Corrosion-resistant material for refrigerator liner and preparation method of corrosion-resistant material
By using high-impact polystyrene and polyethylene combined with modified calcium carbonate and other components in the refrigerator inner liner material, the problem of poor corrosion resistance of the refrigerator inner liner material is solved, and the material is improved Corrosion resistance and mechanical properties extend service life and reduce production costs.
Patent Information
- Application Number
- CN202411093555.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
AI Technical Summary
The existing refrigerator inner liner material has poor performance in resisting foaming liquid corrosion, which leads to the inner liner being prone to cracking and affecting the service life.
High impact polystyrene and polyethylene are used as base materials, combined with modified calcium carbonate, compatible agent, lubricant and antioxidant, and corrosion-resistant materials are prepared by double screw extrusion granulation. Modified calcium carbonate is dispersed by ultrasonic and surface modification improve dispersion and compatibility, enhancing material properties.
The prepared corrosion-resistant materials have good corrosion resistance, low temperature resistance, excellent mechanical properties, improved crack resistance, extended service life, simple production and low cost, and are suitable for large-capacity refrigerator applications.
Smart Images

Figure BDA0004987233920000081 
Figure BDA0004987233920000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of refrigerator liner materials, and in particular relates to a refrigerator liner anti-corrosion material and a preparation method thereof. Background Art
[0002] With the gradual saturation of the home appliance market, the demand for refrigerators mainly comes from replacement and upgrading of products. The overall high-end development is the general trend of the refrigerator market. Large-capacity refrigerators are one of the products favored by customers, and large-capacity refrigerators put forward higher requirements on various technical indicators of the product.
[0003] At present, in the refrigerator industry, the refrigerator box liner and door liner are mainly made of ABS or HIPS. Among them, ABS is superior to HIPS in comprehensive mechanical properties, glossiness, oil resistance and corrosion resistance, but because of its high cost and lower food safety than HIPS, ABS is gradually replaced by HIPS. However, when using HIPS to manufacture refrigerator liner, there are still drawbacks that plague the entire refrigerator industry, that is, limited by the environmental stress cracking resistance of HIPS itself, its liner performs poorly in oil resistance and foaming liquid corrosion resistance, which increases the quality risk of cracking of the refrigerator liner before and after use.
[0004] Therefore, how to develop a corrosion-resistant material for refrigerator liner has become a technical problem that needs to be solved urgently. Summary of the invention
[0005] The present invention aims to provide a refrigerator liner anti-corrosion material and a preparation method thereof, so as to solve the problem that the materials used to prepare refrigerator liner in the prior art have poor performance in resistance to foaming liquid corrosion.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] The first aspect of the present invention provides a refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0008] High impact polystyrene 40-55 parts, polyethylene 30-50 parts, modified calcium carbonate 10-15 parts, compatibilizer 6-10 parts, lubricant 0.1-3 parts, antioxidant 0.05-1 parts;
[0009] The modified calcium carbonate is prepared by the following steps:
[0010] Calcium carbonate and ammonia water are added to anhydrous ethanol, ultrasonically dispersed, tetraethyl silicate and 1H,1H,2H,2H-perfluorooctyltriethoxysilane are added, stirring is continued, centrifugal filtration is performed, washing is performed, drying is performed to constant weight, and grinding is performed to obtain modified calcium carbonate.
[0011] As a preferred embodiment of the present invention, the usage ratio of calcium carbonate, ammonia water, anhydrous ethanol, tetraethyl silicate and 1H,1H,2H,2H-perfluorooctyltriethoxysilane is 0.50-0.55 g:10 mL:40 mL:4-5 mL:0.5-0.6 mL.
[0012] As a preferred embodiment of the present invention, the particles are ground to a particle size of 200-350 nm.
[0013] As a preferred embodiment of the present invention, the compatibilizer is one of maleic anhydride grafted ethylene-vinyl acetate copolymer and maleic anhydride grafted styrene-butadiene block copolymer.
[0014] As a preferred embodiment of the present invention, the lubricant is at least one of stearic acid, butyl stearate, oleamide, polyethylene wax and sodium stearate.
[0015] As a preferred embodiment of the present invention, the antioxidant is at least one of antioxidant 1010, antioxidant 1076, antioxidant 1035, antioxidant 168 and antioxidant 264.
[0016] A second aspect of the present invention provides a method for preparing a corrosion-resistant material for a refrigerator liner, comprising the following steps:
[0017] S1. Weigh high-impact polystyrene, polyethylene, modified calcium carbonate, a compatibilizer, a lubricant and an antioxidant in parts by weight, add them into a mixer and mix them evenly to obtain a mixture;
[0018] S2. The mixed material obtained in step S1 is fed into a twin-screw extruder. The mixed material is fully fused under the shearing, mixing and conveying of the screw, and then extruded, cooled and granulated to obtain a corrosion-resistant material.
[0019] As a preferred embodiment of the present invention, the temperature of zone 1 in the twin-screw extruder is 190-200°C, the temperature of zone 2 is 205-215°C, the temperature of zone 3 is 210-220°C, the temperature of zone 4 is 225-235°C, the temperature of zone 5 is 230-240°C, and the head temperature is 235-245°C.
[0020] As a preferred embodiment of the present invention, the rotation speed of the twin-screw extruder is 200-350 r / min.
[0021] Beneficial effects of the present invention:
[0022] 1. The anti-corrosion material for refrigerator liner provided by the present invention selects high-impact polystyrene (HIPS) and polyethylene (PE) as base materials, and then mixes them with modified calcium carbonate, a compatibilizer, a lubricant and an oxidant according to an appropriate ratio, and finally prepares it by extrusion granulation. The obtained anti-corrosion material has the characteristics of corrosion resistance and low temperature resistance, and at the same time has excellent mechanical properties and high melt strength. The use of the anti-corrosion material in the present invention to prepare a refrigerator liner has a good anti-corrosion effect, and the obtained refrigerator liner is sturdy and durable, not easy to crack, and has a long service life.
[0023] 2. In the present invention, HIPS and PE are selected as base materials. The PE / PS alloy material obtained after blending under the action of a compatibilizer has excellent barrier properties and has better anti-foaming corrosion ability than conventional HIPS materials.
[0024] 3. The modified calcium carbonate in the present invention is surface-coated with fluorine-containing long chains and tetraethyl silicate. Low surface energy modification reduces the surface activity of calcium carbonate, prevents particle agglomeration, and improves the dispersibility and compatibility of calcium carbonate, so that calcium carbonate as a reinforcing and toughening filler can be evenly dispersed in the base material, further improving the mechanical properties and impact strength of the composite material. At the same time, after the organic fluorine-modified calcium carbonate is mixed with the base material, a rough structure is formed on the surface of the composite material, showing a large contact angle, improving the oil and water resistance of the composite material, and then improving the antibacterial and antifouling properties of the composite material. In addition, the addition of calcium carbonate increases the crystallinity of PE, refines the grains, and improves the crystal density, further improving the barrier properties of PE and further enhancing the corrosion resistance of the composite material.
[0025] 4. The preparation method provided by the present invention is simple, easy to operate, has high production efficiency, low production cost, and is convenient for large-scale production. The obtained corrosion-resistant material has excellent comprehensive properties and can be widely used in the application field of refrigerator liners. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] This embodiment provides a modified calcium carbonate, and the preparation steps are as follows:
[0029] Add 0.50 g of calcium carbonate and 10 mL of ammonia water to 40 mL of anhydrous ethanol, ultrasonically disperse for 0.5 h, add 4.5 mL of tetraethyl silicate and 0.5 mL of 1H,1H,2H,2H-perfluorooctyltriethoxysilane, continue stirring for 4 h, place in a 50°C oven to dry to constant weight, centrifuge, wash, and grind to a particle size of 250 nm to obtain modified calcium carbonate.
[0030] Example 2
[0031] This embodiment provides a modified calcium carbonate, and the preparation steps are as follows:
[0032] Add 0.5 g of calcium carbonate and 10 mL of ammonia water to 40 mL of anhydrous ethanol, ultrasonically disperse for 0.5 h, add 4.5 mL of tetraethyl silicate and 0.55 mL of 1H,1H,2H,2H-perfluorooctyltriethoxysilane, continue stirring for 5 h, centrifuge and filter, wash, place in an oven at 50 ° C to dry to constant weight, grind to a particle size of 250 nm, and obtain modified calcium carbonate.
[0033] Example 3
[0034] This embodiment provides a modified calcium carbonate, and the preparation steps are as follows:
[0035] Add 0.55 g of calcium carbonate and 10 mL of ammonia water to 40 mL of anhydrous ethanol, ultrasonically disperse for 0.5 h, add 5 mL of tetraethyl silicate and 0.6 mL of 1H,1H,2H,2H-perfluorooctyltriethoxysilane, continue stirring for 4 h, centrifuge and filter, wash, place in an oven at 50 ° C to dry to constant weight, grind to a particle size of 300 nm, and obtain modified calcium carbonate.
[0036] Comparative Example 1
[0037] This comparative example provides a modified calcium carbonate, and the preparation steps are as follows:
[0038] 0.50 g of calcium carbonate and 10 mL of ammonia water were added to 40 mL of anhydrous ethanol, and ultrasonically dispersed for 0.5 h. Stirring was continued for 4 h. The mixture was centrifugally filtered, washed, dried in an oven at 50° C. to constant weight, and ground to a particle size of 250 nm to obtain modified calcium carbonate.
[0039] Example 4
[0040] This embodiment provides a refrigerator liner anti-corrosion material, including the following raw materials in parts by weight:
[0041] 40 parts of high impact polystyrene, 30 parts of polyethylene, 10 parts of modified calcium carbonate in Example 1, 6 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.5 parts of stearic acid, 0.1 parts of antioxidant 1010;
[0042] The preparation steps are as follows:
[0043] S1. Weigh high-impact polystyrene, polyethylene, the modified calcium carbonate in Example 1, maleic anhydride grafted ethylene-vinyl acetate copolymer, stearic acid and antioxidant 1010 in parts by weight and add them into a mixer and mix them evenly to obtain a mixture;
[0044] S2. Feed the mixed material obtained in step S1 into a twin-screw extruder, and the mixed material is fully fused under the shearing, mixing and conveying of the screw, wherein the temperature of zone 1 in the twin-screw extruder is 190°C, the temperature of zone 2 is 205°C, the temperature of zone 3 is 210°C, the temperature of zone 4 is 225°C, the temperature of zone 5 is 230°C, the temperature of the die head is 235°C, the rotation speed is 250r / min, and then the mixed material is extruded, cooled, and granulated to obtain the corrosion-resistant material.
[0045] Example 5
[0046] Compared with Example 4, the only difference is:
[0047] The modified calcium carbonate in Example 1 is replaced by the modified calcium carbonate in Example 2, and the amount used remains unchanged.
[0048] Example 6
[0049] Compared with Example 4, the only difference is:
[0050] The modified calcium carbonate in Example 1 is replaced by the modified calcium carbonate in Example 3, and the amount used remains unchanged.
[0051] Example 7
[0052] Compared with Example 4, the only difference is:
[0053] 10 parts of the modified calcium carbonate in Example 1 were replaced with 12.5 parts of the modified calcium carbonate in Example 1.
[0054] Example 8
[0055] Compared with Example 4, the only difference is:
[0056] 10 parts of the modified calcium carbonate in Example 1 were replaced with 15 parts of the modified calcium carbonate in Example 1.
[0057] Example 9
[0058] Compared with Example 4, the only difference is:
[0059] A refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0060] 48 parts of high impact polystyrene, 40 parts of polyethylene, 12 parts of modified calcium carbonate in Example 1, 8 parts of maleic anhydride grafted styrene-butadiene block copolymer, 1 part of polyethylene wax, and 0.5 parts of antioxidant 168.
[0061] Example 10
[0062] Compared with Example 4, the only difference is:
[0063] A refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0064] 52 parts of high impact polystyrene, 48 parts of polyethylene, 15 parts of modified calcium carbonate in Example 1, 8 parts of maleic anhydride grafted styrene-butadiene block copolymer, 2.8 parts of sodium stearate, and 0.85 parts of antioxidant 1076.
[0065] Embodiment 11
[0066] Compared with Example 4, the only difference is:
[0067] S2. Feed the mixed material obtained in step S1 into a twin-screw extruder, and the mixed material is fully fused under the shearing, mixing and conveying of the screw, wherein the temperature of zone 1 in the twin-screw extruder is 200°C, the temperature of zone 2 is 210°C, the temperature of zone 3 is 215°C, the temperature of zone 4 is 230°C, the temperature of zone 5 is 235°C, the temperature of the die head is 245°C, the rotation speed is 350r / min, and then the mixture is extruded, cooled, and granulated to obtain the corrosion-resistant material.
[0068] Comparative Example 2
[0069] Compared with Example 4, the only difference is:
[0070] The modified calcium carbonate in Example 1 was replaced by the modified calcium carbonate in Comparative Example 1, and the amount used remained unchanged.
[0071] Comparative Example 3
[0072] Compared with Example 4, the only difference is:
[0073] 10 parts of the modified calcium carbonate in Example 1 were replaced by 7 parts of the modified calcium carbonate in Example 1.
[0074] Comparative Example 4
[0075] Compared with Example 4, the only difference is:
[0076] 10 parts of the modified calcium carbonate in Example 1 were replaced with 20 parts of the modified calcium carbonate in Example 1.
[0077] Comparative Example 5
[0078] Compared with Example 4, the only difference is:
[0079] A refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0080] 40 parts of high impact polystyrene, 30 parts of polyethylene, 6 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.5 parts of stearic acid, and 0.1 parts of antioxidant 1010.
[0081] Comparative Example 6
[0082] Compared with Example 4, the only difference is:
[0083] A refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0084] 40 parts of high impact polystyrene, 10 parts of modified calcium carbonate in Example 1, 6 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.5 parts of stearic acid, and 0.1 parts of antioxidant 1010.
[0085] Comparative Example 7
[0086] Compared with Example 4, the only difference is:
[0087] A refrigerator liner anti-corrosion material, comprising the following raw materials in parts by weight:
[0088] 65 parts of high impact polystyrene, 20 parts of polyethylene, 10 parts of modified calcium carbonate in Example 1, 6 parts of maleic anhydride grafted ethylene-vinyl acetate copolymer, 0.5 parts of stearic acid, and 0.1 parts of antioxidant 1010.
[0089] Comparative Example 8
[0090] Compared with Example 4, the only difference is:
[0091] S2. Feed the mixed material obtained in step S1 into a twin-screw extruder, and the mixed material is fully fused under the shearing, mixing and conveying of the screw, wherein the temperature of zone 1 in the twin-screw extruder is 180°C, the temperature of zone 2 is 200°C, the temperature of zone 3 is 200°C, the temperature of zone 4 is 215°C, the temperature of zone 5 is 220°C, the temperature of the die head is 225°C, the rotation speed is 250r / min, and then the mixture is extruded, cooled, and granulated to obtain the corrosion-resistant material.
[0092] The following performance tests were performed on the anti-corrosion materials obtained in Examples 4 to 11 and Comparative Examples 2 to 8:
[0093] (1) Tensile strength: The tensile strength test was carried out according to GB / T 1040;
[0094] (2) Elongation at break: Elongation at break test is conducted according to GB / T 1040;
[0095] (3) Notched impact strength: notched impact strength test is carried out according to standard GB / T 1843;
[0096] (4) Bending strength: Bending strength test is carried out according to standard GB / T 9341;
[0097] (5) Melt index: Melt index test is carried out according to standard GB / T 3682;
[0098] The above test results are shown in Table 1:
[0099] Table 1
[0100]
[0101] It can be seen from Table 1 that, compared with Comparative Examples 2-8, the anti-corrosion materials obtained in Examples 4-11 have excellent tensile strength, impact strength and crack resistance, etc. It can be seen that the anti-corrosion material for refrigerator liner provided by the present invention has excellent mechanical properties, so that the obtained refrigerator liner is not easy to crack and has excellent comprehensive performance.
[0102] (6) Oil resistance: Bend the American standard tensile specimen and fix it with a clamp (inner diameter of the arc is 20 cm), soak it in a container filled with sesame oil, and place it at room temperature (23°C, 48 hours) and high and low temperature cycles (-40°C, 70°C for 4 hours each, five cycles). After the test, observe its surface;
[0103] (7) Antibacterial performance: The antibacterial rate is tested according to ISO 22196-2011 "Evaluation method for antibacterial properties of plastic products surface".
[0104] The above test results are shown in Table 2:
[0105] Table 2
[0106]
[0107] It can be seen from Table 2 that, compared with Comparative Examples 2-8, the oil resistance and antibacterial rate of the anti-corrosion materials obtained in Examples 4-11 are higher than those in Comparative Examples 2-8. It can be seen that the anti-corrosion material for refrigerator liner provided by the present invention has excellent oil resistance, water resistance and antibacterial properties, so that the prepared refrigerator liner is not easily corroded, and at the same time has a very positive effect on the cleaning of the prepared refrigerator liner and people's healthy life.
[0108] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0109] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A corrosion-resistant material for refrigerator liner, It is characterized in that The invention comprises the following raw materials in parts by weight: 40-55 parts of high impact polystyrene, 30-50 parts of polyethylene, 10-15 parts of modified calcium carbonate, 6-10 parts of compatibilizer, 0.1-3 parts of lubricant and 0.05-1 parts of antioxidant; The modified calcium carbonate is prepared by the following steps: Calcium carbonate and ammonia water are added to anhydrous ethanol, ultrasonically dispersed, tetraethyl silicate and 1H,1H,2H,2H-perfluorooctyltriethoxysilane are added, stirring is continued, centrifugal filtration is performed, washing is performed, drying is performed to constant weight, and grinding is performed to obtain modified calcium carbonate.
2. The anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that The dosage ratio of calcium carbonate, ammonia water, anhydrous ethanol, tetraethyl silicate and 1H,1H,2H,2H-perfluorooctyltriethoxysilane is 0.50-0.55g:10mL:40mL:4-5mL:0.5-0.6mL.
3. The anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that Grind to a particle size of 200-350 nm.
4. The anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that The compatibilizer is one of maleic anhydride grafted ethylene-vinyl acetate copolymer and maleic anhydride grafted styrene-butadiene block copolymer.
5. The anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that The lubricant is at least one of stearic acid, butyl stearate, oleamide, polyethylene wax and sodium stearate.
6. The anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that The antioxidant is at least one of antioxidant 1010 , antioxidant 1076 , antioxidant 1035 , antioxidant 168 and antioxidant 264 .
7. The method for preparing the anti-corrosion material for refrigerator liner according to claim 1, It is characterized in that The following steps are involved: S1. Weigh high-impact polystyrene, polyethylene, modified calcium carbonate, a compatibilizer, a lubricant and an antioxidant in parts by weight, add them into a mixer and mix them evenly to obtain a mixture; S2. The mixed material obtained in step S1 is fed into a twin-screw extruder. The mixed material is fully fused under the shearing, mixing and conveying of the screw, and then extruded, cooled and granulated to obtain a corrosion-resistant material.
8. The method for preparing the anti-corrosion material for refrigerator liner according to claim 7, It is characterized in that In the twin-screw extruder, the temperature of zone 1 is 190-200°C, the temperature of zone 2 is 205-215°C, the temperature of zone 3 is 210-220°C, the temperature of zone 4 is 225-235°C, the temperature of zone 5 is 230-240°C, and the temperature of the die head is 235-245°C.
9. The method for preparing the anti-corrosion material for refrigerator liner according to claim 7, It is characterized in that The speed of twin-screw extruder is 200-350r / min.