step S3, preparing a second protective layer,
[0071] Step S31, adding the components of the second protective layer into a reactor according to a preset mass ratio, and heating and stirring the reactor;
[0072] Step S32, when the running time of the reactor reaches an integer multiple of the preset stirring time, obtaining archived image information of each component in the reactor, and determining whether the preparation parameters for the protective layer meet the preset standards based on the particle features in the acquired archived image information;
[0073] Step S33, adjusting the stirring power, heating temperature, or preset stirring time of the reaction kettle for each component according to the area difference between the particle area ratio and the first preset particle area ratio;
[0074] Step S34, the reactor uses the adjusted parameters to process the mixed material;
[0075] Step S35, extruding the mixed material determined to meet the preset standard through an extruder;
[0076] Step S36, vulcanizing the cable sheath obtained after extrusion, and sequentially cooling and winding the vulcanized cable sheath;
[0077] Step S4, wrapping a plurality of cable cores in the first protective layer, filling the filling composition between the cable cores in the first protective layer, and wrapping the second protective layer outside the first protective layer to complete the preparation of the anti-ant flame-retardant cable.
[0078] It should be pointed out that the data in this embodiment are obtained by comprehensive analysis and evaluation of the historical test data and the corresponding historical test results three months before this test. It can be understood by those skilled in the art that the method of the present invention can determine the single parameter by selecting the highest value as the preset standard parameter according to the data distribution, using weighted summation to use the obtained value as the preset standard parameter or other selection methods, as long as the system of the present invention can clearly define the different specific situations in the single determination process through the obtained value.
[0079] Specifically, each particle feature in the archived image information is obtained, and the total area of each particle feature and the particle area ratio of the total area of the archived image information are calculated, and whether the preparation parameters of the protective layer meet the preset standards is determined according to the obtained particle area ratio, including:
[0080] If the particle area ratio is greater than the second preset particle area ratio, determining a treatment method for the reactor according to the area difference between the particle area ratio and the first preset particle area ratio;
[0081] If the particle area ratio is less than or equal to the second preset particle area ratio and greater than the first preset particle area ratio, re-determining whether the preparation parameters of the protective layer meet the preset standards according to the slope of the drawn time-particle area ratio curve at the current time node;
[0082] If the particle area ratio is less than or equal to the first preset particle area ratio, it is determined that the mixed material meets the preset standard.
[0083] During the mass production of anti-ant flame-retardant cables, the preparation process of the second protective layer used for anti-ant flame retardancy is precisely controlled, the mixing situation is monitored during the mixing process of each component, the archived image information is obtained, and the corresponding method of processing raw materials is determined according to the specific situation of the particle characteristics in the archived image information. While effectively improving the preparation efficiency of the second protective layer, the preparation efficiency of the anti-ant flame retardant cable is further improved.
[0084] Among them, the first preset particle area ratio is 0.085, and the second preset particle area ratio is 0.172.
[0085] Specifically, the treatment method for the reactor is determined based on the area difference, including:
[0086] If the area difference is less than or equal to the first preset area difference, determining the stirring power of the reactor for each component according to the obtained mixing deviation of each component in the reactor;
[0087] If the area difference is less than or equal to the second preset area difference and greater than the first preset area difference, the heating temperature of the reactor is adjusted to a corresponding value according to the rotation speed deviation; the first preset area difference is less than the second preset area difference;
[0088] If the area difference is greater than the second preset area difference, the preset stirring time is adjusted to a corresponding value according to the difference between the area difference and the second preset area difference, and after the adjustment of the preset stirring time is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
[0089] Among them, the first preset area difference is 0.061, and the second preset area difference is 0.192.
[0090] The specific treatment method for the reactor is determined according to the area difference. When the area difference between the particle area ratio and the first preset particle area ratio is less than or equal to the first preset area difference, there are only small-scale incompletely fused components. In this case, the components cannot be fully processed due to stirring problems. At this time, the stirring power is processed; when the area difference is less than or equal to the second preset area difference and greater than the first preset area difference, there are large areas of incompletely fused components. In this case, the components cannot be fully melted due to temperature problems. At this time, the heating temperature of the reactor is increased; when the area difference is greater than the second preset area difference, considering that the components cannot be fully processed due to early detection time, the acquisition of the conditions of the components in the reactor is delayed in order to further determine whether to process the reactor. While effectively and accurately controlling the preparation process of the cable protective layer, the preparation efficiency of the anti-ant flame-retardant cable is further improved.
[0091] Specifically, the archived image information of each component in the reactor is re-obtained at a preset interval, and the particle area ratio of the archived image information is obtained, and the absolute value of the difference between the two particle area ratios is calculated, and the absolute value is recorded as the mixing deviation;
[0092] The adjustment method of the stirring power of the reactor for each component is determined according to the mixing deviation, wherein:
[0093] If the mixing deviation is less than or equal to the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the first preset stirring adjustment coefficient;
[0094] If the mixing deviation is less than or equal to the second preset mixing deviation and greater than the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the second preset stirring adjustment coefficient; the first preset mixing deviation is less than the second preset mixing deviation;
[0095] If the mixing deviation is greater than the second preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the third preset stirring adjustment coefficient;
[0096] After the adjustment of the stirring power is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
[0097] Among them, the first preset mixing deviation is 0.077, the second preset mixing deviation is 0.126, the first preset stirring adjustment coefficient is 1.28, the second preset stirring adjustment coefficient is 1.19, and the third preset stirring adjustment coefficient is 1.11.
[0098] The processing conditions of the components in the reactor are obtained, and the adjustment range of the stirring power is determined specifically. The adjustment range of the stirring power is determined according to the change range of the particle area ratio between the archived image information obtained twice. The change range of the particle area ratio is inversely proportional to the adjustment range of the stirring power. The operating parameters of the reactor are determined in detail, and the preparation parameters for the cable protective layer are determined. While effectively ensuring the quality of the generated cable, the preparation efficiency of the anti-ant flame-retardant cable is further improved.
[0099] Specifically, whether the preparation parameters of the protective layer meet the preset standards is determined based on the re-acquired archived image information, including:
[0100] When the reacquired particle area ratio is greater than the first preset particle area ratio, the heating temperature is adjusted to the corresponding value according to the speed deviation; when the reacquired particle area ratio is less than or equal to the first preset particle area ratio, the reactor is controlled to continue operating using the current operating parameters.
[0101] Specifically, the adjustment method for the heating temperature is determined based on the rotation speed deviation, wherein:
[0102] If the speed deviation is less than or equal to the first preset speed deviation, the heating temperature is adjusted to a corresponding value using the first preset temperature adjustment coefficient;
[0103] If the speed deviation is less than or equal to the second preset speed deviation and greater than the first preset speed deviation, the heating temperature is adjusted to the corresponding value using the second preset temperature adjustment coefficient; the first preset speed deviation is less than the second preset speed deviation;
[0104] If the speed deviation is greater than the second preset speed deviation, the heating temperature is adjusted to a corresponding value using a third preset temperature adjustment coefficient;
[0105] The process of obtaining the speed deviation is to obtain the stirring speed of the current reactor, obtain the preset speed corresponding to the current stirring power, calculate the difference between the preset speed and the stirring speed, and obtain the speed deviation.
[0106] Specifically, the stirring speed of the current reactor can be optionally obtained by continuously monitoring the stirring process inside the reactor through a visual detector. This is a prior art and will not be described in detail.
[0107] Among them, the first preset speed deviation is 2 rpm, the second preset speed deviation is 6 rpm, the first preset temperature adjustment coefficient is 1.101, the second preset temperature adjustment coefficient is 1.151, and the third preset temperature adjustment coefficient is 1.231.
[0108] Based on the speed deviation, it is determined whether the material cannot be mixed evenly due to the viscosity not meeting the standard. The stirring power corresponds to a preset speed. The stirring paddle should reach the corresponding speed under the corresponding stirring power. However, if the actually measured stirring speed does not meet the standard, the heating temperature is adjusted at this time. While effectively improving the anti-ant stability of the prepared anti-ant flame-retardant cable, the preparation efficiency of the anti-ant flame-retardant cable is further improved.
[0109] Specifically, the difference between the area difference and the second preset area difference is calculated and recorded as the particle difference, and the adjustment method for the preset stirring time is determined based on the particle difference, wherein:
[0110] If the particle difference is less than or equal to the first preset particle difference, the preset stirring time is adjusted to a corresponding value using the first preset time adjustment coefficient;
[0111] If the particle difference is less than or equal to the second preset particle difference and greater than the first preset particle difference, the preset stirring time is adjusted to the corresponding value using the second preset time adjustment coefficient; the first preset particle difference is less than the second preset particle difference;
[0112] If the particle difference is greater than the second preset particle difference, the preset stirring time is adjusted to a corresponding value using the third preset time adjustment coefficient.
[0113] Among them, the first preset particle difference is 0.16, the second preset particle difference is 0.28, the first preset duration adjustment coefficient is 1.12, the second preset duration adjustment coefficient is 1.25, and the third preset duration adjustment coefficient is 1.31.
[0114] Specifically, the archived image information of each component in the reactor is continuously obtained at preset intervals, a time-particle area ratio curve is drawn based on each archived image information, and the preparation parameters of the protective layer are determined according to the slope of the time-particle area ratio curve at the current time node to determine whether they meet the preset standards, including:
[0115] If the slope is greater than the preset slope, a treatment method for the reactor is determined according to the area difference between the current particle area ratio and the first preset particle area ratio;
[0116] If the slope is less than or equal to a preset slope, it is determined that the mixed material meets the preset standard.
[0117] Among them, the preset slope is -0.0027.
[0118] The change of the particle area ratio in the reactor is obtained. When the slope is greater than the preset slope, the change of the particle area ratio is small, and the melting speed of each material is slow. In this case, specific treatment is performed on the reactor. If the slope is less than or equal to the preset slope, the change of the particle area ratio is large, and the melting speed of each material is fast. The processing of each material can be completed according to the current operating parameters, which effectively ensures the quality of the generated cable and further improves the preparation efficiency of the anti-ant flame-retardant cable. Example 1
[0119] The second protective layer was prepared by preparing the raw materials, weighing 47.15 parts of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 49.15 parts of aluminum hydroxide and magnesium hydroxide, 0.2 parts of antioxidant 1010, 2 parts of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, silane coupling agent 172, peroxide vulcanizer DCP and polyethylene wax lubricant. 1.5 parts.
[0120] Mix 47.15 parts of base polymer, ethylene-vinyl acetate copolymer and ethylene propylene diene monomer rubber with 49.15 parts of other solid additives, aluminum hydroxide and magnesium hydroxide;
[0121] 0.5 parts of silane coupling agent 172 is mixed with fillers aluminum hydroxide and magnesium hydroxide to improve the compatibility of the filler with the polymer matrix.
[0122] Add 0.2 parts of liquid additive antioxidant 1010, 2 parts of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent;
[0123] Add 1 part of peroxide curing agent DCP and polyethylene wax lubricant;
[0124] Obtain archived image information of each component in the reactor, obtain each particle feature in the archived image information, and calculate the particle area ratio of the total area of each particle feature to the total area of the archived image information to be 0.31, which is greater than the second preset particle area ratio of 0.172,
[0125] According to the area difference between the particle area ratio and the first preset particle area ratio of 0.085, the area difference is 0.225, which is greater than the second preset area difference of 0.192. The difference between the area difference of 0.225 and the second preset area difference of 0.192 is calculated to be 0.033, and the particle difference is 0.033, which is less than or equal to the first preset particle difference of 0.16. The preset stirring time is adjusted to the corresponding value using the first preset time adjustment coefficient of 1.12. The archived image information is retrieved, and the particle area ratio is retrieved to be 0.091, which is greater than the first preset particle area ratio of 0.085. The stirring speed of the current reactor is 67rpm, the current stirring power is 34KW, and the preset speed corresponding to the current stirring power is 70rpm. The stirring power-preset speed comparison table is as follows:
[0126] The difference between the preset speed and the stirring speed is calculated to obtain a speed deviation of 3 rpm, which is less than or equal to the second preset speed deviation of 6 rpm and greater than the first preset speed deviation of 2 rpm. The heating temperature is adjusted to the corresponding value using the second preset temperature adjustment coefficient of 1.151; the reactor uses the adjusted parameters to process the mixed material;
[0127] Re-acquire the features of each particle in the archived image information to recalculate the particle area ratio as 0.013, which is less than or equal to the first preset particle area ratio of 0.085, and determine that the mixed material meets the preset standard. The mixed material determined to meet the preset standard is extruded through an extruder; the cable sheath obtained after extrusion is vulcanized, and the vulcanized cable sheath is successively cooled and rolled up to obtain a second protective layer. Example 2
[0128] The second protective layer was prepared by weighing 47.8 parts of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 45.8 parts of aluminum hydroxide and magnesium hydroxide, 0.4 parts of antioxidant 1010, 4 parts of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, 2 parts of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant to prepare the second protective layer.
[0129] The archived image information of each component in the reactor is obtained, each particle feature in the archived image information is obtained, and the total area of each particle feature is calculated. The particle area ratio to the total area of the archived image information is 0.152, which is less than or equal to the second preset particle area ratio of 0.172 and greater than the first preset particle area ratio of 0.085. The archived image information of each component in the reactor is continuously obtained at preset intervals, and a time-particle area ratio curve is drawn based on each archived image information. The slope of the current time node is calculated to be -0.0031, which is less than or equal to the preset slope of -0.0027. The mixed material is determined to meet the preset standard, and the mixed material determined to meet the preset standard is extruded through an extruder; the cable sheath obtained after extrusion is vulcanized, and the cable sheath after the vulcanization treatment is successively cooled and rolled up to obtain a second protective layer. Example 3
[0130] For the preparation of the filling composition, 100 parts of EPDM rubber, 2.3 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide vulcanizer, 0.3 parts of co-vulcanizer, 50 parts of calcined clay filling reinforcing agent activated by silane coupling agent, 5 parts of microcrystalline wax, 0.8 parts of coupling agent, 8 parts of low-density polyethylene, 5 parts of zinc oxide nanopowder, 1.2 parts of antioxidant, 5 parts of red lead, 1.0 parts of magnesium oxide nanopowder, 15 parts of white carbon black, 0.2 parts of ion scavenger, 2 parts of nano-montmorillonite, and 10 parts of flame retardant Al(OH)3 were weighed.
[0131] 100 parts of EPDM rubber, 50 parts of calcined clay filler and reinforcing agent activated by silane coupling agent, 5 parts of microcrystalline wax, 0.8 parts of coupling agent, 8 parts of low-density polyethylene, 5 parts of zinc oxide nanopowder, 1.2 parts of antioxidant, 5 parts of red lead, 1.0 part of magnesium oxide nanopowder, 15 parts of white carbon black, 0.2 parts of ion scavenger, 2 parts of nano-montmorillonite and 10 parts of flame retardant Al(OH)3 were put into an internal mixer for mixing.
[0132] Mix at 110°C and filter through a filter to ensure the mixture is uniform and free of lumps.
[0133] Add 2.3 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide curing agent and 0.3 parts of co-curing agent into an internal mixer and continue mixing until completely dispersed.
[0134] The tensile strength was measured to be 9.5 MPa, the elongation at break was 520%, the elongation under a load of 0.2 MPa for 15 min at 200°C was 58%, and the permanent deformation was 5%. Example 4
[0135] For the preparation of the filling composition, 100 parts of EPDM rubber, 3.2 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide vulcanizer; 1.2 parts of co-vulcanizer, 67 parts of calcined clay filling reinforcing agent activated by silane coupling agent; 7 parts of microcrystalline wax, 1.2 parts of coupling agent, 10 parts of low-density polyethylene, 8 parts of zinc oxide nanopowder, 1.6 parts of antioxidant, 6 parts of red lead, 5 parts of magnesium oxide nanopowder, 25 parts of white carbon black, 5 parts of ion scavenger, 5 parts of nano-montmorillonite, and 15 parts of flame retardant Al(OH)3 were weighed to prepare the filling composition.
[0136] The tensile strength was measured to be 9.5 MPa, the elongation at break was 520%, the tensile strength was measured to be 9.5 MPa, the elongation at break was 520%, the elongation under a load of 0.2 MPa for 15 min at 200°C was 58%, and the permanent deformation was 5%. Example 5
[0137] The first protective layer was prepared by weighing 100 parts of chlorinated polyethylene, 30 parts of acetylene black, 50 parts of graphite powder, 1 part of antioxidant, 3 parts of organic peroxide, 4 parts of accelerator, 1 part of coupling agent, 10 parts of magnesium oxide, 1 part of stabilizer, 4 parts of methyl silicone oil, 4 parts of alkaline neutralizer and 30 parts of processing oil, and mixing them in a high-speed mixer. The mixed materials were placed in an internal mixer for internal mixing to ensure that all components were evenly dispersed.
[0138] The kneaded mixture is extruded through an extruder, the extruded semi-finished product is vulcanized, the vulcanized first protective layer is cooled by a cooling device, and then coiled.
[0139] The prepared first protective layer has a tensile strength of 15 MPa and an elongation at break of 300%.
[0140] At 200°C and 0.2 MPa for 15 min, the elongation is 173% and the permanent deformation is 15%. Example 6
[0141] The first protective layer is prepared by weighing 100 parts of chlorinated polyethylene, 50 parts of acetylene black, 70 parts of graphite powder, 2 parts of antioxidant, 4 parts of organic peroxide, 5 parts of accelerator, 2 parts of coupling agent, 20 parts of magnesium oxide, 1.5 parts of stabilizer, 8 parts of methyl silicone oil, 5 parts of alkaline neutralizer, and 40 parts of processing oil to prepare the first protective layer;
[0142] The tensile strength of the prepared first protective layer is 16 MPa and the elongation at break is 400%.
[0143] At 200°C and 0.2 MPa for 15 min, the elongation is 173% and the permanent deformation is 15%. Example 7
[0144] A second protective layer was prepared by weighing 48.3 parts of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 48.3 parts of aluminum hydroxide and magnesium hydroxide, 0.2 parts of antioxidant 1010, 2 parts of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, 1.2 parts of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant to prepare the second protective layer.
[0145] The second protective layer prepared by this scheme has a tensile strength of 11Mpa, an elongation at break of 300%, and the longest distance of the carbonized part in the cable bundle combustion test is 2.3 meters. Because capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent are added to the formula, it has effective rodent and ant repellent properties. The second protective layer prepared by this formula can effectively retard flames. Example 8
[0146] The second protective layer was prepared by weighing 47.8 parts of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 47.8 parts of aluminum hydroxide and magnesium hydroxide, 0.4 parts of antioxidant 1010, 2 parts of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, 2 parts of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant.
[0147] The second protective layer prepared by this scheme has a tensile strength of 11Mpa, an elongation at break of 300%, and the longest distance of the carbonized part in the cable bundle combustion test is 2.3 meters. Because capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent are added to the formula, it has effective rodent and ant repellent properties. The second protective layer prepared by this formula can effectively retard flames.
[0148] Comparative Example 1
[0149] The filling composition was prepared by the prior art, and 100 parts of EPDM rubber, 50 parts of calcined clay filler reinforcing agent activated by silane coupling agent, 5 parts of microcrystalline wax, 0.8 parts of coupling agent, 8 parts of low-density polyethylene, 5 parts of zinc oxide nanopowder, 5 parts of red lead, 1.0 parts of magnesium oxide nanopowder, 15 parts of white carbon black, 0.2 parts of ion scavenger, 2 parts of nano-montmorillonite and 10 parts of flame retardant Al(OH)3 were weighed and put into an internal mixer for mixing.
[0150] The tensile strength was measured to be 7.2 MPa and the elongation at break was 350%.
[0151] The elongation under load of 0.2MPa for 15min at 200℃ is 86% and the permanent deformation is 8%.
[0152] Comparing Example 3 and Example 4 with Comparative Example 1, the performance is significantly improved.
[0153] Comparative Example 2
[0154] The first protective layer is prepared by the existing technology, and 100 parts of chlorinated polyethylene, 30 parts of acetylene black, 50 parts of graphite powder, 1 part of antioxidant, 3 parts of organic peroxide, 3 parts of accelerator, 10 parts of magnesium oxide, 4 parts of methyl silicone oil, 4 parts of alkaline neutralizer and 30 parts of processing oil are weighed and put into a high-speed mixer for mixing, and the mixed materials are put into an internal mixer for internal mixing.
[0155] The tensile strength was measured to be 13MPa and the elongation at break was 210%;
[0156] At 200°C and 0.2 MPa for 15 min, the elongation is 180% and the permanent deformation is 18%.
[0157] Comparing Example 5 and Example 6 with Comparative Example 2, the performance is significantly improved.
[0158] Comparative Example 3
[0159] The second protective layer was prepared by the existing technology, and 48.3 parts of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 48.3 parts of aluminum hydroxide and magnesium hydroxide, 0.2 parts of antioxidant 1010, 1.2 parts of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant were weighed and added into a reactor for preparation.
[0160] The measured tensile strength is 9Mpa and the elongation at break is 210%; the longest distance of the carbonized part in the cable bundle combustion test is 3.2 meters.
[0161] Comparing Example 7 and Example 8 with Comparative Example 3, the performance is significantly improved.
[0162] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
[0163] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An anti-ant flame retardant cable, It is characterized in that include: Several cable cores, Each cable core is coated in a first protective layer, and a filling composition is filled between each cable core in the first protective layer, and a second protective layer is coated outside the first protective layer; The filling composition includes, by weight, 100 parts of EPDM rubber, 2.3-3.2 parts of 2,5-dimethyl-2,5-dibutyl peroxyacetylene peroxide vulcanizer; 0.3-1.2 parts of co-vulcanizer, 50-67 parts of calcined clay filling reinforcing agent activated by silane coupling agent; 5-7 parts of microcrystalline wax, 0.8-1.2 parts of coupling agent, 8-10 parts of low-density polyethylene, 5-8 parts of zinc oxide nanopowder, 1.2-1.6 parts of antioxidant, 5-6 parts of red lead, 1.0-5 parts of magnesium oxide nanopowder, 15-25 parts of white carbon black, 0.2-5 parts of ion scavenger, 2-5 parts of nano-montmorillonite, and 10-15 parts of flame retardant Al(OH)3; The first protective layer comprises, by weight, 30-50 parts of acetylene black, 50-70 parts of graphite powder, 1-2 parts of antioxidant, 3-4 parts of organic peroxide, 4-5 parts of accelerator, 1-2 parts of coupling agent, 10-20 parts of magnesium oxide, 1-1.5 parts of stabilizer, 4-8 parts of methyl silicone oil, 4-5 parts of alkaline neutralizer, and 30-40 parts of processing oil added to 100 parts of chlorinated polyethylene; The second protective layer includes 40% to 50% by mass of ethylene-vinyl acetate copolymer and ethylene propylene rubber, 40% to 55% by mass of aluminum hydroxide and magnesium hydroxide, 0.2% to 0.4% by mass of antioxidant 1010, 2% to 4% by mass of capsaicin environmentally friendly rodent repellent and cypermethrin low-toxic termite repellent, and 1.5% to 2% by mass of silane coupling agent 172, peroxide curing agent DCP and polyethylene wax lubricant; Preparation of anti-ant flame retardant cable, including: Step S1, adding each component of the filling composition into an internal mixer in a predetermined ratio for mixing, so as to complete the preparation of the filling composition; Step S2, adding the components of the first protective layer into an internal mixer for mixing, so as to complete the preparation of the first protective layer; Step S3, preparing a second protective layer, Step S31, adding the components of the second protective layer into a reactor according to a preset mass ratio, and heating and stirring the reactor; Step S32, when the running time of the reactor reaches an integer multiple of the preset stirring time, obtaining archived image information of each component in the reactor, obtaining each particle feature in the archived image information, and calculating the total area of each particle feature and the particle area ratio of the total area of the archived image information, and determining whether the preparation parameters of the protective layer meet the preset standards according to the obtained particle area ratio, including: If the particle area ratio is greater than the second preset particle area ratio, determining a treatment method for the reactor according to the area difference between the particle area ratio and the first preset particle area ratio; If the particle area ratio is less than or equal to the second preset particle area ratio and greater than the first preset particle area ratio, re-determining whether the preparation parameters of the protective layer meet the preset standards according to the slope of the drawn time-particle area ratio curve at the current time node; If the particle area ratio is less than or equal to the first preset particle area ratio, it is determined that the mixed material meets the preset standard; Step S33, adjusting the stirring power, heating temperature, or preset stirring time of each component of the reactor according to the area difference between the particle area ratio and the first preset particle area ratio; Step S34, the reactor processes the mixed material using the adjusted parameters; Step S35, extruding the mixed material determined to meet the preset standard through an extruder; Step S36, vulcanizing the cable sheath obtained after extrusion, and sequentially cooling and winding the vulcanized cable sheath; Step S4, wrapping a plurality of cable cores in the first protective layer, filling the filling composition between the cable cores in the first protective layer, and wrapping the second protective layer outside the first protective layer to complete the preparation of the anti-ant flame-retardant cable.
2. The anti-termite flame-retardant cable according to claim 1, It is characterized in that The treatment method for the reactor is determined based on the area difference, including: If the area difference is less than or equal to the first preset area difference, determining the stirring power of the reactor for each component according to the obtained mixing deviation of each component in the reactor; If the area difference is less than or equal to the second preset area difference and greater than the first preset area difference, the heating temperature of the reactor is adjusted to a corresponding value according to the rotation speed deviation; the first preset area difference is less than the second preset area difference; If the area difference is greater than the second preset area difference, the preset stirring time is adjusted to a corresponding value according to the difference between the area difference and the second preset area difference, and after the adjustment of the preset stirring time is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
3. The anti-termite flame-retardant cable according to claim 2, It is characterized in that Re-acquire archived image information of each component in the reactor at a preset interval, and obtain the particle area ratio of the archived image information, calculate the absolute value of the difference between the two particle area ratios, and record the absolute value as the mixing deviation; The adjustment method of the stirring power of the reactor for each component is determined according to the mixing deviation, wherein: If the mixing deviation is less than or equal to the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the first preset stirring adjustment coefficient; If the mixing deviation is less than or equal to the second preset mixing deviation and greater than the first preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the second preset stirring adjustment coefficient; the first preset mixing deviation is less than the second preset mixing deviation; If the mixing deviation is greater than the second preset mixing deviation, the stirring power of the reactor for each component is adjusted to a corresponding value using the third preset stirring adjustment coefficient; After the adjustment of the stirring power is completed, it is determined whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information.
4. The anti-termite flame-retardant cable according to claim 3, It is characterized in that Determine whether the preparation parameters of the protective layer meet the preset standards based on the re-acquired archived image information, including: When the reacquired particle area ratio is greater than the first preset particle area ratio, the heating temperature is adjusted to the corresponding value according to the speed deviation; when the reacquired particle area ratio is less than or equal to the first preset particle area ratio, the reactor is controlled to continue operating using the current operating parameters.
5. The anti-termite flame-retardant cable according to claim 4, It is characterized in that The regulation method for the heating temperature is determined based on the speed deviation, where: If the speed deviation is less than or equal to the first preset speed deviation, the heating temperature is adjusted to a corresponding value using the first preset temperature adjustment coefficient; If the speed deviation is less than or equal to the second preset speed deviation and greater than the first preset speed deviation, the heating temperature is adjusted to the corresponding value using the second preset temperature adjustment coefficient; the first preset speed deviation is less than the second preset speed deviation; If the speed deviation is greater than the second preset speed deviation, the heating temperature is adjusted to a corresponding value using a third preset temperature adjustment coefficient; The process of obtaining the speed deviation is to obtain the stirring speed of the current reactor, obtain the preset speed corresponding to the current stirring power, calculate the difference between the preset speed and the stirring speed, and obtain the speed deviation.
6. The anti-termite flame-retardant cable according to claim 5, It is characterized in that The difference between the area difference and the second preset area difference is calculated and recorded as the particle difference, and the adjustment method for the preset stirring time is determined based on the particle difference, wherein: If the particle difference is less than or equal to the first preset particle difference, the preset stirring time is adjusted to a corresponding value using the first preset time adjustment coefficient; If the particle difference is less than or equal to the second preset particle difference and greater than the first preset particle difference, the preset stirring time is adjusted to the corresponding value using the second preset time adjustment coefficient; the first preset particle difference is less than the second preset particle difference; If the particle difference is greater than the second preset particle difference, the preset stirring time is adjusted to a corresponding value using the third preset time adjustment coefficient.
7. The anti-termite flame-retardant cable according to claim 6, It is characterized in that The archived image information of each component in the reactor is continuously obtained at preset intervals, a time-particle area ratio curve is drawn based on each archived image information, and whether the preparation parameters of the protective layer meet the preset standards is determined according to the slope of the time-particle area ratio curve at the current time node, including: If the slope is greater than the preset slope, a treatment method for the reactor is determined according to the area difference between the current particle area ratio and the first preset particle area ratio; If the slope is less than or equal to a preset slope, it is determined that the mixed material meets the preset standard.
Citation Information
Patent Citations
Anti-termite flame-retardant cable and preparation method thereof
CN115050511A
Mouse-preventing termite-proof halogen-free flame-retarding environment-friendly low smoke cable for electric lift control
CN101105988A
Peelable insulation shielding material used in mining high-voltage rubber insulated cables
CN101613507A
Ethylene-propylene rubber insulating mouse-proof insect-proof low-smoke halogen-free flame-retardant direct-current high-voltage cable insulating material used for rail traffic
CN102682870A
Degaussing cable with high heat conduction and low temperature rise used for ships and warships and manufacturing method thereof
CN108447600A
Cited By
Anti-rat and anti-termite decay cable and preparation method thereof
CN122050932A