Ceramic diaphragm for lithium ion battery and preparation method thereof
By modifying the combination of nano alumina and carbon nanotubes, the porosity and conductivity of the lithium-ion battery separator are improved, and the problems of insufficient electrolyte affinity and thermal stability of the existing separator are solved, thus achieving higher batteries Performance and security.
Patent Information
- Application Number
- CN202410728589.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-06
AI Technical Summary
The existing lithium-ion battery separators have problems such as weak electrolyte affinity, low porosity, poor wetting and poor thermal stability, which leads to low battery energy density, poor circulation performance and safety hazards, which hinders lithium-ion batteries in the new generation of electric vehicles. Application in.
By modifying the combination of nano alumina and carbon nanotubes, nano alumina is functionalized using gamma-glycidyl etheroxypropyl trimethoxysilane, and carboxylated carbon nanotubes are obtained by sonication and oxidation treatment to form ceramics Coating improves the porosity and conductivity of ceramic diaphragms, enhances the wettability of the electrolyte and the transmission capacity of lithium ions.
It improves the conductivity, tensile strength and thermal stability of the ceramic separator, increases the diffusion speed of lithium ions, extends the service life of the battery, reduces the loss of lithium salt, and improves the safety and performance of the battery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion battery diaphragms, and in particular relates to a ceramic diaphragm for lithium ion batteries and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high specific energy, long cycle life, and no memory effect, and are widely used in many fields such as new energy vehicles, aerospace, and military industry. As an important component of lithium-ion batteries, the diaphragm plays an electronic insulation role between the positive and negative electrodes, while ensuring the free movement of ions. Although the diaphragm does not directly participate in the electrochemical reaction of the battery, its structure and performance play an important role in the battery cycle life, safety, energy density, and power density.
[0003] At present, polyolefin separators include polyethylene separators and polypropylene separators. Due to their low price, good mechanical strength, good chemical and electrochemical stability, they have become the most widely used separator products in lithium battery companies. However, polyolefin separators have problems such as weak electrolyte affinity, low porosity, poor wettability, and poor thermal stability, which lead to problems such as low energy density and poor cycle performance during battery use. In addition, polyolefin separators themselves have poor thermal stability. The melting points of polypropylene and polyethylene are 165°C and 135°C, respectively. Abnormally high battery temperature will cause the separator to shrink and melt, causing serious safety hazards in the use of lithium-ion batteries, which seriously hinders the application of lithium-ion batteries in the new generation of electric vehicles.
[0004] The existing technology improves the thermal stability of the separator by incorporating inorganic materials into organic films to obtain composite separators and using organic or inorganic films with high thermal stability. Among them, coating a layer of inorganic ceramic particles on the surface of polyethylene separators or polypropylene separators is considered to be the most effective and economical method. The ceramic material provides high heat resistance, while the adhesive provides adhesion to maintain the structural integrity of the coating and the entire composite separator. On the one hand, due to the improved thermal stability, the ceramic coated separator can effectively improve the safety of lithium-ion batteries by preventing short circuits at high temperatures; on the other hand, the ceramic coated separator has good infiltration and liquid absorption and retention capabilities with electrolytes and positive and negative electrode materials, which greatly improves the performance and service life of the battery.
[0005] Among them, nano-alumina is an inorganic ceramic particle commonly used as a coating material for lithium-ion battery separators. It has high thermal stability and chemical inertness, and has excellent high temperature resistance, which can greatly improve the safety of lithium-ion batteries. In addition, it can neutralize free HF in the electrolyte and increase the service life of the battery. However, the surface of nano-alumina has a high Gibbs free energy, and the hydroxyl groups adsorbed on the surface can easily form hydrogen bonds, causing the nano-alumina to agglomerate into large particles and uneven distribution in the ceramic coating slurry. In addition, the dense nano-alumina coating on the surface of the ceramic separator can improve the wettability of the electrolyte, but the dense nano-alumina coating and the insulation of nano-alumina will affect the transmission of lithium ions. Summary of the invention
[0006] In order to solve the deficiencies mentioned in the above-mentioned background technology, the purpose of the present invention is to provide a ceramic diaphragm for lithium-ion batteries and a preparation method thereof. By adding modified nano-alumina, the self-aggregation of carbon nanotubes and nano-alumina is avoided, the porosity of the ceramic diaphragm is improved, which is beneficial to the transmission of lithium ions and the storage and retention of electrolyte in the ceramic diaphragm, so that the wettability of the diaphragm electrolyte is improved. At the same time, carbon nanotubes provide abundant paths for the transmission of lithium ions, so that the obtained ceramic diaphragm has good electrical conductivity.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A ceramic diaphragm for lithium-ion batteries comprises a base film and a ceramic coating, wherein the ceramic coating is arranged on at least one side surface of the base film, and the ceramic coating comprises the following raw materials in parts by weight: 10 to 45 parts of modified nano-alumina, 5 to 25 parts of a binder, and 0.5 to 5 parts of a dispersant; the modified nano-alumina is γ-glycidyloxypropyltrimethoxysilane functionalized nano-alumina grafted with carboxylated carbon nanotubes.
[0009] Preferably, the binder is one or more combinations of polyvinyl alcohol, polyvinylidene fluoride, polyacrylate, styrene-butadiene latex, and polyimide; the dispersant is one or more combinations of sodium carboxymethyl cellulose, triethyl phosphate, polyacrylic acid, sodium polyacrylate, polyethylene glycol, and hydroxyethyl cellulose.
[0010] Preferably, the base film is one of a polypropylene base film, a polyethylene base film, and a polypropylene / polyethylene / polypropylene composite film, and the thickness of the base film is 5-25 µm.
[0011] Preferably, the thickness of the ceramic coating is 2-4 μm.
[0012] Preferably, the preparation method of the modified nano-alumina comprises the following steps:
[0013] A. Take anhydrous ethanol and add 10wt% citric acid solution, adjust the pH to 3-4, add γ-glycidyloxypropyltrimethoxysilane and stir for 3-5 minutes, then let it stand for 0.5-1 hour and then add nano-alumina, stir at 75-90℃ for 1-5 hours, cool to room temperature, filter, wash, dry and grind to obtain coupling agent modified nano-alumina;
[0014] B. Place multi-walled carbon nanotubes in a mixture of concentrated sulfuric acid and concentrated nitric acid at a volume ratio of 3:1, ultrasonically shake at room temperature for 20-30 min, stir in an oil bath at 75-90°C for 4-6 h, filter and wash the product until it is neutral, and vacuum dry to obtain carboxylated carbon nanotubes;
[0015] C. Take coupling agent modified nano-alumina and carboxylated carbon nanotubes, add N,N-dimethylformamide and perform ultrasonic treatment, then add triethylamine, place in an oil bath at 110-125°C and stir with nitrogen for 6-8 hours, wait for the reaction liquid to cool to room temperature, perform reduced pressure distillation, wash, filter and dry to obtain modified nano-alumina.
[0016] Preferably, in step A, the addition ratio of anhydrous ethanol, γ-glycidyloxypropyltrimethoxysilane and nano-alumina is 25 mL: 0.4-1.2 mL: 1-2 g.
[0017] Preferably, in step C, the mass ratio of the coupling agent-modified nano-alumina to the carboxylated carbon nanotubes is 1:0.5-0.8 g.
[0018] The method for preparing the ceramic diaphragm for lithium ion battery as described above comprises the following steps:
[0019] (1) Weighing the raw materials according to weight, dissolving the binder in N-methylpyrrolidone, adding the modified nano-alumina and the dispersant, mixing and dispersing the mixture in a ball mill, and obtaining a ceramic coating slurry;
[0020] (2) The ceramic coating slurry is coated on one surface of the base film, dried and rolled up to obtain a ceramic separator for lithium-ion batteries.
[0021] Beneficial effects of the present invention:
[0022] The invention uses γ-glycidyloxypropyltrimethoxysilane to modify nano-alumina. The hydroxyl group at one end of the γ-glycidyloxypropyltrimethoxysilane undergoes a condensation reaction with the hydroxyl group on the surface of the nano-alumina, thereby reducing the surface activity of the nano-alumina, avoiding the agglomeration of the nano-alumina, improving the uniformity of the nano-alumina in the ceramic coating slurry, and further improving the electrical conductivity, tensile strength and thermal stability of the ceramic diaphragm. At the same time, the invention uses concentrated nitric acid and concentrated sulfuric acid to oxidize multi-walled carbon nanotubes to obtain carboxylated carbon nanotubes. The epoxy group at the other end of the γ-glycidyloxypropyltrimethoxysilane undergoes a ring-opening reaction with the carboxyl group on the surface of the carboxylated carbon nanotubes. The carbon nanotubes are grafted onto the surface of the nano-alumina through the bridging effect of the γ-glycidyloxypropyltrimethoxysilane. The carbon nanotubes are hollow cylinders composed of pure carbon and have the characteristics of excellent electrical properties, excellent mechanical strength, high stability and high active surface area. In the ceramic coating, the carbon nanotubes are preferably used as the carbon nanotubes. Carbon nanotubes with good affinity and conductivity for electrolyte are added to the layer. Carbon nanotubes can store and disperse lithium ions during battery operation, prevent the generation of lithium dendrites, and reduce the loss of lithium salts. The storage capacity of lithium ions in carbon nanotubes comes from the effective diffusion of lithium ions through the ports or sidewall openings of carbon nanotubes and the carbon nanotube layer to the surface of carbon nanotubes and the stable position inside a single carbon nanotube. The storage of lithium ions in carbon nanotubes increases the diffusion rate of lithium ions. The base film is coated with modified nano-alumina. The grafting of carbon nanotubes and nano-alumina can avoid the self-aggregation of carbon nanotubes and nano-alumina. At the same time, the network structure formed by a large number of carbon nanotubes can increase the gap between nano-alumina particles, increase the porosity of the ceramic diaphragm, facilitate the transmission of lithium ions and the storage and retention of electrolyte in the ceramic diaphragm, so that the wettability of the diaphragm electrolyte is improved. At the same time, carbon nanotubes provide abundant paths for the transmission of lithium ions, so that the obtained ceramic diaphragm has good conductivity. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1 A method for preparing modified nano-alumina comprises the following steps:
[0025] A. Take 25 mL of anhydrous ethanol and add 10 wt% citric acid solution to adjust the pH to 3, add 0.4 mL of γ-glycidyloxypropyltrimethoxysilane and stir for 3 min, then let stand for 0.5 h and add 1 g of nano-alumina, stir at 75 ° C for 1 h, cool to room temperature, filter, wash, dry and grind to obtain coupling agent modified nano-alumina;
[0026] B. Take 3g of multi-walled carbon nanotubes and place them in 120mL of a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, ultrasonically shake at room temperature for 20 min, stir and react in a 75℃ oil bath for 5 h, filter and wash the product until it is neutral, and vacuum dry to prepare carboxylated carbon nanotubes;
[0027] C. Take 1g of coupling agent-modified nano-alumina and 0.5g of carboxylated carbon nanotubes, add 50mL of N,N-dimethylformamide and perform ultrasonic treatment, then add 2mL of triethylamine, place in a 110°C oil bath and stir with nitrogen for 6h, wait for the reaction liquid to cool to room temperature, perform reduced pressure distillation, wash, filter and dry to obtain modified nano-alumina.
[0028] Example 2 A method for preparing modified nano-alumina comprises the following steps:
[0029] A. Take 25 mL of anhydrous ethanol and add 10 wt% citric acid solution to adjust the pH to 4, add 0.8 mL of γ-glycidyloxypropyltrimethoxysilane and stir for 5 min, then let stand for 1 h and add 1.6 g of nano-alumina, stir at 85 ° C for 4 h, cool to room temperature, filter, wash, dry and grind to obtain coupling agent modified nano-alumina;
[0030] B. 3 g of multi-walled carbon nanotubes were placed in 118 mL of a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, and ultrasonically shaken at room temperature for 25 min. The mixture was stirred in an oil bath at 80 °C for 6 h. The product was filtered and washed until neutral, and then vacuum dried to obtain carboxylated carbon nanotubes.
[0031] C. Take 1g of coupling agent-modified nano-alumina and 0.7g of carboxylated carbon nanotubes, add 50mL of N,N-dimethylformamide and perform ultrasonic treatment, then add 2mL of triethylamine, place in a 120°C oil bath and stir with nitrogen for 7h, wait for the reaction liquid to cool to room temperature, perform reduced pressure distillation, wash, filter and dry to obtain modified nano-alumina.
[0032] Example 3 A method for preparing modified nano-alumina comprises the following steps:
[0033] A. Take 25 mL of anhydrous ethanol and add 10 wt% citric acid solution to adjust the pH to 4, add 1.2 mL of γ-glycidyloxypropyltrimethoxysilane and stir for 5 minutes, then let it stand for 1 hour and add 2 g of nano-alumina, stir at 90 ° C for 5 hours, cool to room temperature, filter, wash, dry and grind to obtain coupling agent modified nano-alumina;
[0034] B. 3 g of multi-walled carbon nanotubes were placed in 120 mL of a mixture of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, and ultrasonically shaken at room temperature for 30 min. The mixture was stirred in an oil bath at 90 °C for 4 h. The product was filtered and washed until neutral, and then vacuum dried to obtain carboxylated carbon nanotubes.
[0035] C. Take 1g of coupling agent-modified nano-alumina and 0.8g of carboxylated carbon nanotubes, add 60mL of N,N-dimethylformamide and perform ultrasonic treatment, then add 2mL of triethylamine, place in a 125°C oil bath and stir with nitrogen for 8h, wait for the reaction liquid to cool to room temperature, perform reduced pressure distillation, wash, filter and dry to obtain modified nano-alumina.
[0036] Example 4 A ceramic separator for lithium-ion batteries includes a polyethylene-based film and a ceramic coating, wherein the ceramic coating includes the following raw materials in parts by weight: 10 parts of modified nano-alumina, 5 parts of a binder, polyvinylidene fluoride, and 1 part of a dispersant, sodium carboxymethyl cellulose.
[0037] The preparation method of the ceramic diaphragm comprises the following steps:
[0038] (1) Weighing the raw materials according to weight, dissolving the binder in N-methylpyrrolidone, adding the modified nano-alumina and the dispersant, mixing and dispersing the mixture in a ball mill, and obtaining a ceramic coating slurry;
[0039] (2) The ceramic coating slurry is coated on one surface of the base film, dried and rolled up to obtain a ceramic separator for lithium-ion batteries.
[0040] Example 5 A ceramic separator for lithium-ion batteries includes a polypropylene base film and a ceramic coating. The ceramic coating includes the following raw materials in parts by weight: 25 parts of modified nano-alumina, 12 parts of a binder polyacrylate, and 2 parts of a dispersant polyacrylic acid.
[0041] The preparation method of the above ceramic diaphragm is the same as that of Example 4.
[0042] Example 6 A ceramic separator for lithium-ion batteries includes a polyethylene-based film and a ceramic coating, wherein the ceramic coating includes the following raw materials in parts by weight: 45 parts of modified nano-alumina, 25 parts of a binder polyvinyl alcohol, and 5 parts of a dispersant polyethylene glycol.
[0043] The preparation method of the above ceramic diaphragm is the same as that of Example 4.
[0044] Comparative Example 1 A ceramic separator for lithium-ion batteries includes a polyethylene-based film and a ceramic coating, wherein the ceramic coating includes the following raw materials in parts by weight: 20 parts of nano-alumina, 10 parts of multi-walled carbon nanotubes, 20 parts of a binder polyvinyl alcohol, and 3 parts of a dispersant polyethylene glycol.
[0045] The preparation method of the above ceramic diaphragm is the same as that of Example 4.
[0046] Comparative Example 2 A ceramic separator for lithium-ion batteries includes a polyethylene-based film and a ceramic coating, wherein the ceramic coating includes the following raw materials in parts by weight: 30 parts of coupling agent-modified nano-alumina, 18 parts of binder polyvinyl alcohol, and 0.5 parts of dispersant polyethylene glycol.
[0047] The preparation method of the above ceramic diaphragm is the same as that of Example 4.
[0048] Performance Testing
[0049] The ceramic diaphragms prepared in Examples 4-6 and Comparative Examples 1-2 were subjected to performance testing:
[0050] (1) Porosity and liquid absorption test: The diaphragm was cut into a size of 2 × 2 cm and its mass was measured as Wdry. The diaphragm was then immersed in a sealed container filled with n-butanol for 2 h. The sample was taken out and its mass was measured as Wwet. The porosity was calculated according to the formula: Porosity = (Wdry − Wwet) / ρV × 100; the liquid absorption was calculated according to the formula: Liquid absorption = (Wdry − Wwet) / Wdry × 100, where Wdry represents the mass of the diaphragm before absorbing the electrolyte, Wwet represents the mass of the diaphragm after absorbing the electrolyte, ρ is the density of n-butanol, and V is the volume of the diaphragm. The data results are shown in Table 1.
[0051] (2) Thermal shrinkage test: The diaphragm sample was cut into a size of 2×2 cm and heated in an electric constant temperature vacuum drying oven at 150°C for 30 min. The dimensional change of the diaphragm was observed and the data results were shown in Table 1.
[0052] (3) Tensile strength test: The diaphragm samples were cut into a size of 45 × 5 mm and stretched at a rate of 5 mm / min. Each sample was grouped into 5 pieces and the average value was taken as the final result. The data results are shown in Table 1.
[0053] (4) Ionic conductivity test: The diaphragm was cut into discs with a diameter of 1.96 cm. The cut diaphragm was fully soaked in the electrolyte in a glove box filled with argon gas, and then placed between two stainless steel electrodes and encapsulated in a CR2032 button battery shell. The conductivity was tested using a Chenhua CH I660E electrochemical workstation at room temperature using a frequency range of 10 mHz-1 MHz. The ionic conductivity was calculated according to the formula: σ=d / (RS), where σ is the ionic conductivity, d is the thickness of the diaphragm, R is the bulk resistance of the diaphragm, and S is the effective contact area of the diaphragm. The data results are shown in Table 1.
[0054] Table 1 Test results of membrane sample performance
[0055]
[0056] From the data in Table 1, it can be seen that the ceramic diaphragms prepared in Examples 4-6 of the present invention have high porosity and electrolyte absorption rate, excellent electrolyte wettability, low thermal shrinkage, good thermal stability, and good tensile strength and ionic conductivity. In Comparative Example 1, γ-glycidyloxypropyltrimethoxysilane was not added to graft nanoalumina and carbon nanotubes, and its various properties were slightly worse than those of Examples 4-6, which may be due to the self-aggregation phenomenon of nanoalumina and carbon nanotubes, resulting in reduced diaphragm performance. In Comparative Example 2, carbon nanotubes were not added, and its various properties were significantly reduced, indicating that the addition of carbon nanotubes can improve the porosity, electrolyte wettability, thermal stability, mechanical properties and ionic conductivity of the diaphragm to a certain extent.
[0057] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A ceramic diaphragm for a lithium-ion battery, comprising a base film and a ceramic coating, characterized in that: The ceramic coating is arranged on at least one side of the base film, and the ceramic coating comprises the following raw materials in parts by weight: 10-45 parts of modified nano-alumina, 5-25 parts of a binder, and 0.5-5 parts of a dispersant; the modified nano-alumina is γ-glycidyloxypropyltrimethoxysilane functionalized nano-alumina grafted with carboxylated carbon nanotubes; The preparation method of the modified nano-alumina comprises the following steps: A. Take anhydrous ethanol and add 10wt% citric acid solution, adjust the pH to 3-4, add γ-glycidyloxypropyltrimethoxysilane and stir for 3-5 minutes, then let it stand for 0.5-1 hour and then add nano-alumina, stir at 75-90℃ for 1-5 hours, cool to room temperature, filter, wash, dry and grind to obtain coupling agent modified nano-alumina; B. Place multi-walled carbon nanotubes in a mixture of concentrated sulfuric acid and concentrated nitric acid at a volume ratio of 3:1, perform ultrasonic oscillation at room temperature for 20-30 minutes, stir in an oil bath at 75-90°C for 4-6 hours, filter and wash the product until it is neutral, and vacuum dry to obtain carboxylated carbon nanotubes; C. Take coupling agent-modified nano-alumina and carboxylated carbon nanotubes, add N,N-dimethylformamide and perform ultrasonic treatment, then add triethylamine, place in an oil bath at 110-125°C and stir with nitrogen for 6-8h, use the epoxy group at the other end of γ-glycidyloxypropyltrimethoxysilane and the carboxyl group on the surface of the carboxylated carbon nanotube to undergo a ring-opening reaction, and graft the carbon nanotubes onto the surface of the nano-alumina through the bridging effect of γ-glycidyloxypropyltrimethoxysilane. After the reaction solution is cooled to room temperature, it is distilled under reduced pressure, washed, filtered and dried to obtain modified nano-alumina.
2. The ceramic separator for lithium ion battery according to claim 1, characterized in that: The binder is one or more combinations of polyvinyl alcohol, polyvinylidene fluoride, polyacrylate, styrene-butadiene latex, and polyimide; the dispersant is one or more combinations of sodium carboxymethyl cellulose, triethyl phosphate, polyacrylic acid, sodium polyacrylate, polyethylene glycol, and hydroxyethyl cellulose.
3. The ceramic separator for lithium ion battery according to claim 1, characterized in that: The base film is one of a polypropylene base film, a polyethylene base film, and a polypropylene / polyethylene / polypropylene composite film, and the thickness of the base film is 5-25 μm.
4. The ceramic separator for lithium ion battery according to claim 1, characterized in that: The thickness of the ceramic coating is 2-4 μm.
5. The ceramic separator for lithium ion battery according to claim 1, characterized in that: In the step A, the addition ratio of anhydrous ethanol, γ-glycidyloxypropyltrimethoxysilane and nano-alumina is 25 mL: 0.4-1.2 mL: 1-2 g.
6. The ceramic separator for lithium ion battery according to claim 1, characterized in that: In the step C, the mass ratio of the coupling agent modified nano-alumina to the carboxylated carbon nanotubes is 1:0.5-0.8g.
7. A method for preparing a ceramic diaphragm for a lithium ion battery according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Weighing the raw materials according to weight, dissolving the binder in N-methylpyrrolidone, adding the modified nano-alumina and the dispersant, mixing and dispersing the mixture in a ball mill, and obtaining a ceramic coating slurry; (2) The ceramic coating slurry is coated on one surface of the base film, dried and rolled up to obtain a ceramic separator for lithium-ion batteries.