Multi-ion doped silicon-carbon composite material and preparation method thereof
By adding a metal conductive agent doped with lithium salt to magnesium-tin doped porous silicon carbon, a multi-ion doped silicon carbon composite material is formed, which solves the problem of poor fast charging performance and large expansion rate of silicon carbon materials in fast charging batteries. problem, achieving higher conductivity and stability, improving the overall performance of the battery.
Patent Information
- Application Number
- CN202410950641.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Existing silicon-carbon materials in fast-charging batteries have poor fast-charging performance, large expansion rates, and poor electronic conductivity, which limits their batch use in the field of high-energy-density fast-charging batteries.
Multi-ion doped silicon carbon composite materials are used, and a metal conductive agent is added to the magnesium-tin doped porous silicon carbon to dope lithium salt to form a matrix and surface layer structure, improve the conductivity and structural stability of the material, and reduce the expansion rate.
It significantly improves the material's fast charging performance and cycle performance, reduces the expansion rate, enhances the battery's rate performance and stability, and improves the battery's overall conductivity and lithium storage capacity.
Smart Images

Figure CN118507696B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery materials, and in particular relates to a multi-ion doped silicon-carbon composite material and a preparation method thereof. Background Art
[0002] Silicon-based materials are favored for their low potential and extremely high theoretical capacity. However, during the process of lithium ion insertion and extraction, the large expansion of nano-silicon easily causes the material on the surface of the pole piece to pulverize and the cycle capacity to decay rapidly. At the same time, silicon has poor electronic conductivity, which causes deviations in the material's normal and low temperature charging capabilities. Therefore, new silicon-carbon materials as a composite material have attracted the attention of technicians in this field.
[0003] The new silicon-carbon material in the related technology is composed of porous carbon and deposited nano-silicon. Although the expansion is improved, the improvement is not large and the fast charging performance of the material is biased, which limits its mass use in the field of high energy density fast charging batteries.
[0004] At the same time, the current new silicon carbon has defects such as poor electronic conductivity, which leads to its insufficient fast charging performance. In this regard, in order to improve the fast charging performance, the main measures adopted include: doping metals (magnesium, lithium, etc.) or non-metallic materials (nitrogen, boron, etc.) in porous carbon to improve the electronic conductivity of the material, but in fact, although the impedance is reduced, the reduction is limited, and it will cause the material to expand. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a multi-ion doped silicon-carbon composite material and a preparation method thereof, aiming to solve the problems of poor fast charging performance and large expansion rate of battery materials.
[0006] To solve the above technical problems, the present invention is implemented as follows: the present invention proposes a multi-ion doped silicon-carbon composite material, which includes a matrix and a surface layer, wherein the surface layer is formed on the outer surface of the matrix, the matrix is magnesium-tin doped porous silicon-carbon, and the surface layer is a metal conductive agent doped lithium salt. Calculated by mass percentage, the mass proportion of the metal conductive agent doped lithium salt is 1~5wt%, and the remainder is the magnesium-tin doped porous silicon-carbon.
[0007] In some embodiments of the present invention, the components in the magnesium-tin-doped porous silicon carbon include magnesium ions, tin ions, porous carbon and nano-silicon, wherein, calculated by mass percentage, the magnesium ions account for 0.5~2wt%, the tin ions account for 0.5~2wt%, the porous carbon accounts for 42~49wt%, and the remainder is the nano-silicon.
[0008] In some embodiments of the present invention, the components in the metal conductive agent-doped lithium salt include a metal conductive agent, a lithium salt compound and amorphous carbon, wherein, calculated by mass percentage, the metal conductive agent accounts for 5-15%, the lithium salt compound accounts for 50-80%, and the remainder is the amorphous carbon.
[0009] The present invention provides a preparation method for preparing a multi-ion doped silicon-carbon composite material, the preparation method comprising the following steps:
[0010] S1, adding mesoporous carbon to a mixed solution of magnesium salt and tin salt to disperse evenly, and transferring to a high-pressure reactor for hydrothermal reaction to obtain a mesoporous carbon mixed solution;
[0011] Wherein, according to the mass ratio, the mesoporous carbon: the magnesium salt: the tin salt = 50:1-5:1-5, the reaction temperature of the hydrothermal reaction is 100-200° C., the reaction pressure is 1-5 MPa, and the reaction time is 12-48 h;
[0012] S2, filtering and vacuum drying the mesoporous carbon mixed solution in sequence, and carbonizing the filter residue to obtain a magnesium-tin co-doped carbon matrix;
[0013] Among them, the drying temperature is 80°C, the drying time is 24h, the carbonization temperature is 800~1200°C, and the carbonization time is 1~6h;
[0014] S3, transferring the magnesium-tin co-doped carbon matrix into a fluidized bed in an inert atmosphere, introducing a chlorosilane mixed gas to perform a deposition reaction, and obtaining magnesium-tin doped porous silicon carbon;
[0015] The chlorosilane mixed gas includes chlorosilane and argon, and the volume ratio of the chlorosilane: the argon is 1-5:1. The flow rate of the chlorosilane mixed gas is 100-1000 sccm. The reaction temperature of the deposition reaction is 400-600° C., and the reaction time is 0.5-2 h.
[0016] S4, uniformly dispersing the organic lithium salt and the metal conductive agent in an organic solvent to obtain a solution A;
[0017] Wherein, according to the mass ratio, the organic lithium salt: the metal conductive agent: the organic solvent = 1-10: 0.5-2: 500-1000;
[0018] S5, adding the magnesium tin doped porous silicon carbon into a reactor in an inert atmosphere, adding the solution A into a spray nozzle for atomization, depositing the atomized solution A on the surface of the magnesium tin doped porous silicon carbon, and then carbonizing the deposited magnesium tin doped porous silicon carbon to prepare the multi-ion doped silicon carbon composite material;
[0019] The reactor is equipped with a spray nozzle, a gas controller and a temperature controller. According to the mass ratio, the magnesium tin doped porous silicon carbon: the solution A=100:100~500, the atomization pressure of the spray nozzle is 0.1~1Mpa, the atomization temperature is 100~200°C, the gas flow rate is 100~500sccm, the reaction temperature of the carbonization reaction is 800~1100°C, and the reaction time is 1~6h.
[0020] In some embodiments of the present invention, in step S5, the step of adding the solution A to the spray nozzle for atomization comprises:
[0021] Setting the injection parameters of the injection nozzle, wherein the injection parameters of the injection nozzle include injection diameter, injection pressure and gas flow rate;
[0022] Obtain the particle size distribution data of the solution A and substitute the particle size distribution data into the fitting curve equation to obtain a fitting result, wherein the fitting curve equation is , is the mass fraction of particles with a diameter smaller than d, is the median particle size, n is the distribution parameter, and the larger the distribution parameter, the smaller the particle size distribution range of the solution A;
[0023] The injection parameters of the injection nozzle are adjusted according to the fitting result until the median particle size and the fraction parameter are both within a preset range.
[0024] In some embodiments of the present invention, the step of depositing the atomized solution A on the surface of the magnesium-tin-doped porous silicon carbon comprises:
[0025] Set target temperature and target gas flow rate;
[0026] Obtaining the actual temperature and the actual gas flow rate and calculating the errors with the target temperature and the target gas flow rate respectively;
[0027] The adjustment value of the gas controller and the adjustment value of the temperature controller are calculated respectively, and the gas controller and the temperature controller are correspondingly adjusted according to the adjustment values until the target temperature and the target gas flow rate are reached.
[0028] In some embodiments of the present invention, the calculation formula of the adjustment value of the temperature controller is: , is the adjustment value of the temperature controller, t is the time, is the first temperature influencing factor, is the second temperature influencing factor, is the third temperature influencing factor, is the error between the actual temperature and the target temperature,
[0029] The calculation formula of the adjustment value of the gas controller is: , is the adjustment value of the gas controller, is the first gas flow rate influencing factor, is the second gas flow rate influencing factor, is the third gas flow rate influencing factor, is the error between the actual gas flow rate and the target gas flow rate.
[0030] In some embodiments of the present invention, in step S1, the magnesium salt includes at least one of magnesium chloride, magnesium sulfate, magnesium carbonate, and magnesium nitrate, with a concentration of 1 to 10 wt%; the tin salt includes at least one of tin chloride, tin tetrachloride, tin sulfate, tin sulfide, and tin oxide, with a concentration of 1 to 10 wt%; the pore volume of the mesoporous carbon is 0.9 to 1.1 cm 3 / g, specific surface area 1000~1500m 2 / g.
[0031] In some embodiments of the present invention, in step S3, the chlorosilane includes at least one of trichlorosilane, tetrachlorosilane, dimethylchlorosilane, propenyltrichlorosilane, pentyltrichlorosilane, methylvinyldichlorosilane, triisopropylchlorosilane, propyltrichlorosilane, and 2-methylbutyltrichlorosilane.
[0032] In some embodiments of the present invention, in step S4, the organic lithium salt includes at least one of lithium pyruvate, lithium stearate, lithium acetate, lithium difluoroborate, lithium 4-methylbenzenesulfonate, and lithium benzoate; the metal conductive agent includes at least one of copper nanowires, silver nanowires, copper nanowires, and tin oxide nanowires; the metal conductive agent has a length of 50 to 200 nm and a diameter of 10 to 30 µm; and the organic solvent includes at least one of methanol, ethanol, butanediol, isopropanol, and benzyl alcohol.
[0033] Compared with the prior art, the multi-ion doped silicon-carbon composite material and the preparation method thereof in the present invention have the following beneficial effects:
[0034] By doping porous carbon with magnesium and tin elements, magnesium silicate formed by magnesium and silicon during the charge and discharge process can improve structural stability and cycle performance, and the catalytic effect of tin can make nano-silicon more evenly deposited in the porous carbon, reducing expansion; at the same time, magnesium-tin doped porous carbon improves the problem of poor electronic conductivity of porous carbon itself and improves rate performance. Lithium salt materials and metal conductive agents have the characteristics of high metal conductivity and electronic conductivity, which are used to improve the rate performance of batteries to enhance fast charging performance. The metal conductive agent coated on the surface of the silicon-carbon material effectively restrains the expansion of silicon during charge and discharge, reducing the expansion of the silicon-carbon composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic diagram of a process of preparing a multi-ion doped silicon-carbon composite material in accordance with an embodiment of the present invention;
[0036] Figure 2 yes Figure 1 A schematic flow chart of the specific steps of step S5;
[0037] Figure 3 This is a SEM image of the multi-ion doped silicon-carbon composite material in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0039] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0040] The present invention proposes a multi-ion doped silicon-carbon composite material, which includes a matrix and a surface layer. The surface layer is formed on the outer surface of the matrix. The matrix is magnesium-tin doped porous silicon-carbon, and the surface layer is a metal conductive agent doped lithium salt. Calculated by mass percentage, the mass proportion of the metal conductive agent doped lithium salt is 1~5wt%, and the remainder is magnesium-tin doped porous silicon-carbon.
[0041] By doping porous carbon with magnesium tin elements, the structural stability and cycle performance are improved by relying on the magnesium silicate formed by magnesium and silicon during the charge and discharge process. The catalytic effect of tin makes the nano-silicon more evenly deposited in the porous carbon, reducing expansion. At the same time, magnesium tin-doped porous carbon improves the problem of poor electronic conductivity of the porous carbon itself and improves the rate performance.
[0042] Lithium salt materials have the characteristics of high metallic conductivity and electronic conductivity, and are used to improve the rate performance of batteries; the high electronic conductivity of the metal conductive agent itself and its coating on the surface of the silicon-carbon material are used to restrain the expansion of silicon during charging and discharging, thereby reducing the expansion of the silicon-carbon composite material.
[0043] Preferably, in one embodiment, the weight of the metal conductive agent doped with lithium salt accounts for 3 wt %, and the remainder is magnesium tin doped porous silicon carbon.
[0044] Specifically, the components in magnesium-tin-doped porous silicon carbon include magnesium ions, tin ions, porous carbon and nano-silicon, wherein, calculated by mass percentage, magnesium ions account for 0.5~2wt%, tin ions account for 0.5~2wt%, porous carbon accounts for 42~49wt%, and the remainder is nano-silicon.
[0045] In one embodiment, magnesium ions account for 1 wt %, tin ions account for 1 wt %, porous carbon accounts for 49 wt %, and the remainder is nano-silicon.
[0046] Magnesium ions have high electrochemical activity and can improve the conductivity and electrochemical reaction rate of multi-ion-doped silicon-carbon composites. Magnesium ion doping can effectively improve the structural stability and conductivity of multi-ion-doped silicon-carbon composites, reduce the volume change of silicon during the charge and discharge process, and thus improve the cycle life and electrochemical performance. Tin ions have good alloying and dealloying properties, and can form alloys with lithium ions during the charge and discharge process to improve the specific capacity and rate performance of the material. Tin ion doping can improve the reversible capacity and rate performance of multi-ion-doped silicon-carbon composites, while improving their conductivity and stability, and increasing the cycle life of multi-ion-doped silicon-carbon composites.
[0047] Porous carbon has a high specific surface area and porous structure, which helps to improve the charge transfer efficiency, electrolyte permeability and diffusion performance of multi-ion doped silicon-carbon composites. Porous carbon plays a supporting and conductive role in multi-ion doped silicon-carbon composites, provides more active sites, buffers the volume change of silicon during the charge and discharge process, and improves the overall stability and conductivity of multi-ion doped silicon-carbon composites. Nano silicon has a high theoretical specific capacity and can form alloys with lithium ions during the charge and discharge process to increase the capacity of the material. Nano silicon is the main active substance of multi-ion doped silicon-carbon composites, which improves the lithium storage capacity of the material. However, the volume expansion of silicon during the charge and discharge process is large, which easily leads to the pulverization and capacity attenuation of multi-ion doped silicon-carbon composites. By compounding with magnesium, tin and porous carbon, these problems can be effectively alleviated, and the cycle performance and stability of multi-ion doped silicon-carbon composites can be improved.
[0048] The components of the metal conductive agent doped lithium salt include a metal conductive agent, a lithium salt compound and amorphous carbon, wherein, calculated by weight percentage, the metal conductive agent accounts for 5~15wt%, the lithium salt compound accounts for 50~80wt%, and the remainder is amorphous carbon.
[0049] In one embodiment, the metal conductive agent accounts for 5 wt %, the lithium salt compound accounts for 50 wt %, and the remainder is amorphous carbon.
[0050] Metallic conductive agents have excellent electrical conductivity and can significantly improve the overall electrical conductivity of composite materials, reduce resistance, and promote the transmission of electrons in electrodes. In multi-ion doped silicon-carbon composite materials, the main function of metallic conductive agents is to improve electrical conductivity and ensure efficient electrode reactions. Common metallic conductive agents include copper, tin, silver, etc. They can form a conductive network inside the material, improve the electronic conductivity of the material, and enhance the rate of electrochemical reactions.
[0051] Lithium salt compounds are the source of lithium ions and have high ionic conductivity. They can provide sufficient lithium ions during the charge and discharge process to ensure the electrode reaction. Lithium salt compounds provide lithium ions in composite materials. Lithium salts can release lithium ions in the electrolyte, allowing them to migrate freely between electrodes to ensure the normal operation of the battery. The high ionic conductivity of lithium salt compounds also helps to improve the charge and discharge efficiency and rate performance of the battery.
[0052] Amorphous carbon has good compatibility with the electrolyte and good conductivity, which can improve the electron transport capacity of multi-ion doped silicon-carbon composites and provide more reaction sites. Amorphous carbon plays a dual role of support and conductivity in multi-ion doped silicon-carbon composites. First, it can provide structural support, alleviate the volume change of multi-ion doped silicon-carbon composites during the charging and discharging process, and enhance the mechanical stability of the material. Secondly, it can improve the conductivity of multi-ion doped silicon-carbon composites and ensure the efficient electrochemical reaction. In addition, amorphous carbon has good compatibility with the electrolyte, reduces side reactions, and isolates the core silicon from direct contact with the electrolyte, reducing side reactions and improving storage performance.
[0053] Embodiment 1:
[0054] Please refer to Figure 1 and Figure 2 Embodiment 1 of the present invention provides a preparation method for preparing a multi-ion doped silicon-carbon composite material, the preparation method comprising the following steps:
[0055] S1. Add mesoporous carbon to a mixed solution of magnesium salt and tin salt and disperse it evenly, and transfer it to a high-pressure reactor for hydrothermal reaction to obtain a mesoporous carbon mixed solution; wherein, according to the mass ratio, mesoporous carbon: magnesium salt: tin salt = 50:3:3, the mesoporous carbon is 50g, and the pore volume of the mesoporous carbon is 0.9cm 3 / g, specific surface area is 1000m 2 / g, the magnesium salt is 60g of 5wt% magnesium chloride solution, the tin salt is 60g of 5wt% tin chloride solution, the reaction temperature of the hydrothermal reaction is 150°C, the reaction pressure is 3Mpa, and the reaction time is 24h.
[0056] Mesoporous carbon has a high specific surface area and good electrical conductivity, which provides a large number of active sites for the loading of magnesium and tin ions. The hydrothermal reaction is carried out under high temperature and high pressure conditions, which can effectively promote the loading and compounding of magnesium and tin ions on mesoporous carbon, and at the same time help to form a uniform nanostructure.
[0057] S2. The mesoporous carbon mixed solution is filtered and vacuum dried in sequence, and the filter residue is carbonized to obtain a magnesium-tin co-doped carbon matrix; wherein the drying temperature is 80°C, the drying time is 24h, the carbonization temperature is 1000°C, and the carbonization time is 3h.
[0058] The carbonization process can optimize the pore structure of mesoporous carbon and convert mesoporous carbon into porous carbon with a higher specific surface area, which is beneficial to the penetration of electrolyte and ion transport. The carbonization treatment is carried out at high temperature, which can make the magnesium salt and tin salt better dispersed in the carbon material and form stable carbides. At the same time, high-temperature carbonization helps to remove organic residues and improve the conductivity of the material.
[0059] The carbonization process can be carried out in a tubular furnace with a temperature control device. The tubular furnace is heated in sections. The sectioned heating can accurately control each stage of the carbonization process by gradually increasing the temperature, ensuring the heat treatment effect of the material in each temperature range.
[0060] S3. Transfer the magnesium-tin co-doped carbon matrix to a fluidized bed in an inert atmosphere, introduce a chlorosilane mixed gas for deposition reaction, and obtain magnesium-tin doped porous silicon carbon; wherein the chlorosilane mixed gas includes trichlorosilane and argon, and the volume ratio of trichlorosilane: argon is 3:1, the flow rate of the chlorosilane mixed gas is 500 sccm, the reaction temperature of the deposition reaction is 500°C, and the reaction time is 1 hour.
[0061] The inert gas introduced into the fluidized bed is argon. The inert atmosphere can effectively reduce the interference of impurities such as oxygen on the reaction, which is conducive to maintaining the purity and efficiency of the reaction. The particles in the fluidized bed in the inert atmosphere are in a suspended state, which can be evenly heated and transferred, avoiding local overheating or uneven reaction problems. Reacting in a fluidized bed can ensure uniform mixing and doping of magnesium, tin and carbon materials, thereby improving the uniformity and performance stability of magnesium-tin doped porous silicon carbon.
[0062] S4, uniformly dispersing the organic lithium salt and the metal conductive agent in an organic solvent to obtain a solution A; wherein, according to the mass ratio, the organic lithium salt: the metal conductive agent: the organic solvent = 5:1:800. The organic lithium salt is 5g of lithium pyruvate, the metal conductive agent is 1g of copper nanowires, the length of the copper nanowires is 100nm, the diameter is 20µm, the organic solvent is 800g of methanol solution, and the dispersion method is ultrasonic dispersion.
[0063] The organic lithium salt and the metal conductive agent are evenly dispersed in the organic solvent by ultrasonic dispersion to ensure the uniform distribution of each component in the solution. Ultrasonic dispersion can effectively break the agglomeration phenomenon, improve the dispersibility of copper nanowires, and ensure that each nanowire can fully exert its conductive effect.
[0064] Methanol as an organic solvent has good solubility and volatility, and can effectively dissolve organic lithium salts and evenly disperse copper nanowires to form a stable solution A, which is helpful for subsequent processes, and the volatility of methanol can be quickly removed in the subsequent drying process.
[0065] S5, adding magnesium tin doped porous silicon carbon to a reactor in an inert atmosphere, adding solution A to a spray nozzle for atomization, depositing the atomized solution A on the surface of the magnesium tin doped porous silicon carbon, and then carbonizing the deposited magnesium tin doped porous silicon carbon to prepare a multi-ion doped silicon carbon composite material. The reactor is equipped with a spray nozzle, a gas sensor, and a temperature sensor.
[0066] Solution A is atomized through a spray nozzle to form tiny droplets, which are uniformly deposited on the surface of magnesium-tin-doped porous silicon-carbon, with good deposition uniformity, high efficiency, and low deposition temperature, which reduces the growth rate of silicon grains, reduces expansion, and gives full play to the high ion conductivity of lithium salt materials and the high metal conductivity and electronic conductivity and the synergistic effect between them to improve the rate performance. Carbonization reaction of the deposited multi-ion doped silicon-carbon composite material can enhance the mechanical strength and conductivity of the multi-ion doped silicon-carbon composite material, and further stabilize the structure of the multi-ion doped silicon-carbon composite material.
[0067] In order to improve the deposition effect of solution A, it is necessary to adjust the parameters of the spray nozzle. The step of adding solution A to the spray nozzle for atomization includes:
[0068] S5.1. Set the injection parameters of the injection nozzle, wherein the injection parameters of the injection nozzle include injection pressure and gas flow rate. The injection parameters set at this time are the injection parameters in the initial state, which can be set based on experience. In the case of preparing multi-ion-doped silicon-carbon composite materials multiple times, the initial injection parameters can be the same or different.
[0069] The spray nozzle is equipped with a control valve to control the spray diameter of the spray nozzle, thereby controlling the spray pressure. Reducing the spray diameter will increase the spray pressure, and increasing the spray pressure will produce finer atomized particles, thereby reducing the average size of the atomized particle size of solution A. Increasing the spray diameter will reduce the spray pressure, and reducing the spray pressure will produce coarser atomized particles, thereby increasing the average size of the atomized particle size of solution A. Increasing the gas flow rate will increase the atomization efficiency, thereby reducing the distribution range of the atomized particle size of solution A, resulting in a more concentrated atomized particle size of solution A, and reducing the difference between each other. Reducing the gas flow rate will increase the atomization efficiency, thereby increasing the distribution range of the atomized particle size of solution A, resulting in a more dispersed atomized particle size of solution A, and increasing the difference between each other.
[0070] S5.2. Obtain the particle size distribution data of solution A and substitute the particle size distribution data into the fitting curve equation to obtain the fitting result, where the fitting curve equation is: , is the mass fraction of particles with a diameter smaller than d, is the median particle size, n is the distribution parameter, and the larger the distribution parameter is, the smaller the particle size distribution range of solution A is.
[0071] The particle size distribution data of solution A can be obtained by emitting laser light from the built-in laser module. The laser light diffracts and scatters through the atomized particles of solution A, and the particle size distribution of the atomized particles is measured. The distribution parameter n is a key parameter that describes the steepness of the particle size distribution. The larger the distribution parameter, the more concentrated the distribution of the atomized particles of solution A is, and the difference in particle size between each other is not large, which is conducive to forming a uniform deposition layer on magnesium-tin-doped porous silicon carbon.
[0072] Median particle size It refers to the particle size when the cumulative distribution in the particle group reaches 50%. It is a key indicator of particle size distribution, reflecting the central trend of particle distribution, median particle size The larger the value, the larger the atomized particles of solution A are. In lithium-ion batteries, larger particle sizes will affect the structure and electrochemical properties of the electrode. Large particles will reduce the surface area of the electrode, affecting the current density and reaction rate.
[0073] Will Convert to , linearize both ends of the two equations to obtain the linear equation , perform linear regression fitting on the straight line equation, that is, n is the slope of the straight line, is the distribution parameter, is the intercept of the straight line, and the median particle size is calculated by substituting the distribution parameter n into .
[0074] S5.3, adjusting the injection parameters of the injection nozzle according to the fitting results until the median particle size and distribution parameters are within the preset range. If the median particle size and distribution parameters in the fitting results are not within the preset range, repeat step S5.1 to adjust the injection parameters.
[0075] That is, when the median particle size in the fitting result is greater than the maximum value of the preset range, the injection diameter is reduced to increase the injection pressure, and when the median particle size in the fitting result is less than the minimum value of the preset range, the injection diameter is increased to reduce the injection pressure. When the distribution parameter in the fitting result is greater than the maximum value of the preset range, the gas flow rate is reduced, and when the distribution parameter in the fitting result is less than the minimum value of the preset range, the gas flow rate is increased.
[0076] Specifically, the set of particle sizes d is [1, 2, 3, 4, 5, 6, 7, 8, 9, 10] (unit: micrometer), The set is [0.1, 0.2, 0.3, 0.45, 0.6, 0.75, 0.85, 0.92, 0.97, 0.99], that is, the calculated fitted median particle size is 7 microns and the fitted distribution parameter is 3.
[0077] According to the mass ratio, magnesium tin doped porous silicon carbon: solution A = 100:300, the injection parameters of the nozzle in the initial state are atomization pressure of 0.5 MPa, gas flow rate of 300 sccm, atomization temperature of 150°C, reaction temperature of carbonization reaction of 1000°C, and reaction time of 3h.
[0078] Furthermore, in order to precisely control the deposition reaction, the step of depositing the atomized solution A on the surface of the magnesium-tin-doped porous silicon-carbon comprises:
[0079] S5.4. Set the target temperature and target gas flow rate.
[0080] The target temperature was set to be 150°C for atomization, and the target gas flow rate was set to be 300 sccm.
[0081] S5.5. Obtain the actual temperature and the actual gas flow rate and calculate the errors with the target temperature and the target gas flow rate respectively; the error between the actual temperature and the target temperature is the difference between the two, and the error between the actual temperature and the target temperature is the difference between the two.
[0082] S5.6. Calculate the adjustment value of the gas controller and the adjustment value of the temperature controller respectively, and adjust the gas controller and the temperature controller accordingly according to the adjustment values until the target temperature and the target gas flow rate are reached.
[0083] The calculation formula for the adjustment value of the temperature controller is , is the adjustment value of the temperature controller, t is the time, is the error between the actual temperature and the target temperature, and the adjustment value of the temperature controller is the power of the heating wire.
[0084] The first temperature influence factor determines the influence of the current error on the temperature controller. The larger the first temperature influence factor, the faster the controller responds to the current error. In other words, increasing the first temperature influence factor will speed up the response of the temperature controller, but may cause overshoot and oscillation. A too small first temperature influence factor will make the system respond slowly and fail to correct the error quickly.
[0085] The second temperature influence factor determines the degree of influence of the cumulative error on the control output. The cumulative error is the cumulative value of the error in the period from 0 to t. The larger the second temperature influence factor, the stronger the temperature controller reacts to the accumulation of past errors. By integrating the accumulated errors over time, the steady-state error of the system is eliminated. Increasing the second temperature influence factor can eliminate the steady-state error of the system and make the output value reach the set value accurately. An excessively large second temperature influence factor may cause the system to respond slowly and cause oscillation or overshoot.
[0086] The third temperature influence factor determines the degree of influence of the error change rate on the control output. The larger the third temperature influence factor, the faster the temperature controller reacts to the trend of error change. By calculating the derivative of the error, the error change trend is predicted and the dynamic response of the system is improved. Increasing the third temperature influence factor can reduce the overshoot of the system, improve stability, and quickly slow down the error change. An excessively large third temperature influence factor leads to unstable control signals.
[0087] The calculation formula for the adjustment value of the gas controller is , is the adjustment value of the gas controller, is the first gas flow rate influencing factor, is the second gas flow rate influencing factor, is the third gas flow rate influencing factor, is the error between the actual gas flow and the target gas flow, and the adjustment value of the gas controller is the opening of the gas valve. The functions of the first gas flow influencing factor, the second gas flow influencing factor and the third gas flow influencing factor are the same as above and will not be repeated.
[0088] Taking the calculation formula of the adjustment value of the temperature controller as an example, how to determine the corresponding The impact factors can be achieved through the following steps:
[0089] Only the first temperature influence factor is set and the first temperature influence factor is gradually increased until the temperature output by the temperature controller approaches the target temperature;
[0090] Maintaining the first temperature influence factor unchanged, and continuously adjusting the second temperature influence factor until the temperature output by the temperature controller is closer to the target temperature;
[0091] The first temperature influence factor and the second temperature influence factor are maintained unchanged, and the third temperature influence factor is continuously adjusted until the temperature output by the temperature controller reaches the target temperature.
[0092] The first temperature influence factor, the second temperature influence factor, and the third temperature influence factor have a proportional relationship, and the first temperature influence factor is the largest and the third temperature influence factor is the smallest. =2, =0.1 , =0.01 =0.02.
[0093] Embodiment 2:
[0094] Embodiment 2 of the present invention provides a preparation method for preparing a multi-ion doped silicon-carbon composite material, the preparation method comprising the following steps:
[0095] S1. Add mesoporous carbon to a mixed solution of magnesium salt and tin salt and disperse it evenly, and transfer it to a high-pressure reactor for hydrothermal reaction to obtain a mesoporous carbon mixed solution; wherein, according to the mass ratio, mesoporous carbon: magnesium salt: tin salt = 50:1:1, the mesoporous carbon is 50g, and the pore volume of the mesoporous carbon is 1cm 3 / g, specific surface area is 1200m 2 / g, the magnesium salt is 100g of 1wt% magnesium sulfate solution, the tin salt is 100g of 1wt% tin sulfate solution, the reaction temperature of the hydrothermal reaction is 100°C, the reaction pressure is 5Mpa, and the reaction time is 48h.
[0096] S2. The mesoporous carbon mixed solution is filtered and vacuum dried in sequence, and the filter residue is carbonized to obtain a magnesium-tin co-doped carbon matrix; wherein the drying temperature is 80°C, the drying time is 24h, the carbonization temperature is 800°C, and the carbonization time is 6h.
[0097] S3. Transfer the magnesium-tin co-doped carbon matrix to a fluidized bed in an inert atmosphere, introduce a chlorosilane mixed gas for deposition reaction, and obtain magnesium-tin doped porous silicon carbon; wherein the chlorosilane mixed gas includes tetrachlorosilane and argon, and the volume ratio of tetrachlorosilane: argon is 1:1, the flow rate of the chlorosilane mixed gas is 1000 sccm, the reaction temperature of the deposition reaction is 400°C, and the reaction time is 0.5h.
[0098] S4. Disperse the organic lithium salt and the metal conductive agent uniformly in an organic solvent to obtain solution A; wherein, according to the mass ratio, the organic lithium salt: the metal conductive agent: the organic solvent = 1:0.5:500. The organic lithium salt is 1g of lithium stearate, the metal conductive agent is 0.5g of silver nanowires, the length of the silver nanowires is 100nm, the diameter is 20µm, the organic solvent is 500g of butanediol solution, and the dispersion method is ultrasonic dispersion.
[0099] S5. Add magnesium tin doped porous silicon carbon into a reactor with an inert atmosphere, add solution A into the nozzle for atomization, deposit the atomized solution A on the surface of the magnesium tin doped porous silicon carbon, and then carbonize the deposited magnesium tin doped porous silicon carbon to prepare a multi-ion doped silicon carbon composite material.
[0100] The reactor is equipped with a spray nozzle, a gas sensor and a temperature sensor. According to the mass ratio, magnesium tin doped porous silicon carbon: solution A = 100:100, the spray parameters of the spray nozzle in the initial state are atomization pressure of 0.1Mpa, gas flow rate of 100sccm, atomization temperature of 100°C, carbonization reaction temperature of 800°C, and reaction time of 6h. The adjustment of the spray nozzle and the reaction control in the reactor are the same as in Example 1, only adaptive changes are made, and no further description is given here.
[0101] Embodiment 3:
[0102] Embodiment 3 of the present invention provides a preparation method for preparing a multi-ion doped silicon-carbon composite material, the preparation method comprising the following steps:
[0103] S1. Add mesoporous carbon to a mixed solution of magnesium salt and tin salt and disperse it evenly, and transfer it to a high-pressure reactor for hydrothermal reaction to obtain a mesoporous carbon mixed solution; wherein, according to the mass ratio, mesoporous carbon: magnesium salt: tin salt = 50:5:5, the mesoporous carbon is 50g, and the pore volume of the mesoporous carbon is 1.1cm 3 / g, specific surface area is 1300m 2 / g, the magnesium salt is 50g of 10wt% magnesium sulfate solution, the tin salt is 50g of 10wt% tin sulfate solution, the reaction temperature of the hydrothermal reaction is 200°C, the reaction pressure is 1Mpa, and the reaction time is 12h.
[0104] S2. The mesoporous carbon mixed solution is filtered and vacuum dried in sequence, and the filter residue is carbonized to obtain a magnesium-tin co-doped carbon matrix; wherein the drying temperature is 80°C, the drying time is 24h, the carbonization temperature is 1200°C, and the carbonization time is 1h.
[0105] S3. Transfer the magnesium-tin co-doped carbon matrix to a fluidized bed in an inert atmosphere, introduce a chlorosilane mixed gas for deposition reaction, and obtain magnesium-tin doped porous silicon carbon; wherein the chlorosilane mixed gas includes dimethylchlorosilane and argon, and the volume ratio of dimethylchlorosilane: argon is 5:1, the flow rate of the chlorosilane mixed gas is 100 sccm, the reaction temperature of the deposition reaction is 600°C, and the reaction time is 2h.
[0106] S4. Disperse the organic lithium salt and the metal conductive agent uniformly in an organic solvent to obtain solution A; wherein, according to the mass ratio, the organic lithium salt: the metal conductive agent: the organic solvent = 5:1:500. The organic lithium salt is 10g of lithium acetate, the metal conductive agent is 2g of copper nanowires, the length of the copper nanowires is 100nm, the diameter is 20µm, the organic solvent is 1000g of isopropanol solution, and the dispersion method is ultrasonic dispersion.
[0107] S5. Add magnesium tin doped porous silicon carbon into a reactor with an inert atmosphere, add solution A into the nozzle for atomization, deposit the atomized solution A on the surface of the magnesium tin doped porous silicon carbon, and then carbonize the deposited magnesium tin doped porous silicon carbon to prepare a multi-ion doped silicon carbon composite material.
[0108] The reactor is equipped with a spray nozzle, a gas sensor and a temperature sensor. According to the mass ratio, magnesium tin doped porous silicon carbon: solution A = 100:500, the spray parameters of the spray nozzle in the initial state are atomization pressure of 1Mpa, gas flow rate of 500sccm, atomization temperature of 200°C, carbonization reaction temperature of 1100°C, and reaction time of 1h. The adjustment of the spray nozzle and the reaction control in the reactor are the same as in Example 1, only adaptive changes are made, and no further description is given here.
[0109] Comparative Example 1:
[0110] The difference from Example 1 is that magnesium carbonate solution and tin oxide solution are not added in step S1, and the rest is the same as Example 1.
[0111] Comparative Example 2:
[0112] Different from Example 1, instead of using gas atomization to deposit lithium salt and metal nanowires on its surface, the porous silicon carbon is doped with magnesium tin in step 3, and oxygen (500 SCCM) is introduced at a temperature of 100° C. for 2 h to perform a passivation treatment to obtain a multi-ion doped silicon-carbon composite material.
[0113] Experiment 1: Morphology determination of multi-ion doped silicon-carbon composites.
[0114] The multi-ion-doped silicon-carbon composite materials in Examples 1-3 and Comparative Examples 1-2 were subjected to SEM testing.
[0115] Table 1, morphology comparison table of each embodiment and comparative example:
[0116]
[0117] According to Table 1, the particle sizes of Examples 1-3 and Comparative Example 2 are uniformly distributed, the surface has a porous structure, and a fibrous material is bonded to the surface. However, in Comparative Example 1, magnesium ions, tin ions, lithium ions, and metal conductive agents are not introduced, and it is difficult to form a fibrous material on the surface layer.
[0118] Figure 3 This is the SEM picture of Example 1. The multi-ion doped silicon-carbon composite material of Example 1 presents a granular structure, a porous structure on the surface, and fibrous materials are bonded on the surface, with a particle size between 5µm and 10μm.
[0119] Experiment 2: Electrical performance test.
[0120] (1) Physical and chemical properties test:
[0121] According to the method in the national standard GB / T38823-2020 "Silicon Carbon", the specific surface area and tap density of the silicon-carbon composite materials of Examples 1-3 and the multi-ion-doped silicon-carbon composite materials in Comparative Examples 1-2 were tested. The powder resistivity of the materials and the compaction density of the powder materials at 2T were tested using a four-probe tester. The gas production (45°C, 24h) test of the multi-ion-doped silicon-carbon composite materials was also carried out.
[0122] Table 2, Physical and chemical properties test results:
[0123]
[0124] It can be seen from Table 2 that the powder conductivity of the multi-ion doped silicon-carbon composite material of the present invention is significantly improved compared with the comparative example. The reason is that magnesium and tin are doped in Examples 1-3 to improve the electronic conductivity of the material, reduce impedance and reduce powder resistivity. At the same time, the atomization method deposits lithium salt and conductive agent on its surface to improve the coating integrity of the multi-ion doped silicon-carbon composite material and reduce gas production.
[0125] (2) Button battery test:
[0126] The multi-ion doped silicon-carbon composite materials of Examples 1-3 and the silicon-based composite materials of Comparative Examples 1-2 were used as active materials to prepare pole pieces. The specific preparation method was as follows: 9 g of active material, 0.5 g of conductive agent SP, and 0.5 g of binder LA133 were added to 220 mL of deionized water and stirred evenly to obtain slurry; the slurry was coated on a copper foil current collector to obtain a pole piece.
[0127] The pole piece using the multi-ion doped new silicon-carbon composite material as the active material is marked as A, the pole piece using the multi-ion doped new silicon-carbon composite material as the active material is marked as B, the pole piece using the multi-ion doped new silicon-carbon composite material as the active material is marked as C, the pole piece using the silicon-based composite material of comparative example 1 as the active material is marked as D, and the pole piece using the silicon-based composite material of comparative example 2 as the active material is marked as E.
[0128] The prepared electrode was then used as the positive electrode and assembled into a button cell with a lithium sheet, electrolyte and separator in a glove box where the oxygen and water content were both less than 0.1 ppm. The separator was celegard 2400; the electrolyte was LiPF 6 Solution, LiPF 6 The concentration is 1.1 mol / L, and the solvent is a mixed solution of ethylene carbonate (EC) and diethyl carbonate (DMC) (weight ratio is 1:1). The button batteries are marked as A-1, B-1, C-1 and D-1, E-1 respectively. Then the performance of the button batteries is tested with a blue electric tester. The test conditions are: 0.1C rate charge and discharge, voltage range of 0.05~2V, stop after 3 cycles, and then test the full charge expansion of the negative electrode and its charging DCR (50% SOC).
[0129] Table 3, button battery test results:
[0130] Serial number First discharge specific capacity (mAh / g) First efficiency (%) Full charge expansion (%) DCR(Ω) A-1 1923.5 93.1 85.8 56.8 B-1 1910.3 92.8 90.5 68.6 C-1 1998.8 93.4 82.8 49.5 D-1 1821.2 91.4 94.6 114.6 E-1 1783.4 90.2 108.5 84.8
[0131] It can be seen from the data in Table 3 that the multi-ion doped silicon-carbon composite materials of Examples 1-3 of the present invention have significantly improved first efficiency compared with Comparative Examples 1-2. The reason is that the organic lithium salts deposited by the atomization method in the example materials have high density and strong uniformity, which can restrain the expansion of the inner core silicon; at the same time, the inner core is doped with magnesium and tin to reduce the polarization of the material, improve the electronic conductivity, and improve the specific capacity of the active material, thereby improving the first discharge specific capacity and its first efficiency.
[0132] Experiment 3: Soft pack battery test.
[0133] The multi-ion doped silicon-carbon composite materials of Examples 1-3 and Comparative Examples 1-2 were mixed with 90% artificial graphite as negative electrode materials to prepare negative electrode sheets. 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 ) as the positive electrode; the electrolyte is lithium hexafluorophosphate (LiPF 6) as electrolyte, a mixture of ethylene carbonate (EC) and ethyl methyl carbonate (DEC) in a volume ratio of 1:1 as solvent, and an electrolyte concentration of 1.3 mol / L; Celgard 2400 membrane as separator, 5Ah soft-pack batteries were prepared. The prepared soft-pack batteries were marked as A-2, B-2, C-2, D-2, and E-2 respectively.
[0134] The following performance tests are performed on each soft pack battery:
[0135] (1) Expansion rate test.
[0136] The soft-pack batteries A-2 to E-2 after constant capacity were dissected to test the thickness D1 of their negative electrode plates. Then, each soft-pack battery was fully charged after cycling 100 times (1C / 1C@25±3℃@2.5-4.2V). Then, the thickness D2 of the negative electrode plates after cycling was dissected again to test the expansion rate (the expansion rate is = (D2-D1) / D1).
[0137] Table 4, expansion rate test results:
[0138]
[0139] It can be seen from Table 4 that the expansion rate of the negative electrode sheet of the soft-pack lithium-ion battery using the multi-ion-doped silicon-carbon composite material of the embodiment of the present invention is significantly lower than that of the comparative example. The reason is that the multi-ion-doped silicon-carbon composite material of the present invention has a large pore volume and low full-charge expansion, thereby reducing the full-charge expansion of its negative electrode sheet.
[0140] (2) Cycle performance and rate test.
[0141] The soft pack batteries A-2 to E-2 were subjected to cycle performance tests and rate tests. The test conditions were: charge and discharge voltage range of 2.5 to 4.2 V, temperature of 25 ± 3.0 °C, charge and discharge rate of 0.5C / 1.0C, and cycle number of 500 times. Rate test: The batteries were charged at a rate of 3C and the charging DCR impedance at different SOCs was tested (10%, 30%, 50%, 70%, 90%).
[0142] Table 5, Cycle performance and rate test data:
[0143]
[0144] It can be seen from Table 5 that the cycle performance and rate performance of the soft-pack lithium-ion battery prepared using the multi-ion doped silicon-carbon composite material of the present invention are better than those of the comparative example. The reason is that the multi-ion doped silicon-carbon composite material of the present invention has lower expansion and higher specific surface area, which improves the liquid retention of the material and improves the cycle performance; at the same time, the example material has lower powder resistivity, which improves its kinetic performance, thereby improving its constant current ratio during the charge and discharge process, that is, improving its power performance.
[0145] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a multi-ion doped silicon-carbon composite material, characterized in that: The multi-ion doped silicon-carbon composite material comprises a matrix and a surface layer, wherein the surface layer is formed on the outer surface of the matrix, the matrix is magnesium-tin doped porous silicon-carbon, and the surface layer is a metal conductive agent doped lithium salt, and the metal conductive agent doped lithium salt accounts for 1-5wt% by weight, and the rest is the magnesium-tin doped porous silicon-carbon; The method for preparing the multi-ion doped silicon-carbon composite material comprises the following steps: S1, adding mesoporous carbon to a mixed solution of magnesium salt and tin salt to disperse evenly, and transferring to a high-pressure reactor for hydrothermal reaction to obtain a mesoporous carbon mixed solution; Wherein, according to the mass ratio, the mesoporous carbon: the magnesium salt: the tin salt = 50:1-5:1-5, the reaction temperature of the hydrothermal reaction is 100-200° C., the reaction pressure is 1-5 MPa, and the reaction time is 12-48 h; S2, filtering and vacuum drying the mesoporous carbon mixed solution in sequence, and carbonizing the filter residue to obtain a magnesium-tin co-doped carbon matrix; Among them, the drying temperature is 80°C, the drying time is 24h, the carbonization temperature is 800~1200°C, and the carbonization time is 1~6h; S3, transferring the magnesium-tin co-doped carbon matrix into a fluidized bed in an inert atmosphere, introducing a chlorosilane mixed gas to perform a deposition reaction, and obtaining magnesium-tin doped porous silicon carbon; The chlorosilane mixed gas includes chlorosilane and argon, and the volume ratio of the chlorosilane: the argon is 1-5:
1. The flow rate of the chlorosilane mixed gas is 100-1000 sccm. The reaction temperature of the deposition reaction is 400-600° C., and the reaction time is 0.5-2 h. S4, uniformly dispersing the organic lithium salt and the metal conductive agent in an organic solvent to obtain a solution A; Wherein, according to the mass ratio, the organic lithium salt: the metal conductive agent: the organic solvent = 1-10: 0.5-2: 500-1000; S5, adding the magnesium tin doped porous silicon carbon into a reactor in an inert atmosphere, adding the solution A into a spray nozzle for atomization, depositing the atomized solution A on the surface of the magnesium tin doped porous silicon carbon, and then carbonizing the deposited magnesium tin doped porous silicon carbon to prepare the multi-ion doped silicon carbon composite material; The reactor is equipped with a spray nozzle, a gas controller and a temperature controller. According to the mass ratio, the magnesium tin doped porous silicon carbon: the solution A=100:100~500, the atomization pressure of the spray nozzle is 0.1~1Mpa, the atomization temperature is 100~200°C, the gas flow rate is 100~500sccm, the reaction temperature of the carbonization reaction is 800~1100°C, and the reaction time is 1~6h.
2. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: In step S5, the step of adding the solution A to the spray nozzle for atomization includes: Setting the injection parameters of the injection nozzle, wherein the injection parameters of the injection nozzle include injection diameter, injection pressure and gas flow rate; Obtain the particle size distribution data of the solution A and substitute the particle size distribution data into the fitting curve equation to obtain a fitting result, wherein the fitting curve equation is , is the mass fraction of particles with a diameter smaller than d, is the median particle size, n is the distribution parameter, and the larger the distribution parameter, the smaller the particle size distribution range of the solution A; The injection parameters of the injection nozzle are adjusted according to the fitting result until the median particle size and the fraction parameter are both within a preset range.
3. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: The step of depositing the atomized solution A on the surface of the magnesium-tin-doped porous silicon carbon comprises: Set target temperature and target gas flow rate; Acquire the actual temperature and the actual gas flow rate and calculate the errors with the target temperature and the target gas flow rate respectively; The adjustment value of the gas controller and the adjustment value of the temperature controller are calculated respectively, and the gas controller and the temperature controller are correspondingly adjusted according to the adjustment values until the target temperature and the target gas flow rate are reached.
4. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 3, characterized in that: The calculation formula of the adjustment value of the temperature controller is: , is the adjustment value of the temperature controller, t is the time, is the first temperature influencing factor, is the second temperature influencing factor, is the third temperature influencing factor, is the error between the actual temperature and the target temperature, The calculation formula of the adjustment value of the gas controller is: , is the adjustment value of the gas controller, is the first gas flow rate influencing factor, is the second gas flow rate influencing factor, is the third gas flow rate influencing factor, is the error between the actual gas flow rate and the target gas flow rate.
5. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: In step S1, the magnesium salt includes at least one of magnesium chloride, magnesium sulfate, magnesium carbonate, and magnesium nitrate, with a concentration of 1 to 10 wt %; the tin salt includes at least one of tin chloride, tin tetrachloride, tin sulfate, tin sulfide, and tin oxide, with a concentration of 1 to 10 wt %; the pore volume of the mesoporous carbon is 0.9 to 1.1 cm 3 / g, specific surface area 1000~1500m 2 / g.
6. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: In the step S3, the chlorosilane includes at least one of trichlorosilane, tetrachlorosilane, dimethylchlorosilane, propenyltrichlorosilane, pentyltrichlorosilane, methylvinyldichlorosilane, triisopropylchlorosilane, propyltrichlorosilane and 2-methylbutyltrichlorosilane.
7. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: In the step S4, the organic lithium salt includes at least one of lithium pyruvate, lithium stearate, lithium acetate, lithium difluoroborate, lithium 4-methylbenzenesulfonate, and lithium benzoate; the metal conductive agent includes at least one of copper nanowires, silver nanowires, copper nanowires, and tin oxide nanowires; the length of the metal conductive agent is 50-200 nm and the diameter is 10-30 µm; the organic solvent includes at least one of methanol, ethanol, butanediol, isopropanol, and benzyl alcohol.
8. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: The components in the magnesium-tin-doped porous silicon carbon include magnesium ions, tin ions, porous carbon and nano-silicon, wherein, calculated by mass percentage, the magnesium ions account for 0.5~2wt%, the tin ions account for 0.5~2wt%, the porous carbon accounts for 42~49wt%, and the remainder is the nano-silicon.
9. The method for preparing the multi-ion doped silicon-carbon composite material according to claim 1, characterized in that: The components in the metal conductive agent-doped lithium salt include a metal conductive agent, a lithium salt compound and amorphous carbon, wherein, calculated by weight percentage, the metal conductive agent accounts for 5-15%, the lithium salt compound accounts for 50-80%, and the remainder is the amorphous carbon.